Optical excitation regulation heterojunction solid electrolyte membrane and preparation method thereof

Through photoexcitation, the heterojunction solid electrolyte membrane is regulated, and the electric field is used to generate an electric field to improve the electrolyte performance, solving the brittleness and conductivity problems of all-solid lithium metal batteries, and achieving efficient application of flexible energy storage equipment.

CN118970170APending Publication Date: 2024-11-15UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411294097.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

All-solid lithium metal batteries are difficult to use due to the brittleness of inorganic solid electrolytes, limited thermodynamic stability, sensitivity to moisture and the need for high external pressure in specific molds to work properly, resulting in difficulty in practical application, and polyoxyethylene electrolytes. The ionic conductivity is low and the mechanical properties are limited, which limits its wide application.

Method used

Using photoexcitation to regulate heterojunction solid electrolyte membranes, it is prepared by blending polymer matrix materials, heterojunction fillers, bacterial cellulose soft fillers and lithium salts. It uses photoexcitation to generate a powerful and stable photogenerating electric field, improve the performance of electrolytes and reduce the performance of the electrolytes. Interfacial impedance accelerates the electrochemical kinetic process, thereby improving ionic conductivity and mechanical toughness.

Benefits of technology

Under room temperature lighting conditions, it can improve ion conductivity and mechanical properties without additional external pressure, ensure that the battery stabilizes the output voltage after repeated bending and folding, and significantly increase the number of lithium ion transfers and mechanical strength, achieving efficient application of flexible energy storage equipment .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970170A_ABST
    Figure CN118970170A_ABST
Patent Text Reader

Abstract

The invention provides an optical excitation regulation heterojunction solid electrolyte membrane and a preparation method thereof, and belongs to the technical field of batteries, the solid electrolyte membrane comprises a polymer matrix material, a heterojunction filler, a bacterial cellulose soft filler and a lithium salt, and the heterojunction filler is a composite material of cobaltosic oxide and titanium dioxide. According to the invention, trace heterojunctions are doped into polyethylene oxide electrolyte, and a generated photo-generated electric field is utilized to reduce interface impedance so as to accelerate an electrochemical kinetics process, so that the ionic conductivity, the lithium ion transfer number and the mechanical toughness are effectively improved; a flexible optical excitation cell device assembled based on the solid electrolyte membrane can normally and stably work even after repeated bending and folding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a light-excited regulated heterojunction solid electrolyte membrane and a preparation method thereof. Background Art

[0002] All-solid-state lithium metal batteries are considered to be one of the most promising flexible energy storage devices. Although inorganic solid electrolytes have good ionic conductivity and a wide voltage window, their inherent brittleness, limited thermodynamic stability, sensitivity to moisture, and the need for high external pressure in a specific mold to work properly have brought many difficulties to practical applications, especially in flexible energy storage devices.

[0003] Among polymer electrolytes, polyoxyethylene electrolytes have become the most studied and promising electrolytes due to their excellent mechanical properties, easy processability, and good interfacial compatibility with electrodes. However, the weak ability of polyoxyethylene polymer electrolytes to promote lithium salt dissociation and lithium ion transport leads to low ionic conductivity and limited mechanical properties, which seriously restricts their widespread application. Constructing composite solid electrolytes and utilizing the complementary advantages of polymer electrolytes and inorganic solid electrolytes has become a viable option for convenient assembly of highly flexible and scalable batteries. Therefore, the correct design of solid polymer electrolytes with high ionic conductivity and room temperature applicability is crucial for the manufacture of next-generation flexible energy storage devices. New perspectives are urgently needed to develop safe, stable, and high-performance solid polymer electrolytes. Summary of the invention

[0004] Based on the photocatalytic design concept, the present invention provides a photoexcitation-regulated heterojunction solid electrolyte membrane and a preparation method thereof. The present invention utilizes the heterojunction to generate a strong and stable photogenerated electric field through photoexcitation, improves electrolyte performance, reduces interface impedance, and accelerates the electrochemical kinetic process, thereby effectively improving ionic conductivity, lithium ion transfer number, and mechanical toughness.

[0005] The purpose of the present invention can be achieved by the following scheme:

[0006] A light-excited regulated heterojunction solid electrolyte membrane is prepared by blending a polymer matrix material, a heterojunction filler, a bacterial cellulose soft filler and a lithium salt to form a membrane.

[0007] Furthermore, the content of the heterojunction filler accounts for 1%-10% of the total mass of the solid electrolyte membrane, the content of the bacterial cellulose soft filler accounts for 0.3%-1.3% of the total mass of the solid electrolyte membrane, and the remainder is the polymer matrix material and the lithium salt.

[0008] Furthermore, the polymer matrix material is one or more of polyethylene oxide, polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene, preferably polyethylene oxide, with an average molecular weight of about 5,000,000.

[0009] Further, the heterojunction filler is a composite material of cobalt trioxide and titanium dioxide, and its preparation method is: cobalt nitrate, titanium tetrachloride, HCl and salicylic acid are added to deionized water in a molar ratio of 8:2:2:4-6 and stirred until dissolved to obtain solution A; urea solution is prepared at the same time; according to the molar ratio of cobalt nitrate to urea of ​​1:10-15, solution A is mixed with the urea solution, and the mixture is treated in an oil bath at 90-120°C and centrifuged and dried. The dried sample is annealed at 300-400°C in a muffle furnace to obtain the heterojunction filler. Preferably: the temperature of the oil bath treatment is 95°C, and the oil bath time is 12 hours. The annealing temperature is 350°C, kept warm for 2 hours and cooled naturally.

[0010] Furthermore, the lithium salt is lithium bis(trifluoromethane)sulfonyl imide (LiTFSI).

[0011] Furthermore, the thickness of the light-excited regulated heterojunction solid electrolyte membrane is 50-100 microns, preferably 75-80 microns.

[0012] The present invention also provides a method for preparing the light-excited regulated heterojunction solid electrolyte membrane: a polymer matrix material, a heterojunction filler, a bacterial cellulose soft filler and a lithium salt are mixed in a solvent to prepare a membrane liquid, and then the light-excited regulated heterojunction solid electrolyte membrane is prepared by coating and drying. The steps are as follows:

[0013] (1) The polymer matrix material and lithium salt are dissolved in acetonitrile at the same time and stirred evenly without generating bubbles.

[0014] (2) After the heterojunction filler and the bacterial cellulose soft filler are mixed in acetonitrile, they are added to the solution of the polymer matrix material and the lithium salt and stirred thoroughly to obtain a membrane liquid; preferably, the mixture is stirred at room temperature for 6-24 hours.

[0015] (3) The membrane solution is coated on a polytetrafluoroethylene plate and vacuum dried for a period of time to obtain a light-excited regulated heterojunction solid electrolyte membrane. Preferably, the vacuum drying temperature is 50-80° C. and the drying time is 24-36 hours.

[0016] The present invention further provides a flexible light-excited battery device, which is assembled from a positive electrode, a negative electrode, a solid electrolyte membrane, a tab and a packaging film, wherein the positive electrode material is lithium iron phosphate (LFP) or lithium nickel cobalt manganese oxide (NCM811), the negative electrode is an ultra-thin perforated metal lithium foil, the solid electrolyte membrane is the above-mentioned light-excited regulated heterojunction solid electrolyte membrane, and the packaging film is a transparent conductive film. Preferably, the packaging film is a light-transmitting indium selenide oxide film.

[0017] The preparation method of the flexible light-excited battery device can be: stacking a transparent conductive film, a positive electrode (pre-connected with a pole ear), a solid electrolyte membrane, a negative electrode (pre-connected with a pole ear) and a transparent conductive film in sequence, and packaging them with a battery sealing machine to obtain a soft-pack battery.

[0018] The beneficial technical effects of the present invention are embodied in the following aspects:

[0019] 1. Compared with traditional polyethylene oxide electrolytes, the photoexcitation-regulated heterojunction solid electrolyte membrane provided by the present invention can convert functionalized inert heterojunction fillers into catalytically active fillers through photoexcitation under room temperature lighting conditions without additional external pressure, thereby generating a strong and stable electric field. The generated photogenerated electric field can improve electrolyte performance, reduce interfacial impedance, accelerate electrochemical kinetics, regulate lithium salt dissociation and ion migration mechanisms in the electrolyte, and effectively improve ionic conductivity and lithium ion transfer number.

[0020] 2. The photoexcitation-regulated heterojunction solid electrolyte membrane provided by the present invention significantly improves the mechanical properties by introducing bacterial cellulose, an environmentally friendly, mechanically strong, lithium-compatible and resource-abundant biomass resource, while maintaining high ionic conductivity, thereby making up for the poor mechanical properties of the composite solid electrolyte.

[0021] 3. The present invention adopts a new light-transmitting flexible soft-pack battery assembly technology, and the battery assembled with a light-excited regulated heterojunction solid electrolyte membrane can still exhibit stable voltage output and cycle stability even after repeated bending and folding. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a diagram showing the mechanism of light-excitation regulation of heterojunction solid electrolyte membranes according to the present invention;

[0023] Figure 2 It is a schematic diagram of the structure of the flexible light-excited battery of the present invention;

[0024] Figure 3 is the X-ray diffraction pattern of the heterojunction material prepared in Example 1 of the present invention;

[0025] Figure 4 is a scanning electron microscope image of the heterojunction material prepared in Example 1 of the present invention;

[0026] Figure 5 is a transmission electron microscope image of the heterojunction material prepared in Example 1 of the present invention;

[0027] Figure 6 is an X-ray diffraction spectrum of the light-excited regulated heterojunction solid electrolyte membrane prepared in Example 1 of the present invention;

[0028] Figure 7 is a scanning electron microscope image of the light-excitation-regulated heterojunction solid electrolyte membrane prepared in Example 1 of the present invention;

[0029] Figure 8 It is the Arrhenius plot of the light-excited regulated heterojunction solid electrolyte membrane prepared in Example 1 of the present invention and the solid electrolyte membrane prepared in Comparative Example 1;

[0030] Fig. 9 It is an infrared thermal imaging temperature change diagram corresponding to the light-excitation-regulated heterojunction solid electrolyte membrane prepared in Example 1 of the present invention and the assembled "perforated steel sheet||solid electrolyte membrane||perforated steel sheet" structure under the irradiation of a xenon lamp cold light source;

[0031] Fig.10 It is a stress-strain test curve diagram of the light-excitation-regulated heterojunction solid electrolyte membrane prepared in Example 1 of the present invention and the solid electrolyte membrane prepared in Comparative Example 1;

[0032] Fig.11 This is a cycle performance curve of the flexible light-excited battery prepared in Example 1 of the present invention at a current density of 0.2C under illumination, wherein the positive electrode material is lithium nickel cobalt manganese oxide (NCM811);

[0033] Fig.12 This is a cycle performance curve of the flexible light-excited battery prepared in Example 1 of the present invention at a current density of 0.2C under illumination, wherein the positive electrode material is lithium iron phosphate (LFP). DETAILED DESCRIPTION

[0034] In an embodiment of the present invention, a light-excited regulated heterojunction solid electrolyte membrane is provided, which is prepared by mixing a polymer matrix material, a heterojunction filler, a bacterial cellulose soft filler and a lithium salt to obtain a membrane liquid, and then coating and drying to obtain a light-excited regulated heterojunction solid electrolyte membrane, wherein: the polymer matrix material is preferably polyethylene oxide, and the average molecular weight is about 5,000,000. The heterojunction filler is a composite material of cobalt tetroxide and titanium dioxide. The mechanism of action of the light-excited regulated heterojunction solid electrolyte membrane in the present invention is as follows Figure 1 As shown: In the traditional polyethylene oxide solid polymer electrolyte, the dissociation of lithium salts and the migration of lithium ions are hindered, which requires optimized design and construction. Although the introduction of semiconductor fillers can weaken the O-Li +coordination, but lithium ion migration still needs to be further accelerated, which can be achieved by forming a strong and stable photogenerated electric field. The photogenerated electric field generated by the photocatalytically active filler can stimulate the dissociation of lithium salts and accelerate lithium ion migration. Among many photocatalysts, titanium dioxide stands out for its good photocatalytic stability and efficient light absorption performance. Due to the narrow band gap (1.7-2.0 eV), cobalt tetroxide can combine with titanium dioxide to form a heterojunction and construct a built-in electric field, accelerating charge separation and further enhancing the photocatalytic ability. The strong adsorption of lithium ions by cobalt tetroxide helps to enhance the dissociation of lithium salts and produce increased lithium ion flux. Therefore, based on the above-mentioned photoexcitation modulation mechanism, cobalt tetroxide / titanium dioxide heterojunctions are designed as photocatalytically active fillers to enhance the charge transfer kinetics of solid polymer electrolytes.

[0035] The present invention further provides a flexible light-excited battery device, which is assembled from a positive electrode, a negative electrode, a solid electrolyte membrane, a tab and a packaging film, wherein the positive electrode material is lithium iron phosphate (LFP) or lithium nickel cobalt manganese oxide (NCM811), the negative electrode is an ultra-thin metal lithium foil, the solid electrolyte membrane is the above-mentioned light-excited regulated heterojunction solid electrolyte membrane, and the packaging film is a transparent conductive film. Preferably, a transparent indium tin oxide film is used as the packaging film to ensure light transmittance and flexibility. The structure of the battery is as follows Figure 2 shown.

[0036] The present invention is further described in detail below through specific examples.

[0037] Example 1

[0038] In this embodiment, a light-excited regulated heterojunction solid electrolyte membrane is first prepared, and a flexible light-excited battery device is further assembled based on the membrane. The specific operation steps are as follows:

[0039] 1. Add 0.016 mol of cobalt nitrate, 0.004 mol of titanium tetrachloride (mixed with an equal volume of hydrochloric acid solution, the molar ratio of titanium tetrachloride to HCl is 1:1) and 0.01 mol of salicylic acid to 150 mL of deionized water and stir until dissolved to obtain solution A. Prepare 50 mL of 4 mol / L urea solution. Then mix the above two solutions and stir well for 30 minutes. Transfer the solution to an oil bath and stir vigorously at 95°C for 12 hours. Then, centrifuge it (wash it alternately with deionized water 3 times and anhydrous ethanol 3 times) and vacuum dry it at 60°C overnight. After drying, the sample is transferred to a porcelain boat, heated to 350°C in a muffle furnace at a heating rate of 1°C / min, and kept warm for 2 hours to obtain a heterojunction filler cobalt oxide / titanium dioxide. The X-ray diffraction pattern of the resulting heterojunction is as follows Figure 3 As shown in the scanning electron microscope image Figure 4 As shown in the transmission electron microscopy image Figure 5 shown.

[0040] 2. Lithium bis(trifluoromethane)sulfonyl imide (LiTFSI) and polyethylene oxide were dissolved in anhydrous acetonitrile, and the molar ratio of ethylene oxide [EO] to [Li] was fixed at 18:1. Then, the mixture was stirred until it was completely dissolved and no bubbles were generated; cobalt tetraoxide / titanium dioxide was dispersed in the above solution at a mass fraction of 5% in the electrolyte membrane and bacterial cellulose was dispersed in the above solution at a mass fraction of 1% in the electrolyte membrane, and then stirred until it was completely dissolved and the bubbles disappeared to obtain a membrane liquid.

[0041] 3. The above film solution was applied to a polytetrafluoroethylene plate, and then vacuum dried at 60°C for 48 hours to obtain a light-excited regulated heterojunction solid electrolyte membrane, whose X-ray diffraction pattern is as follows: Figure 6 As shown in the scanning electron microscope image Figure 7 shown.

[0042] 4. Cut the purchased indium selenide oxide film with a thickness of 0.125 mm and a square resistance of 5 ohms into a size of 5 cm×3 cm, then ultrasonically clean it with detergent, deionized water, ethanol and acetone in sequence, and vacuum dry it.

[0043] LFP (or NCM811), conductive carbon black and polyvinylidene fluoride binder with a mass ratio of 8:1:1 were mixed in N-methylpyrrolidone solution to form a uniform slurry. A 150-micron film stretching preparation device was used to evenly coat the aluminum foil current collector and vacuum dried at 60°C overnight to obtain the LFP positive electrode or NCM811 positive electrode.

[0044] In a glove box filled with argon, ultra-thin lithium foil (pre-punched), photoexcitation-regulated heterojunction solid electrolyte membrane and LFP positive electrode or NCM811 positive electrode are stacked in sequence, and then packaged with indium tin oxide film on a battery packaging machine, and the flexible photoexcitation soft-pack battery is assembled.

[0045] Comparative Example 1

[0046] Polyethylene oxide and LiTFSI were dissolved in anhydrous acetonitrile, with the ratio of ethylene oxide [EO] to [Li] fixed at 18:1. Stir thoroughly until completely dissolved and no bubbles were generated. Then, the mixed slurry was applied to a polytetrafluoroethylene plate and film-drawn with a film-drawing machine, followed by drying at 60°C for 48 hours to obtain a polyethylene oxide solid electrolyte membrane.

[0047] The solid electrolyte membranes obtained in the above embodiments and comparative examples were subjected to the following performance tests:

[0048] 1. Ionic conductivity: Assemble the “perforated steel sheet||solid electrolyte membrane||perforated steel sheet” structure, use a perforated battery shell (CR2032, 5 mm perforation diameter, CROOD Co., Ltd.) for packaging, and use a xenon lamp cold light source to simulate light irradiation from the perforation to illuminate the solid electrolyte membrane, test the bulk impedance R at different temperatures, and calculate the ionic conductivity σ at different temperatures according to the formula σ=l / RS, where l is the thickness of the film, R is the bulk impedance value, and S is the area of ​​the film.

[0049] Test results such as Figure 8 As shown: the solid electrolyte membrane prepared in Comparative Example 1 has no response to light, and its ionic conductivity at 25°C is 0.00305 mS / cm; the solid electrolyte membrane prepared in Example 1 has an ionic conductivity of 0.029 mS / cm at 25°C in the absence of light, and an ionic conductivity of 0.135 mS / cm at 25°C in the presence of light.

[0050] In order to eliminate the influence of temperature, the light-excited regulated heterojunction solid electrolyte membrane prepared in Example 1 and the assembled "perforated steel sheet||solid electrolyte membrane||perforated steel sheet" structure were irradiated by a xenon lamp cold light source, and the temperature was monitored in real time using an infrared thermal imaging camera. Fig. 9 As shown, it is confirmed that the light source does not affect the battery temperature.

[0051] 2. Stress-strain test: The electrolyte membrane is prepared as a 3cm×6cm sample. A tensile test machine is used to apply a gradually increasing tensile load to the membrane to cause deformation until it is destroyed. The maximum tensile stress required for the sample to fail is the stress yield strength.

[0052] Test results such as Fig.10 As shown, by comparing Example 1 and Comparative Example 1, it can be seen that the stress strength of the solid electrolyte membrane provided by the present invention is four times that of Comparative Example 1 by adding bacterial cellulose to polyethylene oxide (the stress yield strength of the solid electrolyte membrane obtained in Example 1 is 2 MPa, and the stress yield strength of the solid electrolyte membrane obtained in Comparative Example 1 is 0.5 MPa). Bacterial cellulose acts as a plasticizer, thereby promoting the fluidity of polyethylene oxide chains and the mechanical properties of solid polymer electrolytes.

[0053] 3. Ion migration number detection: Assemble a symmetrical battery with the structure of "perforated lithium||solid electrolyte membrane||perforated lithium", and clamp the two sides with perforated steel sheets, and use a perforated battery shell (CR2032, 5 mm opening diameter, CROOD Co., Ltd.) for packaging. The opening positions of the lithium sheet steel sheet and the battery shell are consistent to ensure that the light source can irradiate the solid electrolyte membrane. Place it on an electrochemical workstation for testing, and irradiate the solid electrolyte membrane from the opening with a xenon lamp cold light source. The results show that the ion migration number of the solid electrolyte membrane obtained in Example 1 is 0.37 at 25°C under no light conditions and 0.46 at 25°C under light conditions; the solid electrolyte membrane obtained in Comparative Example 1 has no response to light, and its ion migration number at 25°C is 0.15.

[0054] 4. Cycle number detection: Place the flexible light-excited soft-pack battery assembled in the above embodiment and the comparative example on the Xinwei test software, set the charge and discharge rate, cut-off voltage and other test conditions and start the test. At the same time, irradiate the solid electrolyte membrane through the punched position of the ultra-thin lithium foil through a xenon lamp cold light source or natural light, and wait for the cycle.

[0055] Under the irradiation of xenon lamp cold light source, the cycle performance curve of the soft pack battery assembled with NCM811 positive electrode is as follows Fig.11 As shown in the figure, at a current density of 0.2C, the battery can be stably cycled for more than 250 times, providing a specific capacity of 161.9 mAh / g at the 100th cycle. Under natural light, the cycle performance curve of the soft-pack battery assembled with LFP positive electrode is as follows: Fig.12 As shown, at a current density of 0.2C, the battery can be stably cycled for more than 110 times without external stress and natural light conditions.

[0056] In summary, the excellent performance of photoexcitation-regulated heterojunction solid electrolyte membrane in solid polymer batteries can be maintained at high ionic conductivity, high electrochemical stability and good mechanical strength.

[0057] It will be easily understood by those skilled in the art that the above embodiments are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A photo-induced heterojunction solid electrolyte membrane, Features: The light-excitation-regulated heterojunction solid electrolyte membrane is made of a polymer matrix material, a heterojunction filler, a bacterial cellulose soft filler and a lithium salt.

2. The light-excited regulated heterojunction solid electrolyte membrane according to claim 1, Features: The polymer matrix material is one or more of polyethylene oxide, polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene.

3. The light-excited regulated heterojunction solid electrolyte membrane according to claim 2, Features: The polymer matrix material is polyethylene oxide.

4. The light-excited regulated heterojunction solid electrolyte membrane according to claim 1, Features: The heterojunction filler is a composite material of cobalt tetroxide and titanium dioxide.

5. The light-excited regulated heterojunction solid electrolyte membrane according to claim 1 or 4, Features: The content of the heterojunction filler accounts for 1%-10% of the total mass of the solid electrolyte membrane.

6. The light-excited regulated heterojunction solid electrolyte membrane according to claim 1, Features: The content of the bacterial cellulose soft filler accounts for 0.3%-1.3% of the total mass of the solid electrolyte membrane.

7. The light-excited regulated heterojunction solid electrolyte membrane according to claim 4, It is characterized in that The preparation method of the heterojunction filler is as follows: cobalt nitrate, titanium tetrachloride, HCl and salicylic acid are added into deionized water in a molar ratio of 8:2:2:4-6 and stirred until dissolved to obtain solution A; a urea solution is prepared at the same time; solution A is mixed with the urea solution in a molar ratio of cobalt nitrate to urea of ​​1:10-15, the mixture is treated in an oil bath at 90-120°C, centrifuged and dried, and then annealed in a muffle furnace at 300-400°C to obtain the heterojunction filler.

8. The light-excited regulated heterojunction solid electrolyte membrane according to claim 1, Features: The thickness of the light-excited regulated heterojunction solid electrolyte film is 50-100 microns.

9. A method for preparing the light-excited regulated heterojunction solid electrolyte membrane according to any one of claims 1 to 8, Features: The polymer matrix material, the heterojunction filler, the bacterial cellulose soft filler and the lithium salt are mixed in a solvent to obtain a membrane liquid, and then the light-excitation-regulated heterojunction solid electrolyte membrane is obtained by coating and drying.

10. A flexible light-excited battery device, Features: The invention is assembled from a positive electrode, a negative electrode, a solid electrolyte membrane, a tab and a packaging film, wherein the solid electrolyte membrane is the light-excited regulated heterojunction solid electrolyte membrane according to any one of claims 1 to 8.

11. The flexible light-excited battery device according to claim 10, Features: The packaging film is a transparent conductive film.

Citation Information

Cited By

  • Light-driven solid-state electrolyte membrane and integrated flexible light-assisted solid-state sodium metal battery based on light-driven solid-state electrolyte membrane

    CN119833728A

  • A light-driven solid-state electrolyte membrane and integrated flexible light-assisted solid sodium metal battery based thereon

    CN119833728B