Electrolyte, battery and electronic device

By adding negative electrode film-forming additives, bifunctional additives and low-resistance additives to the lithium-ion battery electrolyte, a stable SEI film is formed, which solves the problem of FEC being easily oxidized and decomposed at high temperatures, and significantly improves the cycle stability of lithium-ion batteries. and high temperature performance.

CN118738562AInactive Publication Date: 2024-10-01JIANGSU PUDI LMPORT EXPORT CO LTD

Patent Information

Application Number
CN202411235863.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In lithium-ion batteries, FEC is easily oxidized and decomposed at high temperatures, causing the SEI film to dissolve, increasing the acidity of the electrolyte, causing high gas production, and deteriorating the high-temperature performance of the battery.

Method used

An electrolyte is used that contains organic solvents, lithium salts and specific additives, including negative electrode film-forming additives, bifunctional additives and low-resistance additives. Through the combined use of these additives, a stable SEI film is formed, reducing irreversible reactions and reducing production. gas, inhibiting battery expansion and improving cycle stability.

Benefits of technology

Significantly reduce the irreversible reaction of lithium-ion batteries, extend the cycle life, improve the high-temperature cycle and storage performance of the battery, reduce gas production, enhance interface stability, and improve low-temperature discharge performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

In order to solve the problems that in a high FEC system, FEC is easy to oxidize and decompose at a high temperature, an SEI film is dissolved, the acidity of an electrolyte is increased, the gas production rate is high, and high-temperature storage is deteriorated, the invention provides an electrolyte, a battery and an electronic device, and the electrolyte comprises an organic solvent, a lithium salt and an additive, the additives comprise a negative electrode film-forming additive, a bifunctional additive and a low-impedance additive, and the negative electrode film-forming additive comprises vinylene carbonate and 1, 3-propane sultone; the bifunctional additive is adiponitrile; the low-impedance additive is ethylene sulfate; based on the total mass of the electrolyte being 100%, the mass of the additive accounts for 1%-10% of the total mass of the electrolyte; according to the electrolyte provided by the invention, a low-impedance SEI film can be formed on the surface of a negative electrode, high-temperature gas production is inhibited, the interface stability is improved, side reactions are reduced, and the battery performance is improved; the internal resistance of the battery is reduced, and the high-temperature cycle performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an electrolyte, a battery and an electronic device. Background Art

[0002] In modern society, the core energy source of consumer electronics, electric vehicles, power tools, etc. is lithium-ion batteries, which are due to their advantages of high specific energy density and long cycle life. With the development of science and technology, the energy density of batteries needs to be further improved to meet the demand, but it is difficult to further improve the energy density of lithium-ion batteries without changing the main materials of the positive and negative electrodes.

[0003] Silicon (Si) is considered to be the most promising negative electrode material for the next generation of lithium-ion batteries because of its high theoretical capacity. However, when fully embedded in lithium, silicon expands and contracts by more than 300%, which can cause the SEI membrane to rupture-regenerate-rupture, thereby accelerating electrolyte consumption, causing material particles to pulverize and fall off, and deteriorating electrical performance. In order to alleviate this situation, a large amount of FEC (fluoroethylene carbonate) is often added to the electrolyte, but FEC is thermally unstable and easily oxidized and decomposed, causing the SEI membrane to dissolve at high temperatures, resulting in increased electrolyte acidity, high gas production, and deterioration of the battery's high-temperature performance; therefore, how to overcome the above-mentioned technical problems and defects has become a key issue that needs to be solved. Summary of the invention

[0004] In order to solve the problem that in a high FEC system, FEC is easily oxidized and decomposed at high temperature, causing dissolution of the SEI film, resulting in increased acidity of the electrolyte, high gas production, and deterioration of high-temperature storage, the present invention provides an electrolyte, a battery and an electronic device.

[0005] The technical solution adopted by the present invention to solve the above technical problems is as follows: The first aspect of the present invention provides an electrolyte, comprising an organic solvent, a lithium salt and an additive, wherein the additive comprises a negative electrode film-forming additive, a bifunctional additive and a low-impedance additive, wherein the negative electrode film-forming additive comprises vinylene carbonate and 1,3-propane sultone; the bifunctional additive is adiponitrile; and the low-impedance additive is vinyl sulfate; Taking the total mass of the electrolyte as 100%, the mass of the additive accounts for 1% to 10% of the total mass of the electrolyte; The organic solvent includes fluoroethylene carbonate; taking the total mass of the organic solvent as 100%, the percentage of the fluoroethylene carbonate in the total mass of the organic solvent is 10% to 30%.

[0006] Optionally, taking the total mass of the electrolyte as 100%, the mass of the additive accounts for 2% to 5% of the total mass of the electrolyte.

[0007] Optionally, based on the total mass of the organic solvent being 100%, the percentage of the fluoroethylene carbonate in the total mass of the organic solvent is 15% to 25%.

[0008] Optionally, the feed mass ratio of the negative electrode film-forming additive, the bifunctional additive and the low-impedance additive is 1~4:0.5~2:0.5~2.

[0009] Optionally, the feed mass ratio of the negative electrode film-forming additive, the bifunctional additive and the low-impedance additive is 2~3:1~1.5:1~1.5.

[0010] Optionally, the organic solvent also includes one or more substances selected from the group consisting of fluoroethylene carbonate, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propyl propionate, ethyl propionate, methylpropyl propionate, ethyl acetate, propyl acetate, methyl acetate, methyl butyrate, ethyl butyrate, and propyl butyrate; and the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, and lithium bis(trifluoromethanesulfonyl)imide.

[0011] Optionally, taking the total mass of the electrolyte as 100%, the organic solvent accounts for 60% to 80% of the total mass of the electrolyte, and the lithium salt accounts for 10% to 40% of the total mass of the electrolyte.

[0012] A second aspect of the present invention provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte as described above.

[0013] Optionally, the positive electrode sheet includes a positive electrode active material, and the positive electrode active material is selected from one or more substances of lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate and lithium iron manganese phosphate; the negative electrode sheet includes a negative electrode active material, and the negative electrode active material is selected from Si, Li-Si, SiO x (mit 0≤x≤2), one or more substances selected from SiC, Si-Sn, SiSnFe, SiSnAl, SiFeCo, SnO2.

[0014] A third aspect of the present invention provides an electronic device comprising the lithium-ion battery described above.

[0015] According to the electrolyte provided by the present invention, the present invention uses the negative electrode film-forming additive, the bifunctional additive and the low impedance additive in combination, and utilizes the advantages of each additive and the interaction between them to improve the battery performance. The battery can form a stable SEI film, avoid contact between the electrolyte and the negative electrode material, and continuously decompose the electrolyte, thereby significantly reducing the irreversible reaction of the lithium-ion battery and enhancing its cycle stability; or reducing the gas production of the battery, inhibiting the volume expansion of the battery at high temperature; reducing the interface impedance, improving the positive electrode interface stability, and improving the battery's low-temperature discharge performance, high-temperature cycle and storage performance, etc. DETAILED DESCRIPTION

[0016] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0017] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0018] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.

[0019] In one embodiment, the first aspect of the present invention provides an electrolyte, comprising an organic solvent, a lithium salt and an additive, wherein the additive comprises a negative electrode film-forming additive, a bifunctional additive and a low-impedance additive, wherein the negative electrode film-forming additive comprises vinylene carbonate and 1,3-propane sultone; the bifunctional additive is adiponitrile; the low-impedance additive is vinyl sulfate; Taking the total mass of the electrolyte as 100%, the mass of the additive accounts for 1% to 10% of the total mass of the electrolyte; The organic solvent includes fluoroethylene carbonate; taking the total mass of the organic solvent as 100%, the percentage of the fluoroethylene carbonate in the total mass of the organic solvent is 10% to 30%.

[0020] Specifically, the mass of the additive accounts for a percentage of the total mass of the electrolyte of 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5% or 10%, any one of the values ​​or a range consisting of any two of the values.

[0021] When the mass of the additive accounts for 1% to 10% of the total mass of the electrolyte, it can not only extend the cycle life of the battery and inhibit its expansion behavior at high temperature, but also effectively inhibit the high-temperature gas production of the battery, while improving the room temperature cycle performance and high temperature cycle performance of the battery; when the mass of the additive accounts for less than 1% of the total mass of the electrolyte, the groups cannot react, the passivation film cannot be formed, and the stability of the SEI film will also be affected, resulting in poor cycle performance of the battery, obvious gas production, and battery expansion; when the added mass accounts for more than 10% of the total mass of the electrolyte, the viscosity of the electrolyte will increase, which will have a negative impact on battery performance.

[0022] Specifically, the percentage of the fluoroethylene carbonate in the total mass of the organic solvent is any point value among 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29% or 30%, or a range value consisting of any two point values.

[0023] Specifically, when the percentage of fluoroethylene carbonate in the total mass of the organic solvent is 10-30%, the LUMO energy of FEC is much lower than EC (ethylene carbonate) due to the addition of F element, so FEC decomposes earlier in the electrolyte than the main solvents EC, DMC (dimethyl carbonate), EMC (ethyl methyl carbonate), etc., and the generated interface film contains more LiF components, with high mechanical strength, which can significantly improve the cycle stability of lithium-ion batteries, especially Si-containing lithium-ion batteries; at the same time, it will also form a protective film on the surface of the anode, which can inhibit the reaction of the anode with fluoride ions in the electrolyte; at low temperatures, FEC can reduce the interface impedance and improve the low-temperature performance of the battery; in addition, the SEI film with a high LiF content has a higher surface energy on the surface of metallic lithium, which can promote the uniform deposition of Li and inhibit the growth of dendrites. When the percentage of fluoroethylene carbonate in the total mass of the organic solvent is less than 10%, the cycle stability and low-temperature performance of the battery cannot be effectively improved. When the percentage of fluoroethylene carbonate in the total mass of the organic solvent is greater than 30%, because it will also undergo oxidative polymerization reaction at the positive electrode, when the content is high, it will increase the impedance of the electrolyte and the irreversibility of the positive electrode; and at high temperatures, it will react with LiPF6 and EC (ethylene carbonate), etc., resulting in increased acidity of the electrolyte, high gas production, and deterioration of high-temperature storage performance.

[0024] Specifically, vinylene carbonate (VC) as a negative electrode film-forming additive will undergo a polymerization reaction on the negative electrode surface of lithium-ion batteries to form a dense SEI film, which prevents the electrolyte from further reducing and decomposing on the negative electrode surface, alleviates the gas production of the battery; at the same time, it can improve the low-temperature performance of the electrolyte, increase the capacity and cycle life of the battery. However, VC will have a negative impact on the thermal performance and safety characteristics of the positive electrode of lithium-ion batteries, that is, the electrochemical performance is poor under high temperature conditions, so it needs to be used together with other functional additives.

[0025] Specifically, 1,3-propane sultone (PS) as a negative electrode film-forming additive has good film-forming properties and can form a SEI film containing sulfonic acid groups on the negative electrode surface, improving the first efficiency and the first charge and discharge capacity, and further improving the high temperature performance and cycle performance of the battery. At the same time, PS has certain advantages in high temperature storage, and can inhibit the occurrence of electrolyte gas production side reactions. PS participates in the formation of the negative electrode interface SEI film, protecting the electrolyte from direct contact with the negative electrode active material.

[0026] However, 1,3-propane sultone (PS) has an adverse effect on long-cycle performance, especially in the late stage of high-temperature cycling, where the capacity decay accelerates. This may be because the SEI formed with the participation of 1,3-propane sultone (PS) has high density but poor stability. Therefore, VC is usually used in combination with PS, where the vinyl and sulfone groups interact to form a passivation film with a cross-linked protection network, extending the cycle life of the battery and inhibiting its expansion behavior at high temperatures.

[0027] Specifically, adiponitrile (ADN) is a bifunctional additive. ADN has a CN functional group and can react with water and acid in the electrolyte, thereby reducing the content of free acid and water in the electrolyte and improving the stability of the electrolyte. At the same time, adiponitrile can form a strong bond and conductive electrolyte interface on the surface of lithium metal, and can also react with Ni 4+ The formation of strong coordination reduces the side reactions on the positive electrode surface and improves the positive electrode interface stability.

[0028] Specifically, dithiothreitol (DTD) is a low-impedance additive, which is a low-impedance SEI film-forming additive. It will form oligomers containing sulfate groups, modify the SEI film components on the surface of the negative electrode, and increase the relative content of sulfur atoms and oxygen atoms. Because both contain lone pairs of electrons, they can attract lithium ions and thus speed up the shuttle speed of lithium ions in the SEI film, thereby reducing the impedance of the battery interface and effectively improving the battery charging and discharging performance at low temperatures; improving the battery's high-temperature cycling and storage performance.

[0029] The present application improves battery performance by adding negative electrode film-forming additives, bifunctional additives and low-impedance additives to the electrolyte, utilizing the advantages of various additives and their interactions, so that the final electrolyte can effectively inhibit the high-temperature gas production of the battery, while having a positive impact on the battery's cycle performance and capacity.

[0030] The present invention forms an excellent SEI film on the surface of the negative electrode plate by combining the negative electrode film-forming additive, the bifunctional additive and the low-impedance additive, thereby preventing the electrolyte from continuing to oxidize and decompose on the surface of the negative electrode plate, reducing electrolyte loss and the occurrence of side reactions, improving the cycle performance, and effectively reducing the gas production of the lithium ion battery during the charging and discharging process, thereby improving the safety of the lithium ion battery production process and improving the cycle performance of the lithium ion battery; in addition, the sulfonic acid group and the fluorine-containing group contained in the electrolyte structure can form a low-impedance SEI film on the surface of the negative electrode, inhibit high-temperature gas production, and improve the interface stability; furthermore, the carbon-nitrogen triple bond in the cyanide group has a high bond energy and is not easily oxidized, and has good stability and strong oxidation resistance on the positive electrode, and can also reduce the decomposition effect of the electrode on the electrolyte, while preventing the corrosion of hydrofluoric acid to the positive electrode material and the dissolution of metal ions in the positive electrode material, thereby improving the electrochemical performance of the positive electrode material of the lithium ion battery under high voltage.

[0031] In a preferred embodiment, taking the total mass of the electrolyte as 100%, the mass of the additive accounts for 2% to 5% of the total mass of the electrolyte.

[0032] Specifically, the mass of the additive accounts for a percentage of the total mass of the electrolyte of 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9% or 5.0%, any one of the values ​​or a range consisting of any two of the values.

[0033] When the added mass accounts for 2% to 5% of the total mass of the electrolyte, it can not only extend the cycle life of the battery and inhibit its expansion behavior at high temperatures, but also effectively inhibit the high-temperature gas production of the battery, while improving the battery's room temperature cycle performance and high-temperature cycle performance.

[0034] In a preferred embodiment, based on the total mass of the organic solvent being 100%, the content of the fluoroethylene carbonate is 15% to 25% of the total mass of the organic solvent.

[0035] Specifically, the percentage of the fluoroethylene carbonate in the total mass of the organic solvent is any point value among 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%, or a range value consisting of any two point values.

[0036] Specifically, when the percentage of fluoroethylene carbonate in the total mass of the organic solvent is 15% to 25%, the LUMO energy of FEC is much lower than that of EC (ethylene carbonate) due to the addition of F element, so FEC decomposes earlier in the electrolyte than the main solvents EC, DMC (dimethyl carbonate), EMC (ethyl methyl carbonate), etc., and the generated interface film contains more LiF components, with high mechanical strength, which can significantly improve the cycle stability of lithium-ion batteries, especially Si-containing lithium-ion batteries; at the same time, it will also form a protective film on the surface of the anode, which can inhibit the reaction of the anode with fluoride ions in the electrolyte; at low temperatures, FEC can reduce the interface impedance and improve the low-temperature performance of the battery; in addition, the SEI film with a high LiF content has a higher surface energy on the surface of metallic lithium, which can promote the uniform deposition of Li and inhibit the growth of dendrites. When the percentage of fluoroethylene carbonate in the total mass of the organic solvent is less than 10%, the cycle stability and low-temperature performance of the battery cannot be effectively improved. When the percentage of fluoroethylene carbonate in the total mass of the organic solvent is greater than 30%, because it will also undergo oxidative polymerization reaction at the positive electrode, when the content is high, it will increase the impedance of the electrolyte and the irreversibility of the positive electrode; and at high temperatures, it will react with LiPF6 and EC (ethylene carbonate), etc., resulting in increased acidity of the electrolyte, high gas production, and deterioration of high-temperature storage performance.

[0037] In one embodiment, the feed mass ratio of the negative electrode film-forming additive, the bifunctional additive and the low-impedance additive is 1~4:0.5~2:0.5~2.

[0038] Specifically, the feeding mass ratio of the negative electrode film-forming additive, the bifunctional additive and the low-impedance additive is any ratio of 2:1:1 or 2:1.5:1 or 3:0.5:1 or 3.5:0.5:1 or 1:2:1 or 1:2:2 or 4:0.5:0.5 or 1:1:1 or 1.5:1:1 or 2:1.5:1.5 or any two ratios. In a preferred embodiment, the feeding mass ratio of the negative electrode film-forming additive, the bifunctional additive and the low-impedance additive is 2-3:1-1.5:1-1.5; In one embodiment, the organic solvent further includes one or more substances selected from the group consisting of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propyl propionate, ethyl propionate, methylpropyl propionate, ethyl acetate, propyl acetate, methyl acetate, methyl butyrate, ethyl butyrate, and propyl butyrate.

[0039] In a preferred embodiment, the organic solvent further comprises propylene carbonate and diethyl carbonate.

[0040] In one embodiment, the percentage of propylene carbonate (PC) in the total mass of the organic solvent is 10-30%. In a preferred embodiment, the percentage of propylene carbonate in the total mass of the organic solvent is 20-30%. Specifically, the percentage of propylene carbonate in the total mass of the organic solvent is 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29% or 30%, any one of the values ​​or a range consisting of any two values.

[0041] In one embodiment, the percentage of diethyl carbonate (DEC) in the total mass of the organic solvent is 20-40%. In a preferred embodiment, the percentage of diethyl carbonate in the total mass of the organic solvent is 30-40%. Specifically, the percentage of diethyl carbonate in the total mass of the organic solvent is 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40%, any one of the values ​​or a range consisting of any two values.

[0042] Propylene carbonate is a cyclic organic ester and diethyl carbonate is a chain organic ester. The cyclic structure has a relatively ordered dipole array, while the chain structure is relatively open and flexible, causing the dipoles to cancel each other out. Therefore, cyclic organic esters generally have a wider liquid range, a higher dielectric constant, and a higher viscosity; while chain solvents are the opposite, and as a single solvent they will reduce the conductivity of the electrolyte. Therefore, cyclic and chain solvents are generally mixed in the electrolyte, that is, PC and DEC form a co-solvent system. If the PC content exceeds 30%, it will destroy the structure of graphite, causing the electrode to peel off, affecting the performance of the battery.

[0043] In one embodiment, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate and lithium bis(trifluoromethanesulfonyl)imide.

[0044] In one embodiment, taking the total mass of the electrolyte as 100%, the organic solvent accounts for 60% to 80% of the total mass of the electrolyte, and the lithium salt accounts for 10% to 40% of the total mass of the electrolyte.

[0045] In a preferred embodiment, the organic solvent accounts for 65-75% of the total mass of the electrolyte. Specifically, the organic solvent accounts for any point value or a range of any two point values ​​among 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79% or 80% of the total mass of the electrolyte.

[0046] In a preferred embodiment, the percentage of the lithium salt in the total mass of the electrolyte is 15-25%. Specifically, the percentage of the lithium salt in the total mass of the electrolyte is 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40%, or a range of any two values.

[0047] A second aspect of the present invention provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte as described above.

[0048] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode material layer coated on one side or both sides of the positive electrode current collector, and the positive electrode material layer includes a positive electrode active material, a conductive agent, and a binder.

[0049] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode material layer coated on one side or both sides of the negative electrode current collector, and the negative electrode material layer includes a negative electrode active material, a conductive agent, a binder, and a thickener.

[0050] Specifically, it also includes a diaphragm, which can be various diaphragm materials suitable for lithium-ion batteries or sodium-ion batteries in the art, for example, it can be a combination of one or more including but not limited to single-layer PP (polypropylene), single-layer PE (polyethylene), double-layer PP / PE, double-layer PP / PP, three-layer PP / PE / PP, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fiber.

[0051] In one embodiment, the positive electrode sheet includes a positive electrode active material, and the positive electrode active material is selected from one or more substances of lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate and lithium iron manganese phosphate.

[0052] In some embodiments, the positive electrode conductive agent includes one or more of graphite, superconducting carbon, acetylene black, carbon black, carbon nanotubes, graphene, carbon nanofibers, metal powder, metal fibers, and polyphenylene derivatives.

[0053] In some embodiments, the positive electrode binder includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.

[0054] In some embodiments, the mass percentage of each component in the positive electrode material layer is: 96-98wt% of positive electrode active material, 0.5-2wt% of conductive agent, and 1.0-2.0wt% of binder.

[0055] When the mass proportion of the positive electrode active material in the positive electrode material layer is within the above range, the positive electrode plate can have a higher lithium removal and lithium insertion capacity, and the lithium-ion battery can have a higher capacity.

[0056] The positive electrode current collector is selected from metal materials that can conduct electrons. Preferably, the positive electrode current collector includes one or more materials of copper, nickel, tin, copper, and stainless steel. In a more preferred embodiment, the positive electrode current collector is selected from aluminum foil.

[0057] The positive electrode sheet can be prepared according to conventional methods in the art. For example, the positive electrode material layer is usually prepared by coating a positive electrode slurry made of a positive electrode active material, a positive electrode conductive agent, a positive electrode binder and any other components on a positive electrode current collector, followed by drying and cold pressing. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto.

[0058] In one embodiment, the negative electrode sheet includes a negative electrode active material, and the negative electrode active material is selected from Si, Li-Si, SiO x (mit 0≤x≤2), one or more substances selected from SiC, Si-Sn, SiSnFe, SiSnAl, SiFeCo, SnO2.

[0059] In some embodiments, the negative electrode conductive agent includes one or more of graphite, superconducting carbon, acetylene black, carbon black, carbon nanotubes, graphene, carbon nanofibers, metal powder, metal fibers, and polyphenylene derivatives.

[0060] In some embodiments, the negative electrode binder includes one or more of styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, and polymethacrylic acid.

[0061] In some embodiments, the thickener includes one or more of sodium alginate, sodium carboxymethyl cellulose and carboxymethyl chitosan.

[0062] In some embodiments, the mass percentage of each component in the negative electrode material layer is: 96%-97% of negative electrode active material, 0.5%-1.5% of conductive agent, 1%-2% of binder and 0.5%-1.5% of thickener.

[0063] When the mass proportion of each component in the negative electrode material layer is within the above range, the processing performance and yield of the electrode sheet can be improved; and the stability and cycle performance of the battery can be further improved.

[0064] The negative electrode current collector is selected from metal materials that can conduct electrons. Preferably, the negative electrode current collector includes one or more substances of Al, Ni, tin, copper, and stainless steel. In a more preferred embodiment, the negative electrode current collector is selected from copper foil.

[0065] The negative electrode sheet can be prepared according to conventional methods in the art. For example, the negative electrode material layer is usually prepared by coating a negative electrode slurry made of a negative electrode active material, a negative electrode conductive agent, a negative electrode binder and any other components on a negative electrode current collector, followed by drying and cold pressing. The solvent can be an aqueous solvent, but is not limited thereto.

[0066] Lithium-ion battery production: The positive electrode sheet, the separator and the negative electrode sheet are stacked in order, so that the separator is located between the positive and negative electrodes to play an isolating role, and a bare cell is obtained. The bare cell is placed in the aluminum-plastic film formed by punching and shelling, and the non-aqueous electrolyte prepared above is injected into the baked and dried cell, and a lithium-ion battery is obtained after vacuum packaging, standing, and formation processes.

[0067] A third aspect of the present invention provides an electrical device comprising the lithium-ion battery described above.

[0068] The third aspect of the present invention provides an electric device, which includes the lithium ion battery described in the second aspect of the present invention. The lithium ion battery is used as a power source for the electric device. The number of lithium ion batteries in the electric device can be adjusted according to the application and capacity of the electric device.

[0069] Preferably, the electrical device may be, but is not limited to, an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0070] The beneficial effects of the present invention are further illustrated below in conjunction with embodiments.

[0071] In order to make the invention purpose, technical scheme and beneficial technical effect of the present invention clearer, the present invention is further described in detail below in conjunction with examples. However, it should be understood that the examples of the present invention are only for explaining the present invention, not for limiting the present invention, and the examples of the present invention are not limited to the examples given in the specification. The specific experimental conditions or operating conditions not specified in the examples are made under conventional conditions, or are made under the conditions recommended by the material supplier.

[0072] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0073] In the following examples, the reagents, materials and instruments used, unless otherwise specified, can be purchased commercially or obtained by synthetic methods known in the art.

[0074] Table 1 Design of electrolytes for Examples 1-6 and Comparative Examples 1-9

[0075] Example 1 This embodiment is used to illustrate the electrolyte and battery disclosed in the present invention; it includes the following operating steps: Preparation of electrolyte: In a glove box filled with argon (O2 <1ppm, H2O <1ppm), fluoroethylene carbonate (FEC), PC (propylene carbonate), and diethyl carbonate (DEC) are mixed in a mass ratio of 3:3:4 to obtain a mixed solvent; LiPF6 is slowly added to the mixed solvent to obtain a mixed solution with a LiPF6 concentration of 1.1 mol / L; finally, 4% of an additive is added to the mixed solution to obtain the electrolyte.

[0076] Vinylene carbonate (VC), 1,3-propane sultone (PS), adiponitrile (ADN), and diethylene sulfate (DTD) were mixed in a mass ratio of 1:1:1:1 to obtain an additive.

[0077] Preparation of positive electrode sheet: Mix the positive electrode active material lithium cobalt oxide (NCM), the conductive agent CNT, and the adhesive PVDF in a mass ratio of 97:1.5:1.5. Stir and mix thoroughly in NMP solvent to form a uniform positive electrode slurry. Apply this slurry on at least one side of the positive electrode current collector aluminum foil, and obtain a positive electrode sheet that meets the requirements after drying, rolling, die-cutting and other processes.

[0078] Preparation of negative electrode sheet: The negative electrode active material micron silicon, conductive agent SP, thickener CMC, and binder SBR are fully stirred and mixed in a deionized water solvent at a mass ratio of 96.3:1:1.2:1.5 to form a uniform negative electrode slurry. The slurry is coated on at least one side of the negative electrode current collector copper foil, and after drying, rolling, die cutting and other processes, a usable negative electrode sheet is obtained.

[0079] Production of diaphragm: PE porous polymer film is used as diaphragm.

[0080] Lithium-ion battery production: Stack the positive electrode sheet, separator and negative electrode sheet in order, so that the separator is in the middle of the positive and negative electrodes to play an isolating role, and then obtain the bare battery cell.

[0081] The bare battery cells are placed in aluminum-plastic film bags that have been punched and formed, and the non-aqueous electrolyte prepared above is injected into the baked and dried battery cells. After vacuum packaging, standing, forming and other processes, lithium-ion batteries are obtained.

[0082] Embodiment 2-6 Examples 2-6 are used to illustrate the battery cell assembly and secondary battery disclosed in the present invention, and include most of the operation steps in Example 1, except that: The components and contents of the electrolyte additives and the components and contents of the adhesives shown in Table 1 were used.

[0083] Comparative Examples 1-9 Comparative Examples 1-9 are used to illustrate the battery cell assembly and secondary battery disclosed in the present invention, and include most of the operating steps in Example 1, except that: The components and contents of the electrolyte solvent and the components and contents of the additives shown in Table 1 were used.

[0084] Performance Testing The lithium ion batteries prepared in Examples 1-6 and Comparative Examples 1-9 were subjected to the following performance tests: Normal temperature cycle test The test method is: at 25℃, the battery is left to stand for 6 hours, charged to 4.4V at 1C constant current and constant voltage, the cut-off current is 0.05C, left to stand for 10 minutes, and then discharged to 3V at 1C constant current, and the charge and discharge cycle is performed in this way. Record the first cycle discharge capacity C1 and the first cycle charge capacity C2. Then the first efficiency = C2 / C1*100%; capacity retention rate = discharge capacity of the specified number of cycles / C1*100%; cycle life = the number of cycles when the battery capacity retention rate reaches 80%.

[0085] High temperature cycle test The test method is: charge to 4.4V at 1C constant current and constant voltage at 45℃, with a cut-off current of 0.05C, stand for 5 minutes, then discharge to 3V at 1C, and cycle for 500 cycles. Record the first cycle discharge capacity C3 and the first cycle charge capacity C4, then the first efficiency = C4 / C3*100%; capacity retention rate = discharge capacity of the specified number of cycles / C3*100%; cycle life = the number of cycles when the battery capacity retention rate reaches 80%.

[0086] High temperature storage test The test method is: at room temperature (25°C), charge and discharge once at 0.2C and record the battery discharge capacity C3, then charge to 4.4V at 0.2C constant current and constant voltage, store the battery in a 45°C constant temperature test box for 28 days and then take it out. After the battery returns to normal temperature, use the drainage method to test the battery gas production.

[0087] The test results are shown in Table 2 Table 2 Test results of Examples 1-6 and Comparative Examples 1-9

[0088] From Example 1, it can be seen that when the four additives are in an appropriate ratio, the battery performance can be optimized, and the battery gas production, as well as the cycle and storage performance at high temperature can be improved to the greatest extent. However, when the content of a certain additive is too high or too low, it will have an adverse effect on the battery performance.

[0089] VC and PS are film-forming additives, such as in Examples 3 and 4: when the addition amount is greater than 1%, the PS film-forming impedance is large, which will cause the cycle performance at room temperature to deteriorate, and the first efficiency and cycle performance of the battery will decrease; such as in Comparative Examples 2 and 3: when one film-forming additive is reduced, VC has less effect on the room temperature and high temperature cycles of the battery as a whole, while PS can improve the high temperature cycle performance of the battery. Therefore, VC and PS are usually used in combination, where the vinyl and sulfone groups interact to form a passivation film with a cross-linked protection network, prolonging the cycle life of the battery and inhibiting its expansion behavior at high temperatures.

[0090] For example, in Comparative Example 1 and Example 6, when no additives are added or the content is reduced, the overall performance of the battery becomes worse, especially when there are no additives, the impact on the gas production of the battery is relatively large.

[0091] DTD is a sulfur-based additive that is beneficial for improving high-temperature cycle performance. Therefore, when its content is low or not added, such as in Example 5 and Comparative Example 5, the high-temperature cycle performance of the battery will be affected; when the amount of DTD added is too high, such as in Comparative Example 9, it is easy to undergo an ester exchange reaction with carbonate to generate hydrogen sulfate ester. During the reaction, the carbon chain of the carbonate will be broken to generate olefin compounds, resulting in an increase in the gas production of the battery.

[0092] ADN can inhibit the side reaction between the electrolyte and the high-nickel positive electrode surface, forming a conductive and strong interface on the positive electrode surface; the strong coordination between the nitrile group and Ni4+ can effectively reduce the formation of electrochemically inert NiO-type rock salt structure, reduce the side reaction of the electrolyte on the positive electrode surface, and improve the cycle performance of the battery. Therefore, from Examples 2, 3 and Comparative Example 4, we can intuitively see the effect of the amount of ADN added on the battery cycle performance.

[0093] When the amount of FEC added increases, the HF content will increase, which will corrode the SEI film and increase the acidity of the electrolyte, and the gas production will also increase, as shown in Comparative Example 6.

[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An electrolyte, Features: The invention comprises an organic solvent, a lithium salt and an additive, wherein the additive comprises a negative electrode film-forming additive, a bifunctional additive and a low-impedance additive, wherein the negative electrode film-forming additive comprises vinylene carbonate and 1,3-propane sultone; the bifunctional additive is adiponitrile; and the low-impedance additive is vinyl sulfate; The feeding mass ratio of the negative electrode film-forming additive, the bifunctional additive and the low-impedance additive is 1-4:0.5-2:0.5-2; Taking the total mass of the electrolyte as 100%, the mass of the additive accounts for 1% to 10% of the total mass of the electrolyte; The organic solvent includes fluoroethylene carbonate; taking the total mass of the organic solvent as 100%, the percentage of the fluoroethylene carbonate in the total mass of the organic solvent is 10% to 30%.

2. The electrolyte according to claim 1, Features: Taking the total mass of the electrolyte as 100%, the mass of the additive accounts for 2% to 5% of the total mass of the electrolyte.

3. The electrolyte according to claim 1, Features: Taking the total mass of the organic solvent as 100%, the percentage of the fluoroethylene carbonate in the total mass of the organic solvent is 15% to 25%.

4. The electrolyte according to claim 1, Features: The feed mass ratio of the negative electrode film-forming additive, the bifunctional additive and the low-impedance additive is 2~3:1~1.5:1~1.

5.

5. The electrolyte according to claim 1, Features: The organic solvent also includes one or more substances selected from ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propyl propionate, ethyl propionate, methylpropyl propionate, ethyl acetate, propyl acetate, methyl acetate, methyl butyrate, ethyl butyrate, and propyl butyrate; the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, and lithium bis(trifluoromethanesulfonyl)imide.

6. The electrolyte according to claim 1, Features: Taking the total mass of the electrolyte as 100%, the organic solvent accounts for 60% to 80% of the total mass of the electrolyte, and the lithium salt accounts for 10% to 40% of the total mass of the electrolyte.

7. A lithium ion battery, Features: The invention comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte as claimed in any one of claims 1 to 6.

8. The lithium ion battery according to claim 7, Features: The positive electrode sheet includes a positive electrode active material, which is selected from one or more substances of lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate and lithium iron manganese phosphate; the negative electrode sheet includes a negative electrode active material, which is selected from Si, Li-Si, SiO x (mit 0≤x≤2), SiC, Si-Sn, SiSnFe, SiSnAl, SiFeCo, SnO 2 One or more substances in a 9. An electronic device, Features: Comprising a lithium ion battery according to any one of claims 7-8.

Citation Information

Patent Citations

  • Electrolyte and lithium ion battery adopting same

    CN104269576A

  • Electrolyte and lithium ion battery comprising same

    CN105098244A

  • Lithium ion battery electrolyte and lithium ion battery

    CN107508000A

  • Polymer lithium ion battery with high energy density and fast charge and preparation method thereof

    CN112993379A

  • Non-aqueous electrolyte and lithium ion battery

    CN117766856A

Cited By

  • Electrolyte and battery

    CN119170874A