Sodium ion solid electrolyte material and preparation method and application thereof

By doping salt into the NASICON solid electrolyte, the problems of instability and low ionic conductivity of metallic sodium are solved, the performance of the sodium ion solid electrolyte is improved, the life of the battery is extended and the overall performance is improved.

CN118738533APending Publication Date: 2024-10-01UNIV OF CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410925857.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

NASICON type solid electrolyte has problems with metallic sodium instability and low ionic conductivity in sodium batteries, which leads to the destruction of the electrolyte structure and the growth of sodium dendrites, affecting the cycle life and performance of the battery.

Method used

By doping salt (such as sodium hexafluorosilicate, silicon manganese bromide, etc.) into NASICON, the ionic conductivity and interface stability of the sodium ion solid electrolyte can be improved, and the interface impedance between metallic sodium and the electrolyte can be improved.

Benefits of technology

Significantly improve the ionic conductivity and interface stability of the sodium ion solid electrolyte, reduce the interface impedance, extend the cycle life of the battery and improve the overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738533A_ABST
    Figure CN118738533A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of energy storage materials, and discloses a sodium ion solid electrolyte material and a preparation method and application thereof. The chemical formula of the sodium ion solid electrolyte material is NASICON-yMAX, the NASICON is a sodium super ion conductor, and the MAX is doped salt; in MAX, M is selected from one of Na, K, Pb, Zn, Cu, Ca, Fe and Mn, A is selected from one of Si, B, C and P, and X is selected from one of F, Cl, Br and I; y is the mass percent of MAX in the NASICON, and the value of y is 0.1%-50%. According to the sodium ion solid electrolyte material provided by the invention, the ionic conductivity of the NASICON solid electrolyte can be effectively improved, the interface stability of Na metal and the NASICON solid electrolyte is improved, and the interface impedance is reduced. The sodium-ion solid electrolyte material provided by the invention can be widely applied to sodium-ion batteries so as to improve the performance of the solid-state sodium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of energy storage materials, and in particular relates to a sodium ion solid electrolyte material and a preparation method and application thereof. Background Art

[0002] With the rapid development of the electric vehicle industry, sodium-ion batteries have become a research hotspot in the field of energy storage due to their cost-effectiveness and resource abundance. However, the liquid electrolytes used in them have the risk of thermal runaway and fire and explosion, which limits their use in application scenarios with high safety requirements. Therefore, the development of solid electrolytes with high thermal stability to replace flammable liquid electrolytes has become an important direction of current research. Solid electrolytes can not only significantly improve the thermal safety of batteries, but also effectively inhibit the growth of sodium dendrites, thereby extending the cycle life of the battery and improving its overall performance. Currently, commonly used solid electrolytes are mainly divided into sulfides, halides, polymers and oxides. Among the many electrolytes, oxide Na + Superionic conductor (NASICON) solid electrolytes have aroused great interest due to their advantages such as three-dimensional ion transport framework and easy synthesis. However, NASICON electrolytes mainly have the problems of instability to sodium metal and low ionic conductivity. This is because the PO4 / SiO4 tetrahedrons present in the NASICON structure can easily react with metallic sodium to form substances such as phosphates / silicates or sodium phosphide, which in turn continuously destroy the structure of the electrolyte, leading to the formation of sodium dendrites inside the electrolyte structure, causing the solid-state sodium battery to fail. Therefore, it is urgent to provide a method for enhancing the stability of NASICON electrolytes to metallic sodium and improving ionic conductivity to improve the performance of solid-state sodium batteries. Summary of the invention

[0003] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a sodium ion solid electrolyte material and a preparation method and application thereof. The sodium ion solid electrolyte material provided by the present invention can effectively improve the ionic conductivity of the NASICON solid electrolyte, improve the interface stability between the Na metal and the NASICON solid electrolyte, and reduce the interface impedance.

[0004] The invention provides a sodium ion solid electrolyte material.

[0005] Specifically, a sodium ion solid electrolyte material has a chemical formula of NASICON-yMAX, wherein NASICON is a sodium superion conductor, and MAX is a doped salt (i.e., MAX salt); in the MAX, M is selected from one of Na, K, Pb, Zn, Cu, Ca, Fe, and Mn, A is selected from one of Si, B, C, and P, and X is one of F, Cl, Br, and I; y is the mass percentage of the MAX in the NASICON, and the value of y is 0.1% to 50%.

[0006] A sodium ion solid electrolyte material comprises NASICON (sodium super ion conductor) and MAX salt; the mass of the MAX salt is 0.1% to 50% of the mass of the NASICON.

[0007] In some embodiments of the present invention, the NASICON (sodium superionic conductor) is Na3Zr2Si2PO 12 The chemical formula of the sodium ion solid electrolyte material is Na3Zr2Si2PO 12 -yMAX, wherein y is the mass percentage of the MAX in the NASICON.

[0008] In some embodiments of the present invention, the mass of the MAX is 0.1% to 15% of the mass of the NASICON, such as Na3Zr2Si2PO 12 -(0.1% to 15%) MAX. In some embodiments of the present invention, the mass of the MAX is 0.3% to 10% of the mass of the NASICON, such as Na3Zr2Si2PO 12 -(0.3% to 10%) MAX. In some embodiments of the present invention, the mass of the MAX is 0.3% to 3.0% of the mass of the NASICON, such as Na3Zr2Si2PO 12 -(0.3% to 3.0%) MAX. In some embodiments of the present invention, the mass of the MAX is 0.3% to 2.0% of the mass of the NASICON, such as Na3Zr2Si2PO 12 -(0.3% to 2.0%) MAX. In some embodiments of the present invention, the mass of the MAX is 0.3% to 0.8% of the mass of the NASICON, such as Na3Zr2Si2PO 12 -(0.3%~0.8%)MAX.

[0009] In some embodiments of the present invention, the MAX salt includes at least one of sodium hexafluorosilicate (Na2SiF6), potassium iodide (KSiI3), bromomethyl iron (FeCBr), trichloromethyl copper (CuCCl3), sodium phosphine hexachloride (NaPCl6), lead hexafluorophosphate (Pb(PF6)2), calcium tetrafluoroborate (CaBF4), manganese silicobromide (MnSiBr3), zinc fluorosilicate (ZnSiF6), and sodium fluoride (NaF). Preferably, the MAX salt is sodium hexafluorosilicate or calcium tetrafluoroborate (CaBF4).

[0010] The present invention also provides a method for preparing the sodium ion solid electrolyte material.

[0011] Specifically, the preparation method of the above-mentioned sodium ion solid electrolyte material comprises the following steps:

[0012] The Na source, P source, Zr source, Si source and ball milling agent are mixed, ball milled and then calcined to prepare NASICON precursor; the NASICON precursor is then mixed with MAX salt, tableted and sintered to prepare sodium ion solid electrolyte material.

[0013] In some embodiments of the present invention, the Na source can be selected from at least one of sodium carbonate (Na2CO3), sodium hydroxide (NaOH), sodium oxide (Na2O), sodium sulfate (Na2SO4), sodium nitrate (NaNO3), sodium phosphate (Na3PO4), and sodium chloride. The Si source is selected from at least one of silicon dioxide (SiO2), silicon sulfate, silicon carbonate, silicon nitrate, and silicon oxalate. The P source is selected from at least one of ammonium dihydrogen phosphate (NH4H2PO4), ammonium phosphate, and diammonium hydrogen phosphate. The Zr source is selected from at least one of zirconium dioxide (ZrO2), zirconium oxynitrate, zirconium sulfate, zirconium chloride, zirconium oxalate, and zirconium acetate.

[0014] In some embodiments of the present invention, the ball milling agent includes at least one selected from ethanol, propanol, isopropanol, dichloromethane, ethyl acetate, acetone, and chloroform.

[0015] In some embodiments of the present invention, during the ball milling process, ball milling beads are added for ball milling, and the total mass ratio of the Na source, the P source, the Zr source, and the Si source to the ball milling beads and the ball milling agent is 1: (1-30): (5-15). That is, the mass ratio of the material to the ball milling beads and the ball milling agent is 1: (1-30): (5-15).

[0016] In some embodiments of the present invention, the ball milling process is: ball milling at a rotation speed of 100 to 2000 r / min for 1 to 48 hours; preferably, the ball milling process is: ball milling at a rotation speed of 200 to 1300 r / min for 2 to 25 hours.

[0017] In some embodiments of the present invention, the calcination process is: calcination at 100-1500° C. for 1-48 h; preferably, the calcination process is: calcination at 500-1300° C. for 5-36 h.

[0018] In some embodiments of the present invention, the sintering temperature is 500-2000° C.; preferably, the sintering temperature is 700-1600° C. In some embodiments of the present invention, the sintering time is 1 h-48 h; preferably, the sintering time is 5-24 h.

[0019] The present invention also provides the use of the above sodium ion solid electrolyte material in the preparation of a sodium ion battery.

[0020] The present invention also provides a sodium ion battery comprising the sodium ion solid electrolyte material.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The sodium ion solid electrolyte material provided by the present invention has a chemical formula of NASICON-yMAX, which includes a sodium superion conductor and a MAX salt. The present invention can avoid the destruction of the electrolyte PO4 / SiO4 tetrahedron by metal Na during the operation of the NASICON solid electrolyte by the halogen X element doped into the PO4 / SiO4 tetrahedron, thereby effectively improving the stability of the metal Na to the solid electrolyte. Furthermore, the M metal element and the A non-metal element can change the ratio of Si / P in NASICON, thereby effectively improving the ionic conductivity of the NASICON solid electrolyte. In addition, the addition of MAX can effectively improve the interfacial stability of the Na metal and the NASICON solid electrolyte, greatly reducing the interfacial impedance (especially the addition of sodium hexafluorosilicate).

[0023] (2) The sodium ion solid electrolyte material provided by the present invention has high ionic conductivity and low interface impedance, and can be widely used in sodium ion batteries to improve the performance of solid-state sodium batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 XRD pattern of the composite NASICON solid electrolyte sheet prepared in Example 1;

[0025] Figure 2 Sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet prepared in Example 1;

[0026] Figure 3 XRD pattern of the composite NASICON solid electrolyte sheet prepared in Example 2;

[0027] Figure 4 Sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet prepared in Example 2;

[0028] Figure 5 XRD pattern of the composite NASICON solid electrolyte sheet prepared in Example 3;

[0029] Figure 6 Sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet prepared in Example 3;

[0030] Figure 7 XRD pattern of the composite NASICON solid electrolyte sheet prepared in Example 4;

[0031] Figure 8 Sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet prepared in Example 4;

[0032] Fig. 9 XRD pattern of the composite NASICON solid electrolyte sheet prepared in Example 5;

[0033] Fig.10 Sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet prepared in Example 5;

[0034] Fig.11 XRD pattern of the composite NASICON solid electrolyte sheet prepared in Example 6;

[0035] Fig.12 Sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet prepared in Example 6;

[0036] Fig.13 Impedance test diagram of the sodium symmetric battery prepared in Example 6;

[0037] Fig.14 Sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet prepared in Example 7;

[0038] Fig.15 Sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet prepared in Example 8;

[0039] Fig.16 XRD pattern of pure NASICON solid electrolyte sheet prepared in Comparative Example 1;

[0040] Fig.17 Sodium ion conductivity diagram of pure NASICON solid electrolyte sheet prepared in Comparative Example 1;

[0041] Fig.18Impedance test diagram of the sodium symmetric battery prepared in Comparative Example 1. DETAILED DESCRIPTION

[0042] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0043] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0044] Example 1

[0045] A sodium ion solid electrolyte material, the chemical formula of which is Na3Zr2Si2PO 12 -10% MnSiBr3. It includes NASICON and silicomanganese bromide, and the added amount of silicomanganese bromide is 10% of the mass of NASICON.

[0046] A method for preparing a sodium ion solid electrolyte material comprises the following steps:

[0047] According to the chemical formula, the ratio of Na3Zr2Si2PO 12 Sodium carbonate, zirconium dioxide, silicon dioxide and ammonium dihydrogen phosphate were weighed and placed in an agate ball mill. Ethanol was used as a ball milling agent and the ball milling was performed at a speed of 1200r / min for 4h. The mixed slurry was then placed in a 60℃ oven and dried for 10h to obtain a dry mixed powder. The mixed powder was then sintered at 1100℃ for 10h to obtain the NASICON precursor Na3Zr2Si2PO 12 The powder was then mixed with silicon manganese bromide and pressed into a 15 mm diameter disc, which was sintered at 1200 °C for 8 h to obtain a composite NASICON solid electrolyte sheet (i.e., sodium ion solid electrolyte material). After polishing, the impedance was tested using an electrochemical workstation and the diffraction pattern was analyzed. The XRD pattern of the composite NASICON solid electrolyte sheet is shown in Figure 2. Figure 1 As shown, Figure 2 This is the sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet. Its sodium ion conductivity is 3.8x10 -4 Scm -1 The NASICON solid electrolyte was assembled into a sodium symmetric battery, and the interface impedance was tested using an electrochemical workstation. The total impedance was 423Ωcm 2 .

[0048] Example 2

[0049] A sodium ion solid electrolyte material, the chemical formula of which is Na3Zr2Si2PO 12-5% Pb(PF6)2. It includes NASICON and lead hexafluorophosphate Pb(PF6)2, and the amount of lead hexafluorophosphate added is 5% of the mass of NASICON.

[0050] A method for preparing a sodium ion solid electrolyte material comprises the following steps:

[0051] According to the chemical formula, the ratio of Na3Zr2Si2PO 12 Sodium carbonate, zirconium dioxide, silicon dioxide and ammonium dihydrogen phosphate were weighed and placed in an agate ball mill. Chloroform was used as a ball milling agent and the ball milling was performed at a speed of 200 r / min for 24 hours. The mixed slurry was then placed in a 60°C oven and dried for 10 hours to obtain a dry mixed powder. The mixed powder was then sintered at 600°C for 30 hours to obtain the NASICON precursor Na3Zr2Si2PO 12 The powder was then mixed with lead hexafluorophosphate and pressed into a 15 mm diameter disc, which was sintered at 800 °C for 36 h to obtain a composite NASICON solid electrolyte sheet. After polishing, the impedance was tested using an electrochemical workstation and the diffraction pattern was analyzed. The XRD pattern of the composite NASICON solid electrolyte sheet is shown in Figure 2. Figure 3 As shown, Figure 4 This is the sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet. Its sodium ion conductivity is 5.2x10 -4 Scm -1 The composite NASICON solid electrolyte sheet was assembled into a sodium symmetric battery, and the interface impedance test was performed using an electrochemical workstation. The total impedance was 346Ωcm 2 .

[0052] Example 3

[0053] A sodium ion solid electrolyte material, the chemical formula of which is Na3Zr2Si2PO 12 -3% FeCBr. It includes NASICON and bromomethyl iron, and the amount of bromomethyl iron added is 3% of the mass of NASICON.

[0054] A method for preparing a sodium ion solid electrolyte material comprises the following steps:

[0055] According to the chemical formula, the ratio of Na3Zr2Si2PO 12 Sodium carbonate, zirconium dioxide, silicon dioxide and ammonium dihydrogen phosphate were weighed and placed in an agate ball mill. Acetone was used as a ball milling agent and the ball milling was performed at a speed of 1100 r / min for 6 hours. The mixed slurry was then placed in a 60°C oven and dried for 10 hours to obtain a dry mixed powder. The mixed powder was then sintered at 900°C for 20 hours to obtain the NASICON precursor Na3Zr2Si2PO 12The powder was then mixed with bromomethyl iron and pressed into a 15 mm diameter disc, which was sintered at 1300 °C for 6 h to obtain a composite NASICON solid electrolyte sheet. After polishing, the impedance was tested using an electrochemical workstation and the diffraction pattern was analyzed. The XRD pattern of the composite NASICON solid electrolyte sheet is shown in Figure 2. Figure 5 As shown, Figure 6 This is the sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet. Its sodium ion conductivity is 6.7x10 -4 Scm -1 The composite NASICON solid electrolyte sheet was assembled into a sodium symmetric battery, and the interface impedance test was performed using an electrochemical workstation. The total impedance was 274Ωcm 2 .

[0056] Example 4

[0057] A sodium ion solid electrolyte material, the chemical formula of which is Na3Zr2Si2PO 12 -2% CaBF4. It includes NASICON and calcium tetrafluoroborate, and the added amount of calcium tetrafluoroborate is 2% of the mass of NASICON.

[0058] A method for preparing a sodium ion solid electrolyte material comprises the following steps:

[0059] According to the chemical formula, the ratio of Na3Zr2Si2PO 12 Sodium carbonate, zirconium dioxide, silicon dioxide and ammonium dihydrogen phosphate were weighed and placed in an agate ball mill. Ethyl acetate was used as a ball milling agent and the ball milling was performed at a speed of 1300 r / min for 2 hours. The mixed slurry was then placed in a 60°C oven and dried for 10 hours to obtain a dry mixed powder. The mixed powder was then sintered at 1200°C for 6 hours to obtain the NASICON precursor Na3Zr2Si2PO 12 The powder was then mixed with calcium tetrafluoroborate and pressed into a 15 mm diameter disc, which was sintered at 1400 °C for 16 h to obtain a composite NASICON solid electrolyte sheet. After polishing, the impedance was tested using an electrochemical workstation and the diffraction pattern was analyzed. The XRD pattern of the composite NASICON solid electrolyte sheet is shown in Figure 2. Figure 7 As shown, Figure 8 This is the sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet. Its sodium ion conductivity is 9.2x10 -4 Scm -1 The composite NASICON solid electrolyte sheet was assembled into a sodium symmetric battery, and the interface impedance test was performed using an electrochemical workstation. The total impedance was 196Ωcm 2 .

[0060] Example 5

[0061] A sodium ion solid electrolyte material, the chemical formula of which is Na3Zr2Si2PO 12 -1% KSiI3. It includes NASICON and potassium iodide of silicon, and the added amount of potassium iodide of silicon is 1% of the mass of NASICON.

[0062] A method for preparing a sodium ion solid electrolyte material comprises the following steps:

[0063] According to the chemical formula, the ratio of Na3Zr2Si2PO 12 Sodium carbonate, zirconium dioxide, silicon dioxide and ammonium dihydrogen phosphate were weighed and placed in an agate ball mill. Dichloromethane was used as a ball milling agent and the ball milling was carried out at a speed of 900 r / min for 20 hours. The mixed slurry was then placed in a 60°C oven and dried for 10 hours to obtain a dry mixed powder. The mixed powder was then sintered at 800°C for 15 hours to obtain the NASICON precursor Na3Zr2Si2PO 12 The powder was then mixed with potassium silicon iodide and pressed into a 15 mm diameter disc, which was sintered at 1200 °C for 24 h to obtain a composite NASICON solid electrolyte sheet. After polishing, the impedance was tested using an electrochemical workstation and the diffraction pattern was analyzed. The XRD pattern of the composite NASICON solid electrolyte sheet is shown in Figure 2. Fig. 9 As shown, Fig.10 This is the sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet. Its sodium ion conductivity is 7.8x10 -4 Scm -1 The composite NASICON solid electrolyte sheet was assembled into a sodium symmetric battery, and the interface impedance was tested using an electrochemical workstation. The total impedance was 177Ωcm 2 .

[0064] Example 6

[0065] A sodium ion solid electrolyte material, the chemical formula of which is Na3Zr2Si2PO 12 -0.5% Na2SiF6. It includes NASICON and sodium fluoride silicate, and the amount of sodium fluoride silicate added is 0.5% of the mass of NASICON.

[0066] A method for preparing a sodium ion solid electrolyte material comprises the following steps:

[0067] According to the chemical formula, the ratio of Na3Zr2Si2PO 12Sodium carbonate, zirconium dioxide, silicon dioxide and ammonium dihydrogen phosphate were weighed and placed in an agate ball mill. Isopropyl alcohol was used as a ball milling agent and the ball milling was performed at a speed of 400 r / min for 12 hours. The mixed slurry was then placed in a 60°C oven and dried for 10 hours to obtain a dry mixed powder. The mixed powder was then sintered at 1000°C for 12 hours to obtain the NASICON precursor Na3Zr2Si2PO 12 The powder was then mixed with sodium fluoride silicate and pressed into a 15 mm diameter disc, which was sintered at 1250 °C for 12 h to obtain a composite NASICON solid electrolyte sheet. After polishing, the impedance was tested using an electrochemical workstation and the diffraction pattern was analyzed. The XRD pattern of the composite NASICON solid electrolyte sheet is shown in Figure 2. Fig.11 As shown, Fig.12 This is the sodium ion conductivity diagram of the composite NASICON solid electrolyte sheet, and its sodium ion conductivity is 1.2x10 -3 Scm -1 .

[0068] The composite NASICON solid electrolyte sheet in Example 6 was assembled into a sodium symmetric battery, and the interface impedance test was performed using an electrochemical workstation. The results are as follows: Fig.13 As shown, the total impedance is only 85Ωcm 2 , indicating that the interface contact is close and the interface stability is good.

[0069] Example 7

[0070] A sodium ion solid electrolyte material, the chemical formula of which is Na3Zr2Si2PO 12 -0.3% Na2SiF6. It includes NASICON and sodium fluoride silicate, and the amount of sodium fluoride silicate added is 0.3% of the mass of NASICON.

[0071] A method for preparing a sodium ion solid electrolyte material comprises the following steps:

[0072] According to the chemical formula, the ratio of Na3Zr2Si2PO 12 Sodium carbonate, zirconium dioxide, silicon dioxide and ammonium dihydrogen phosphate were weighed and placed in an agate ball mill. Isopropyl alcohol was used as a ball milling agent and the ball milling was performed at a speed of 400 r / min for 12 hours. The mixed slurry was then placed in a 60°C oven and dried for 10 hours to obtain a dry mixed powder. The mixed powder was then sintered at 1000°C for 12 hours to obtain the NASICON precursor Na3Zr2Si2PO 12 The powder was then mixed with sodium fluoride silicate and pressed into a disc with a diameter of 15 mm. The disc was sintered at 1250 ° C for 12 h to obtain a composite NASICON solid electrolyte sheet. After polishing, the impedance was tested using an electrochemical workstation, such as Fig.14As shown, its sodium ion conductivity is 9.1x10 -4 Scm -1 The composite NASICON solid electrolyte sheet was assembled into a sodium symmetric battery, and the interface impedance test was performed using an electrochemical workstation. The total impedance was 108Ωcm 2 .

[0073] Example 8

[0074] A sodium ion solid electrolyte material, the chemical formula of which is Na3Zr2Si2PO 12 -1.0% Na2SiF6. It includes NASICON and sodium fluorosilicate, and the amount of sodium fluorosilicate added is 1.0% of the mass of NASICON.

[0075] A method for preparing a sodium ion solid electrolyte material comprises the following steps:

[0076] According to the chemical formula, the ratio of Na3Zr2Si2PO 12 Sodium carbonate, zirconium dioxide, silicon dioxide and ammonium dihydrogen phosphate were weighed and placed in an agate ball mill. Isopropyl alcohol was used as a ball milling agent and the ball milling was performed at a speed of 400 r / min for 12 hours. The mixed slurry was then placed in a 60°C oven and dried for 10 hours to obtain a dry mixed powder. The mixed powder was then sintered at 1000°C for 12 hours to obtain the NASICON precursor Na3Zr2Si2PO 12 The powder was then mixed with sodium fluoride silicate and pressed into a disc with a diameter of 15 mm. The disc was sintered at 1250 ° C for 12 h to obtain a composite NASICON solid electrolyte sheet. After polishing, the impedance was tested using an electrochemical workstation, such as Fig.15 As shown, its sodium ion conductivity is 6.4x10 -4 Scm -1 The composite NASICON solid electrolyte sheet was assembled into a sodium symmetric battery, and the interface impedance test was performed using an electrochemical workstation. The total impedance was 122Ωcm 2 .

[0077] Example 9

[0078] A sodium ion solid electrolyte material, the chemical formula of which is Na3Zr2Si2PO 12 -0.5% NaF. It includes NASICON and sodium fluoride, and the added amount of sodium fluoride is 0.5% of the mass of NASICON.

[0079] A method for preparing a sodium ion solid electrolyte material comprises the following steps:

[0080] According to the chemical formula, the ratio of Na3Zr2Si2PO 12Sodium carbonate, zirconium dioxide, silicon dioxide and ammonium dihydrogen phosphate were weighed and placed in an agate ball mill. Isopropyl alcohol was used as a ball milling agent and the ball milling was performed at a speed of 400 r / min for 12 hours. The mixed slurry was then placed in a 60°C oven and dried for 10 hours to obtain a dry mixed powder. The mixed powder was then sintered at 1000°C for 12 hours to obtain the NASICON precursor Na3Zr2Si2PO 12 The powder was then mixed with sodium fluoride and pressed into a 15 mm diameter disc. The disc was sintered at 1250 °C for 12 h to obtain a composite NASICON solid electrolyte sheet. After polishing, the impedance was tested using an electrochemical workstation. The sodium ion conductivity was 8.6x10 -4 Scm -1 The composite NASICON solid electrolyte was assembled into a sodium symmetric battery, and the interface impedance was tested using an electrochemical workstation. The total impedance was 168Ωcm 2 .

[0081] Comparative Example 1

[0082] Study the ionic conductivity of pure NASICON solid electrolyte.

[0083] According to the chemical formula, the ratio of Na3Zr2Si2PO 12 Sodium carbonate, zirconium dioxide, silicon dioxide and ammonium dihydrogen phosphate were weighed and placed in an agate ball mill. Propanol was used as a ball milling agent and the ball milling was carried out at a speed of 400 r / min for 12 hours. The mixed slurry was then placed in a 60°C oven and dried for 10 hours to obtain a dry mixed powder. The mixed powder was then sintered at 1000°C for 12 hours to obtain the NASICON precursor Na3Zr2Si2PO 12 The powder was then mixed with potassium silicon iodide and pressed into a 15 mm diameter disc, which was sintered at 1250°C for 12 hours to obtain a pure NASICON solid electrolyte sheet. After polishing, the impedance was tested using an electrochemical workstation and the diffraction pattern was analyzed. The XRD pattern of the pure NASICON solid electrolyte sheet is shown in Figure 2. Fig.16 As shown, Fig.17 This is the sodium ion conductivity diagram of pure NASICON solid electrolyte sheet, and its sodium ion conductivity is 1.6x10 -4 Scm -1 .

[0084] The NASICON solid electrolyte sheet in Comparative Example 1 was assembled into a sodium symmetric battery, and the interface impedance test was performed using an electrochemical workstation. The results are as follows: Fig.18 As shown, the total impedance is only 700Ωcm 2 , indicating that a large number of side reactions occurred at its interface and the interface stability was poor.

[0085] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A sodium ion solid electrolyte material, characterized in that: The chemical formula is NASICON-yMAX, wherein NASICON is a sodium superionic conductor, and MAX is a doped salt; in the MAX, M is selected from one of Na, K, Pb, Zn, Cu, Ca, Fe, and Mn, A is selected from one of Si, B, C, and P, and X is one of F, Cl, Br, and I; y is the mass percentage of the MAX to the NASICON, and the value of y is 0.1% to 50%.

2. The sodium ion solid electrolyte material according to claim 1, characterized in that The NASICON is Na3Zr2Si2PO 12 The chemical formula of the sodium ion solid electrolyte material is Na3Zr2Si2PO 12 -yMAX.

3. The sodium ion solid electrolyte material according to claim 1 or 2, characterized in that The mass of the MAX is 0.1% to 15% of the mass of the NASICON; preferably, the mass of the MAX is 0.3% to 10% of the mass of the NASICON.

4. The sodium ion solid electrolyte material according to claim 1 or 2, characterized in that The MAX includes at least one of sodium hexafluorosilicate, potassium iodide, bromomethyl iron, trichloromethyl copper, sodium phosphine hexachloride, lead hexafluorophosphate, calcium tetrafluoroborate, manganese silicobromide, zinc fluorosilicate, and sodium fluoride.

5. The method for preparing the sodium ion solid electrolyte material according to any one of claims 1 to 4, characterized in that: The following steps are involved: The Na source, P source, Zr source, Si source and ball milling agent are mixed, ball milled and then calcined to prepare NASICON precursor; the NASICON precursor is then mixed with MAX salt, tableted and sintered to prepare sodium ion solid electrolyte material.

6. The preparation method according to claim 5, characterized in that: The Na source is selected from at least one of sodium carbonate, sodium hydroxide, sodium oxide, sodium sulfate, sodium nitrate, sodium phosphate, and sodium chloride; the Si source is selected from at least one of silicon dioxide, silicon sulfate, silicon carbonate, silicon nitrate, and silicon oxalate; the P source is selected from at least one of ammonium dihydrogen phosphate, ammonium phosphate, and diammonium hydrogen phosphate; the Zr source is selected from at least one of zirconium dioxide, zirconium oxynitrate, zirconium sulfate, zirconium chloride, zirconium oxalate, and zirconium acetate.

7. The preparation method according to claim 5 or 6, characterized in that: The ball milling agent comprises at least one selected from ethanol, propanol, isopropanol, dichloromethane, ethyl acetate, acetone and chloroform.

8. The preparation method according to claim 5 or 6, characterized in that: The calcination process is as follows: calcination at 100-1500° C. for 1-48 hours; the sintering temperature is 500-2000° C., and the sintering time is 1 hour to 48 hours.

9. Use of the sodium ion solid electrolyte material according to any one of claims 1 to 4 in the preparation of a sodium ion battery.

10. A sodium ion battery, characterized in that: The sodium ion battery comprises the sodium ion solid electrolyte material according to any one of claims 1 to 4.