High-dielectric composite solid electrolyte, integrated all-solid-state battery and preparation method
By using high-dielectric composite solid electrolytes in solid-state batteries and using dielectric ceramic fillers to reduce interface impedance and improve high-voltage stability, the problems of high cathode/electrolyte interface impedance and poor high-voltage stability of traditional solid-state batteries are solved, achieving all-solid-state High energy density and long cycle life of lithium batteries.
Patent Information
- Application Number
- CN202410869496.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional solid-state batteries have high cathode/electrolyte interface impedance and poor high-voltage stability, which affects their lower energy density in practical applications.
Using a high dielectric composite solid electrolyte, by dissolving bis(trifluoromethane)sulfonylimide lithium salt and difluoroxalate borate lithium salt in polyethylene glycol methyl ether acrylate, and adding dielectric ceramic filler barium titanate, Inject into the electrospinning support separator to prepare a composite solid electrolyte, which reduces the interface impedance and improves high-voltage stability.
It significantly reduces the interface resistance between the positive electrode and the electrolyte, builds a stable positive electrode interface layer, improves high-voltage stability, and achieves high energy density and long cycle life of all-solid-state lithium batteries, making it suitable for large-scale applications.
Smart Images

Figure CN118738524A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid-state lithium metal batteries, and specifically relates to an all-solid-state battery integrating a high-dielectric composite solid electrolyte with reduced interface impedance and improved high-voltage stability, and a preparation method thereof. Background Art
[0002] With the development of new energy vehicles and electrochemical energy storage industries, the energy density requirements for lithium-ion batteries are getting higher and higher. Higher energy density can be achieved by using high-capacity lithium metal anodes and high-nickel ternary cathodes and applying higher cut-off voltages. However, when the electrolyte composed of traditional organic solvents and lithium salts is matched with high-nickel ternary cathodes and lithium metal anodes, dendrite growth is prone to occur, leading to internal short circuits, which in turn leads to thermal runaway, combustion, and even explosion; when high cut-off voltages are applied, the decomposition and gas production of organic electrolytes will further cause safety issues. The use of solid electrolytes (SSEs) to match lithium metal anodes can effectively inhibit dendrite growth, and their high electrochemical stability can be used to match high-voltage high-nickel ternary cathodes to achieve higher energy density and higher safety. Among various SSEs, polymer solid electrolytes (SPEs) have good flexibility, are easy to prepare on a large scale, and are highly compatible with existing processes. They are considered to be the SSEs most likely to be commercially applied first. However, SPE still has many problems: traditional SPE is difficult to fill the gaps between the particles inside the positive electrode, lacking the internal ion path of the positive electrode; and there is a significant interface potential difference between the polymer phase and the positive electrode active material phase, resulting in a large interface impedance; traditional SPE represented by polyethylene oxide (PEO) has poor high voltage stability and is still difficult to match the high-voltage positive electrode, becoming an obstacle to the further development of high-energy-density all-solid-state lithium batteries. Therefore, studying the positive electrode interface problems of all-solid-state lithium batteries, reducing the interface impedance, and improving the interface stability are the challenges faced in promoting the development of high-energy-density all-solid-state lithium batteries.
[0003] It should be noted that the information disclosed in the above background technology section is only used for understanding the background of the present application, and therefore may include information that does not constitute prior art known to ordinary technicians in the field. Summary of the invention
[0004] The main purpose of the present invention is to overcome the defects of the above-mentioned background technology, to provide a high dielectric composite solid electrolyte and an integrated all-solid-state battery and a preparation method, to solve the problem of high positive electrode / electrolyte interface impedance and poor high voltage stability of traditional solid-state batteries, which affects the lower energy density in practical applications.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing a high dielectric composite solid electrolyte and an integrated all-solid-state battery, characterized in that it comprises the following steps:
[0007] S1: using polyethylene glycol methyl ether acrylate, dissolving bis(trifluoromethane)sulfonyl imide lithium salt, difluorooxalato borate lithium salt and azobisisobutyronitrile to obtain a mixed solution;
[0008] S2: adding a dielectric ceramic filler into the mixed solution to obtain a precursor solution A;
[0009] S3: Inject the precursor solution A into the electrospinning support membrane, and assemble the battery to obtain a composite solid electrolyte and an integrated all-solid-state battery.
[0010] Furthermore, in step S1, the molar ratio of bis(trifluoromethane)sulfonyl imide lithium salt to difluorooxalatoborate lithium salt is 2:8 to 8:2, and the total concentration of lithium salt is 0.5 to 4 mol / L.
[0011] Furthermore, in step S1, the concentration of azobisisobutyronitrile is 0.5-5 mg / mL.
[0012] Furthermore, in step S2, the dielectric ceramic filler is barium titanate BaTiO3, with a particle size of 100 to 1000 nm and an addition amount of 0.01 to 0.5 g / mL.
[0013] Furthermore, in step S3, the electrospinning support membrane is a membrane with micron-scale pores.
[0014] A composite solid electrolyte is prepared using the method.
[0015] An integrated all-solid-state battery comprises the composite solid-state electrolyte, a lithium metal negative electrode, and a high-nickel ternary positive electrode material.
[0016] Furthermore, the high-nickel ternary positive electrode material is a nickel-cobalt-manganese oxide positive electrode.
[0017] In some embodiments, a method for preparing a high dielectric composite solid electrolyte and an integrated all-solid-state battery comprises the following steps:
[0018] S1: using polyethylene glycol methyl ether acrylate to dissolve bis(trifluoromethane)sulfonyl imide lithium salt, difluorooxalato borate lithium salt and azobisisobutyronitrile, stirring for 1 to 3 hours to obtain a uniform transparent solution;
[0019] S2: Add the dielectric ceramic filler to the uniform transparent solution obtained in S1, and stir for 2 to 4 hours to obtain a white precursor solution A;
[0020] S3: Injecting the precursor solution A into the electrospinning support membrane, then assembling the battery and keeping it warm for 10 to 20 hours to obtain a composite solid electrolyte and an integrated all-solid-state battery.
[0021] In some embodiments, in step S3, the electrospinning support membrane is a membrane with micron-scale pores to ensure that the nanoscale filler can be evenly dispersed therein.
[0022] The present invention also provides a composite solid electrolyte, which is prepared using the composite solid electrolyte preparation method as described above.
[0023] In some embodiments, a battery includes the composite solid electrolyte, a negative electrode composed of lithium metal, and a positive electrode composed of high-capacity nickel-cobalt-manganese oxide.
[0024] The present invention has the following beneficial effects:
[0025] The present invention proposes a high-dielectric composite solid electrolyte and an integrated all-solid-state lithium battery and a preparation method, which greatly reduces the interface impedance between the positive electrode and the electrolyte, constructs a stable positive electrode interface layer, and improves high-voltage stability.
[0026] In the present invention, the dielectric ceramic filler can interact with the polyethylene glycol methyl ether acrylate in the composite solid electrolyte to reduce the coordination of lithium ions with the polyethylene glycol methyl ether acrylate, increase the coordination of lithium ions with anions, and generate a stable interface layer rich in inorganic lithium fluoride and borofluoride components during the battery cycle. The dielectric ceramic reduces the interface potential difference between the composite solid electrolyte and the positive electrode active material, and reduces the interface impedance. The composite solid electrolyte uniformly fills the internal pores of the positive electrode, and the positive electrode active material and the composite solid electrolyte have good interface contact.
[0027] The present invention is used to uniformly fill the composite solid electrolyte into the internal pores of the positive electrode, realizing an efficient lithium ion transport path; the interface potential difference is reduced by the nano-dielectric ceramic filler, the interface impedance is reduced, and the room temperature operation of the polymer-based composite electrolyte all-solid-state lithium battery is realized, the continuous cycle time exceeds one year, and the number of cycles exceeds 1300 times. By utilizing the interaction between the nano-dielectric ceramic filler and the polymer, the lithium ion coordination structure is adjusted, and a high-stable CEI rich in anion-derived inorganic components is constructed, realizing the stable cycle of the all-solid-state lithium battery at 4.7V. The method is low-cost, compatible with existing production processes, and suitable for rapid promotion and large-scale application. The present invention provides an effective solution for the industrial development of high-energy-density and high-safety all-solid-state lithium batteries.
[0028] Other beneficial effects of the embodiments of the present invention will be further described below. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is an optical photograph of the composite solid electrolyte prepared in an embodiment of the present invention.
[0030] Figure 2This is a SEM image of the composite solid electrolyte prepared in an embodiment of the present invention.
[0031] Figure 3 The XRD diagram of the composite solid electrolyte prepared in the embodiment of the present invention.
[0032] Figure 4 This is a SEM image of the integrated all-solid-state lithium battery positive electrode prepared in an embodiment of the present invention.
[0033] Figure 5 This is an EDS image of the integrated all-solid-state lithium battery positive electrode prepared in an embodiment of the present invention.
[0034] Figure 6 This is a cross-sectional SEM image of an integrated all-solid-state lithium battery prepared in an embodiment of the present invention.
[0035] Figure 7 This is a surface potential diagram of the positive electrode interface of the integrated all-solid-state lithium battery prepared in an embodiment of the present invention.
[0036] Figure 8 This is a line scan of the positive electrode interface surface potential of the integrated all-solid-state lithium battery prepared in an embodiment of the present invention.
[0037] Fig. 9 The low impedance performance of the positive electrode interface of the integrated all-solid-state lithium battery prepared in the embodiment of the present invention.
[0038] Fig.10 This is the coordination structure of the composite solid electrolyte ion aggregate prepared in the embodiment of the present invention.
[0039] Fig.11 The composite solid electrolyte prepared in the embodiment of the present invention has high voltage resistance and stability.
[0040] Fig.12 The room temperature high-voltage cycle performance of the composite solid electrolyte assembled button-type battery prepared in the embodiment of the present invention. DETAILED DESCRIPTION
[0041] The following is a detailed description of the embodiments of the present invention. It should be emphasized that the following description is only exemplary and is not intended to limit the scope and application of the present invention.
[0042] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0043] The present invention provides a method for preparing a high dielectric composite solid electrolyte and an integrated all-solid-state battery, comprising the following steps:
[0044] S1: using polyethylene glycol methyl ether acrylate, dissolving bis(trifluoromethane)sulfonyl imide lithium salt, difluorooxalato borate lithium salt and azobisisobutyronitrile to obtain a mixed solution;
[0045] S2: adding a dielectric ceramic filler into the mixed solution to obtain a precursor solution A;
[0046] S3: Inject the precursor solution A into the electrospinning support membrane, and assemble the battery to obtain a composite solid electrolyte and an integrated all-solid-state battery.
[0047] In some embodiments, in step S1, the molar ratio of bis(trifluoromethane)sulfonyl imide lithium salt to difluorooxalato borate lithium salt is 2:8-8:2, for example 2:8, 4:6, 5:5, 6:4, 8:2. The total concentration of lithium salt is 0.5-4 mol / L, for example 0.5, 1, 2, 4 mol / L.
[0048] In some embodiments, in step S1, the concentration of azobisisobutyronitrile is 0.5-5 mg / mL, for example, 0.5, 1.5, 3, or 5 mg / mL.
[0049] In some embodiments, in step S2, the dielectric ceramic filler is barium titanate BaTiO3, with a particle size of 100 to 1000 nm, such as 100, 500, 1000 nm, and an addition amount of 0.01-0.5 g / mL, such as 0.109 g / mL.
[0050] In the present invention, the in-situ polymerization method can effectively fill the internal pores of the positive electrode, build a good interface contact, and provide a rich lithium ion transmission interface. The nano dielectric ceramic filler can significantly reduce the interface potential difference between the positive electrode active material and the electrolyte, and can reduce the interface impedance at different temperatures and different potentials. In addition, the filler can also interact with the polymer, adjust the lithium ion coordination structure, build a more stable CEI, and improve the high voltage stability and long cycle life of the all-solid-state lithium battery.
[0051] A composite solid electrolyte is prepared using the method.
[0052] An integrated all-solid-state battery comprises the composite solid-state electrolyte, a lithium metal negative electrode, and a high-nickel ternary positive electrode material.
[0053] In a preferred embodiment, the nano dielectric ceramic filler in the composite solid electrolyte is barium titanate (BaTiO3).
[0054] Due to the dielectric effect, nano dielectric ceramic barium titanate can reduce the interface potential difference between the positive electrode active material and the electrolyte, and reduce the lithium ion transfer impedance at the positive electrode interface. At the same time, the interaction between nano dielectric ceramic barium titanate and polymer can reduce the coordination ability of polymer and lithium ions, produce more ion aggregate structures, and construct a positive electrode electrolyte interface phase (CEI) rich in lithium fluoride and boron fluorine inorganic components. The embodiment of the present invention prepares an integrated all-solid-state lithium battery by an in-situ polymerization method. Figure 3 As shown in Figure 2, the in situ polymerized polymer is amorphous and has good chain segment mobility, which is conducive to ion transport. Figure 4 As shown, the in-situ polymerization method can make the polymer solid electrolyte and nano-dielectric ceramic filler evenly dispersed to fill the internal pores of the positive electrode, greatly improving the interface contact ability and interface transmission performance between the positive electrode and the electrolyte.
[0055] A method for preparing a composite solid electrolyte, for preparing a composite solid electrolyte filled with a dielectric filler, comprising the following steps:
[0056] S1: using polyethylene glycol methyl ether acrylate to dissolve bis(trifluoromethane)sulfonyl imide lithium salt, difluorooxalato borate lithium salt and azobisisobutyronitrile, stirring for 1 to 3 hours to obtain a uniform transparent solution;
[0057] S2: Add the dielectric ceramic filler to the uniform transparent solution obtained in S1, and stir for 2 to 4 hours to obtain a white precursor solution A;
[0058] S3: Injecting the precursor solution A into the electrospinning support membrane, then assembling the battery and keeping it warm for 10 to 20 hours to obtain a composite solid electrolyte and an integrated all-solid-state battery.
[0059] In a preferred embodiment, the dielectric ceramic filler is barium titanate, and the particle size of the dielectric ceramic filler barium titanate is nanometer-level, which can retain high dielectric properties and be evenly dispersed in the integrated all-solid-state battery. At the same time, the composite solid-state electrolyte preparation method may also include W4: injecting the white precursor solution A prepared in step S3 into the stacked or wound soft-pack battery, and after encapsulating the soft-pack battery, placing the soft-pack battery in an oven for 10 to 20 hours.
[0060] In an embodiment of the present invention, the composite solid electrolyte prepared by the above-mentioned composite solid electrolyte preparation method has a thickness of 18 to 25 um; it can be matched with a high-voltage high-nickel ternary positive electrode material to improve the energy density.
[0061] In the embodiment of the present invention, lithium metal is used as the negative electrode, and high-capacity nickel cobalt manganese oxide (LiNi0.8Co0.1Mn0.1O2, NCM811) is used as the positive electrode active material to match the composite solid electrolyte to assemble a solid-state lithium metal battery. The nano-dielectric ceramic filler can significantly reduce the interface impedance between the positive electrode and the electrolyte, and the nano-dielectric ceramic filler can induce the production of more ion aggregate coordination structures, thereby producing a stable positive electrode interface layer, which can significantly enhance the cycle stability of the integrated all-solid-state lithium battery matching the high-voltage positive electrode at room temperature.
[0062] like Figure 5 As shown, the composite solid electrolyte and nano-dielectric ceramics in the embodiment of the present invention are evenly dispersed inside the positive electrode of the integrated all-solid-state lithium battery, which helps to improve the ion transmission efficiency between the solid phases inside the positive electrode; Figure 6 As shown in the figure, from top to bottom, they are lithium metal negative electrode, composite solid electrolyte and composite positive electrode. There is no obvious gap between the three, forming an integrated all-solid-state lithium battery with interface fusion; Figure 7 As shown in the figure, the positive electrode interface surface potential diagram of the integrated all-solid-state lithium battery prepared in the embodiment of the present invention shows that the positive electrode active material particles and the electrolyte present a uniform surface potential distribution. Since the test value of the surface potential corresponds to the work function of the material, when two solids with different work functions come into contact, an interface potential difference will be generated at the interface, which will hinder the ion transport at the interface, such as Figure 8 As shown, the interface potential difference between the composite solid electrolyte and the positive electrode active material in the embodiment of the invention is only 20mV; Fig. 9 As shown, the cathode / electrolyte interface of the integrated all-solid-state lithium battery in the embodiment of the invention exhibits low impedance at different temperatures. Different from the research on fillers in the prior art, the embodiment of the present invention focuses on the regulation of interface potential difference and interface impedance, using dielectric ceramic fillers to reduce interface impedance and improve ion transport flux. Fig.10As shown, the dielectric ceramic filler increases the proportion of ion aggregate structure, which can improve the stability of the positive electrode interface layer formed in situ during the charge and discharge process. Based on the dielectric ceramic filler barium titanate in the embodiment of the present invention, the interface impedance between the positive electrode and the electrolyte is reduced, and the coordination structure is regulated by interacting with the polymer to construct a stable positive electrode interface layer, thereby improving the characteristics of high voltage stability; therefore, the embodiment of the present invention is intended to propose a method for preparing a high dielectric composite solid electrolyte and an integrated all-solid-state lithium battery. In the embodiment of the present invention, it is found that the dielectric ceramic filler barium titanate can adjust the positive electrode / electrolyte interface potential difference and reduce the interface impedance. In addition, the dielectric ceramic filler can also interact with the polymer to induce the generation of more ion aggregate coordination structures, forming a uniform and stable positive electrode interface layer, which greatly improves the high voltage stability and cycle life of the integrated all-solid-state lithium battery. The method of using the dielectric ceramic filler barium titanate to reduce the interface impedance and construct a high voltage stable interface layer is simple and easy, low cost, and the in-situ polymerization method is simple to operate to prepare an integrated all-solid-state lithium battery, compatible with the existing large-scale production process of lithium-ion batteries, suitable for rapid promotion and application, and will promote the development of the all-solid-state battery industry.
[0063] Specifically, the embodiment of the present invention proposes a method for preparing a composite solid electrolyte and an integrated all-solid-state lithium battery based on a method of reducing the interface impedance between the positive electrode and the electrolyte using a dielectric ceramic filler barium titanate. The integrated all-solid-state lithium battery can make the lithium-lithium symmetrical battery at 0.2 mA / cm 2 The all-solid-state lithium metal battery with NCM811 as the positive electrode can stably cycle 1300 times at a high voltage of 4.7V and 1600 times at a high voltage of 4.6V, which significantly improves the long cycle life of the polymer-based composite solid electrolyte all-solid-state lithium battery under high voltage and will promote the industrialization of solid-state batteries.
[0064] like Fig.11 As shown, the high-dielectric composite solid electrolyte prepared in an embodiment of the present invention is subjected to a high-voltage stability test. It can be seen that the electrolyte obtained by the preparation method thereof (the dark color is a high-dielectric composite solid electrolyte) remains stable under a high voltage above 5V, and no obvious oxidation decomposition reaction occurs.
[0065] The embodiment of the present invention further provides a battery, which includes the composite solid electrolyte prepared as described above, a negative electrode composed of lithium metal, and a positive electrode composed of high-voltage nickel-cobalt-manganese oxide.
[0066] The advantages of the battery prepared in the embodiment of the present invention are compared and illustrated by Experimental Example 1 and Experimental Example 2 below:
[0067] Experimental Example 1
[0068] This embodiment provides a method for preparing a polymer solid electrolyte and assembling an integrated all-solid-state lithium battery, which comprises at least the following steps:
[0069] Step 1: First, weigh 100 mg PVDF5130 (binder), 100 mg Super P (conductive carbon black) and 800 mg NCM811 active substance and grind them in a mortar for 10 minutes (the grinding process is carried out under infrared light to reduce the moisture absorption of the powder). After fully mixing, add 2.4 mL NMP and stir at room temperature for more than 4 hours.
[0070] Step 2: coat the positive electrode slurry obtained in step 1 on aluminum foil, dry it at 80°C for more than 30 minutes to remove NMP, cut it into discs of appropriate size to obtain NCM811 positive electrode, weigh it, dry it in a vacuum oven at 120°C for 2 hours to remove moisture, and store it in a glove box.
[0071] Step 3: Under an inert atmosphere, weigh 459 mg LiTFSI and 57 mg LiDFOB, place in a stirring bottle, add 2 mL polyethylene glycol methyl ether acrylate and 3 mg AIBN, stir at room temperature for more than 4 hours in a small stirrer, and the lithium salt and AIBN are completely dissolved to obtain a uniform transparent solution.
[0072] Step 4: Inject the solution obtained in step 3 into both sides of the electrospinning support membrane, and place the NCM811 positive electrode and the lithium metal negative electrode on both sides of the support membrane respectively, encapsulate them with a battery shell, and keep them in an oven at 70°C for 12 hours to complete the in-situ polymerization reaction to obtain a polymer solid electrolyte and an integrated all-solid-state lithium battery.
[0073] Experimental Example 2
[0074] This embodiment provides a method for preparing a composite solid electrolyte and assembling an integrated all-solid-state lithium battery, which comprises at least the following steps:
[0075] Step 1: First, weigh 100 mg PVDF5130 (binder), 100 mg Super P (conductive carbon black) and 800 mg NCM811 active substance and grind them in a mortar for 10 minutes (the grinding process is carried out under infrared light to reduce the moisture absorption of the powder). After fully mixing, add 2.4 mL NMP and stir at room temperature for more than 4 hours.
[0076] Step 2: coat the positive electrode slurry obtained in step 1 on aluminum foil, dry it at 80°C for more than 30 minutes to remove NMP, cut it into discs of appropriate size to obtain NCM811 positive electrode, weigh it, dry it in a vacuum oven at 120°C for 2 hours to remove moisture, and store it in a glove box.
[0077] Step 3: Under an inert atmosphere, weigh 459 mg LiTFSI and 57 mg LiDFOB, place them in a stirring bottle, add 2 mL polyethylene glycol methyl ether acrylate, 3 mg AIBN and 0.218 g nano-BaTiO3, stir at room temperature for more than 4 hours in a small stirrer, and the lithium salt and AIBN are completely dissolved to obtain a uniform transparent solution.
[0078] Step 4: Inject the solution obtained in step 3 into both sides of the electrospinning support membrane, and place the NCM811 positive electrode and the lithium metal negative electrode on both sides of the support membrane respectively, encapsulate them with a battery shell, and keep them in a 70°C oven for 12 hours to complete the in-situ polymerization reaction to obtain a polymer solid electrolyte and an integrated all-solid-state lithium battery.
[0079] like Fig.12 As shown, a schematic diagram of the room temperature high-voltage cycle performance of a button-type battery assembled with a composite solid electrolyte prepared by the invention (the dark color is a high dielectric composite solid electrolyte, and the light color is a polymer solid electrolyte) is shown in the figure. By comparison, it can be seen that the battery assembled with the high dielectric composite solid electrolyte has long cycle stability at high voltage. The battery prepared in Example 1 has multiple overcharges and reduced coulombic efficiency in the first 100 cycles at 4.7V, and completely fails after 700 cycles. The battery prepared in Example 2 has stable cycles of more than 1300 times at 4.7V. By comparison, it can be seen that the battery assembled with the high dielectric composite solid electrolyte can achieve high voltage and long life operation.
[0080] The composite solid electrolyte and all-solid-state battery prepared by this method have excellent high voltage stability and low interface impedance, long cycle life, are compatible with existing lithium-ion battery production processes, are very suitable for rapid promotion and large-scale applications, and will promote the development of the all-solid-state battery industry.
[0081] The above content is a further detailed description of the present invention in combination with specific / preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, it can also make several substitutions or modifications to these described embodiments, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention. In the description of this specification, the description of the reference terms "an embodiment", "some embodiments", "preferred embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in combination with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily target the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In the absence of mutual contradiction, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions and modifications can be made herein without departing from the scope of protection of the patent application.
Claims
1. A method for preparing a high dielectric composite solid electrolyte and an integrated all-solid-state battery, It is characterized in that The steps include: S1: using polyethylene glycol methyl ether acrylate, dissolving bis(trifluoromethane)sulfonyl imide lithium salt, difluorooxalato borate lithium salt and azobisisobutyronitrile to obtain a mixed solution; S2: adding a dielectric ceramic filler into the mixed solution to obtain a precursor solution A; S3: Inject the precursor solution A into the electrospinning support membrane, and assemble the battery to obtain a composite solid electrolyte and an integrated all-solid-state battery.
2. The method according to claim 1, It is characterized in that In step S1, the molar ratio of bis(trifluoromethane)sulfonyl imide lithium salt to difluorooxalatoborate lithium salt is 2:8 to 8:2, and the total concentration of lithium salt is 0.5 to 4 mol / L.
3. The method according to claim 1, It is characterized in that In step S1, the concentration of azobisisobutyronitrile is 0.5-5 mg / mL.
4. The method according to claim 1, It is characterized in that In step S2, the dielectric ceramic filler is barium titanate BaTiO3, with a particle size of 100 to 1000 nm, and the added amount is preferably 0.01 to 0.5 g / mL.
5. The method according to claim 1, It is characterized in that In step S3, the electrospinning support membrane is a membrane with micron-scale pores.
6. A composite solid electrolyte, It is characterized in that Prepared by the method according to any one of claims 1 to 5.
7. An integrated all-solid-state battery, It is characterized in that It comprises the composite solid electrolyte as claimed in claim 6, a lithium metal negative electrode, and a high-nickel ternary positive electrode material.
8. The integrated all-solid-state battery according to claim 7, It is characterized in that The high-nickel ternary positive electrode material is a nickel-cobalt-manganese oxide positive electrode.
Citation Information
Cited By
All-solid-state battery, preparation method thereof and electric equipment
CN119725683A
Composite solid electrolyte containing oxygen-vacancy-rich filler and preparation method of composite solid electrolyte
CN120637573A