Ionic liquid-based ether-based electrolyte suitable for high-voltage lithium metal battery greater than 4V as well as preparation method and application of ionic liquid-based ether-based electrolyte

By using a combination of lithium salts and additives in lithium batteries, a stable solid electrolyte interphase is formed, which broadens the electrochemical window, solves the problem of the narrow electrochemical window of lithium battery electrolyte under high voltage conditions, and achieves high energy density. and long-life battery performance.

CN118738564AInactive Publication Date: 2024-10-01KUNMING UNIV OF SCI & TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411099078.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium battery electrolytes have a narrow electrochemical window under high voltage conditions and are difficult to match high-voltage cathode materials, resulting in limited energy density, poor cycle stability, and potential safety hazards.

Method used

An ether-based electrolyte based on ionic liquids is used, including lithium salts, additives and solvents. By drying and activating molecular sieves, a stable solid electrolyte interphase is formed, which broadens the electrochemical window and improves cycle performance and safety performance.

Benefits of technology

Under high voltage conditions greater than 4V, the electrolyte shows good cycle performance and service life, avoiding the risk of battery explosion and improving the energy density and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738564A_ABST
    Figure CN118738564A_ABST
Patent Text Reader

Abstract

The invention relates to an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V as well as a preparation method and application of the ether-based electrolyte, and belongs to the technical field of lithium battery materials. The ether-based electrolyte comprises a lithium salt, an additive and a solvent, the lithium salt is lithium bis (fluorosulfonyl) imide or lithium bis (trifluoromethanesulfonyl) imide, and the final concentration of the lithium salt is 1-1.5 mol / L; the additive is at least one of lithium nitrate, lithium difluorophosphate and lithium difluoro (oxalato) borate, and the final concentration of the additive is 0.02-0.5 mol / L; the solvent is a mixed solvent of ionic liquid and an ether solvent in a volume ratio of 1: (1-10). The electrochemical window of the electrolyte is greater than 4.5 V, the cycle stability of the battery under the condition of high voltage greater than 4V is effectively improved, the safety performance is good, the service life of the battery is long, and the electrolyte is easy to popularize and apply.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium battery materials, and specifically relates to an ether-based electrolyte based on ionic liquid suitable for high-voltage lithium metal batteries greater than 4V, and a preparation method and application thereof. Background Art

[0002] Due to the good electrochemical properties of lithium-ion batteries, they are widely used in portable electronic products, electric vehicles, smart grids and military fields. However, lithium-ion batteries have almost reached the theoretical upper limit of their embedded chemical energy density and can no longer meet people's demand for high-energy-density energy storage devices. Therefore, high-voltage lithium metal batteries with high energy density have come into people's view. In this case, high-voltage lithium metal batteries have put forward higher requirements for electrolytes. High operating voltage is one of the effective ways to improve the energy density of lithium batteries, as shown in formula (1):

[0003]

[0004] Where: E is energy density; Q is specific capacity; V is operating voltage; V up and V low Low refers to the cut-off voltage during charging and discharging. Under high working voltage, the electrolyte needs to have good oxidation resistance and a stable electrochemical window so that the lithium-ion battery can maintain stable cycling under high voltage. In this case, high-voltage lithium metal batteries have higher requirements for electrolytes.

[0005] Lithium battery electrolytes are usually divided into two categories: ether electrolytes and ester electrolytes. Ester electrolytes usually have an electrochemical window greater than 4V, but in lithium metal batteries, the coulombic efficiency is low and the battery cycle stability is poor. "Col ossal granular lithium deposits enabled by the grain-coarsening effect for high-efficiency lithium metal full batteries" and "A sustainable solid electrolyte interphase for high-energy-density lithium metal batteries under practical conditions" reported that the lithium deposition coulombic efficiency was less than 80% using 1M LiPF6 EC / DEC ester electrolyte. Ether electrolytes have good compatibility with metallic lithium and have attracted widespread attention from researchers. For example: Chinese invention patent 202311323256.1 prepares an ether electrolyte by adding a co-solvent, forms a stable SEI film through the synergistic effect of lithium salt and co-solvent, and the assembled Li||Gr battery cycle performance shows good cycle stability. Chinese invention patent 202310658402.X forms a composite ether solvent by adding aromatic hydrocarbon ether compounds to ethylene glycol dimethyl ether, and forms an ether electrolyte after adding lithium salt. The assembled Li||LiFeP O4 battery is cycled in the 2.8-3.7V voltage range. The battery exhibits good rate performance and cycle performance. However, the narrow electrochemical window inherent in ether electrolytes limits its application in high-voltage lithium metal batteries. As shown in Table 1, when assembling a full battery with a narrow electrochemical window electrolyte, the positive electrode can often only choose a positive electrode with a voltage lower than 4V such as lithium titanate or lithium iron phosphate, and the energy density of such a full battery is very limited.

[0006] Table 1

[0007]

[0008] Therefore, there is an urgent need to develop a high-voltage electrolyte that is highly compatible with lithium metal for high-voltage lithium batteries greater than 4V. Summary of the invention

[0009] The purpose of the present invention is to solve the shortcomings of the prior art and provide an ether-based electrolyte based on ionic liquid suitable for high-voltage lithium metal batteries greater than 4V, and a preparation method and application thereof. The ether-based electrolyte has stable cycle performance under high voltage conditions greater than 4V, good safety performance in use, and long service life, solving the problem that ether electrolytes have a narrow electrochemical window and decompose under high voltage conditions.

[0010] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0011] Ionic liquid-based ether electrolytes for high-voltage lithium metal batteries greater than 4 V, including lithium salts, additives and solvents;

[0012] The lithium salt is lithium bis(fluorosulfonyl)imide or lithium bis(trifluoromethanesulfonyl)imide, with a final concentration of 1-1.5 mol / L;

[0013] The additive is at least one of lithium nitrate, lithium difluorophosphate and lithium difluorooxalate borate, and the total final concentration of the additive is 0.02-0.5 mol / L;

[0014] The solvent is a mixed solvent of an ionic liquid and an ether solvent, with a volume ratio of 1:1-10.

[0015] Further, preferably, the ionic liquid is 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt or 1-ethyl-3-methylimidazolium tetrafluoroborate.

[0016] Furthermore, preferably, the ether solvent is ethylene glycol dimethyl ether.

[0017] The present invention also provides a method for preparing the above-mentioned ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V, comprising the following steps:

[0018] Step (1), drying the lithium salt, ionic liquid and additive separately at 70-100° C. for at least 10 hours;

[0019] Step (2), The molecular sieve is placed in a muffle furnace and activated at 350-500℃ for at least 10h; Add molecular sieves to ether solvent and let stand for 3-7 days;

[0020] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0021] Furthermore, preferably, in step (1), the drying time is 10 h to 24 h.

[0022] The present invention also provides the use of the above-mentioned ether-based electrolyte based on ionic liquid suitable for high-voltage lithium metal batteries with a voltage greater than 4V in the preparation of high-voltage lithium metal batteries.

[0023] When multiple additives are used in the present invention, there is no ratio limit between the additives, and they can be adjusted according to the required electrolyte properties. The total final concentration of the additives can be 0.02-0.5 mol / L.

[0024] The present invention uses lithium bis(fluorosulfonyl)imide or lithium bis(trifluoromethanesulfonyl)imide, which has a high ionic conductivity in a dilute electrolyte (concentration <3M), can effectively improve the mobility of lithium ions during charging and discharging, and accelerate the battery reaction kinetics.

[0025] The present invention uses lithium nitrate to effectively form a solid electrolyte interphase containing nitrogen-containing inorganic components, alleviating the occurrence of a series of side reactions during the battery cycle. The use of lithium difluorophosphate can improve the conductivity of the electrolyte solution, inhibit the decomposition of the positive electrode surface that may occur during high-temperature cycles, and prevent the oxidation reaction of the electrolyte solution, thereby improving the output characteristics and swelling characteristics after high-temperature storage. The use of lithium difluorooxalatoborate can not only provide lithium ions, but also its good film-forming properties can play a synergistic role with lithium nitrate, forming a highly stable solid electrolyte interphase at the positive electrode, inhibiting the decomposition of the electrolyte, thereby extending the service life of the battery.

[0026] The present invention adopts 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt or 1-ethyl-3-methylimidazolium tetrafluoroborate, and introduces TFSI- or BF4 by adding ionic liquid. - Anionic groups construct anion-rich weakly solvated coordination sheaths, which reduce the desolvation energy barrier while promoting the formation of an inorganic-rich solid electrolyte interphase protective layer, further stabilizing the solid electrolyte interphase and widening the electrochemical window of the electrolyte.

[0027] The present invention adopts chain organic ether to promote the dissolution of lithium salt, reduce the viscosity of the electrolyte and improve the wettability of the electrolyte.

[0028] Appendix: The specific meanings of English abbreviations or codes with special meanings and the commonly used Chinese names in the industry

[0029] LiFSI: lithium bis(trifluoromethanesulfonyl)imide; LiTFSI: lithium bis(trifluoromethanesulfonyl)imide; LiNO3: lithium nitrate; LiPO2F2: lithium difluorophosphate; LiDFOB: lithium difluorooxalatoborate; PP14TFSI: 1-methyl-1-propylpiperidinium bis(trifluoromethanesulfonyl)imide; EMIMBF4: 1-ethyl-3-methylimidazolium tetrafluoroborate; DME: ethylene glycol dimethyl ether.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) Ether electrolytes have good compatibility with lithium metal and are widely used in lithium metal batteries. However, their narrow electrochemical window is usually only used to match positive electrode materials such as lithium titanate (LTO) or lithium iron phosphate (LFP). The energy density of such lithium metal full batteries may not even be as good as that of commercial lithium-ion batteries. Therefore, it is particularly important to broaden the electrochemical window of ether electrolytes to match high-voltage positive electrode materials and improve battery energy density. The present invention provides a high-voltage ether electrolyte for lithium batteries, which solves the problem that ether electrolytes have a narrow electrochemical window and decompose under high voltage conditions greater than 4V. It has stable cycle performance under high voltage conditions, good safety performance in use, and a long service life.

[0032] The present invention adopts lithium salts and additives to add organic ether solvents, and at the same time mixes ionic liquids, so that the cycle performance and safety performance of the obtained electrolyte in a high voltage environment greater than 4V are improved, and the battery explosion caused by overcharging and other reasons is avoided; at the same time, the introduction of additives further enriches the types of anions in the electrolyte, increases the components of the anion-derived solid electrolyte interface during the cycle process, effectively stabilizes the electrode interface, reduces the side reactions of the solvent at the electrode interface, and improves the electrochemical window of the ether electrolyte. It avoids the electrolyte from continuously and directly contacting the positive or negative electrode of the battery, and improves the cycle performance and service life of the battery. As shown in Table 1, compared with most ether-based electrolyte studies, its electrochemical window is generally lower than 4V, which is difficult to match with high-voltage positive electrode materials. Figure 1 As shown, the electrochemical window of the ether-based electrolyte in Comparative Example 1 is less than 3.8V. In contrast, the ester-based electrolyte in Comparative Example 2 shows a good electrochemical window, but its compatibility with the electrode is poor, and serious side reactions during the cycle process are prone to produce a large number of side reaction products, resulting in battery volume expansion and serious dendrite growth, which greatly limits the application of the two electrolytes. The electrolyte of the present invention has a good electrochemical window and shows good compatibility with the electrode material. The lithium metal negative electrode shows a dense and smooth deposition morphology during the cycle, and the assembled Li||NCM811 battery shows good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 It is the linear voltammetric scanning diagram of the electrolyte of comparative example 1 and comparative example 2 of Example 7 of the present invention;

[0035] Figure 22 is a diagram of the coulombic efficiency of Li||Cu batteries assembled with the electrolytes of Example 7 of the present invention and Comparative Example 2;

[0036] Figure 3 The electrolytes of Example 7 and Comparative Example 2 deposited 1 mAh cm -2 Scanning electron microscope image of metallic lithium;

[0037] Figure 4 It is a graph of discharge specific capacity and coulombic efficiency of Li||NCM811 battery assembled with electrolyte of Example 7 of the present invention and Comparative Example 2. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with embodiments.

[0039] Those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in this field or the product specifications are used. If the materials or equipment used do not specify the manufacturer, they are all conventional products that can be purchased. In the examples of the present invention, if there are no special instructions, the concentrations are all final concentrations.

[0040] Example 1

[0041] Ionic liquid-based ether electrolytes for high-voltage lithium metal batteries greater than 4 V, including lithium salts, additives and solvents;

[0042] The lithium salt is lithium bis(fluorosulfonyl)imide, with a final concentration of 1.2 mol / L;

[0043] The additive is lithium nitrate, and the final concentration of the additive is 0.3 mol / L;

[0044] The solvent is a mixed solvent of an ionic liquid and an ether solvent, with a volume ratio of 1:5.

[0045] This embodiment is applicable to a method for preparing an ether-based electrolyte based on an ionic liquid for a high-voltage lithium metal battery greater than 4V, comprising the following steps:

[0046] Step (1), drying the lithium salt, ionic liquid and additive separately at 70° C. for 36 hours;

[0047] Step (2), The molecular sieve was placed in a muffle furnace and activated at 400°C for 15 h. The molecular sieves were added to the ether solvent and allowed to stand for 5 days;

[0048] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0049] Example 2

[0050] Ionic liquid-based ether electrolytes for high-voltage lithium metal batteries greater than 4 V, including lithium salts, additives and solvents;

[0051] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the final concentration is 1 mol / L;

[0052] The additive is lithium difluorophosphate, and the final concentration of the additive is 0.02 mol / L;

[0053] The solvent is a mixed solvent of an ionic liquid and an ether solvent, with a volume ratio of 1:1.

[0054] The ionic liquid is 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt.

[0055] The ether solvent is ethylene glycol dimethyl ether.

[0056] This embodiment is applicable to a method for preparing an ether-based electrolyte based on an ionic liquid for a high-voltage lithium metal battery greater than 4V, comprising the following steps:

[0057] Step (1), drying the lithium salt, ionic liquid and additive separately at 70° C. for 10 h;

[0058] Step (2), The molecular sieve was placed in a muffle furnace and activated at 350°C for 10 h. The molecular sieves were added to the ether solvent and allowed to stand for 3 days;

[0059] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0060] Example 3

[0061] Ionic liquid-based ether electrolytes for high-voltage lithium metal batteries greater than 4 V, including lithium salts, additives and solvents;

[0062] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, with a final concentration of 1.5 mol / L;

[0063] The additives are lithium nitrate and lithium difluorophosphate, and the final concentration of the additives is 0.5 mol / L (the final concentrations of lithium nitrate and lithium difluorophosphate are both 0.25 mol / L); the solvent is a mixed solvent of an ionic liquid and an ether solvent, with a volume ratio of 1:10.

[0064] The ionic liquid is 1-ethyl-3-methylimidazolium tetrafluoroborate.

[0065] The ether solvent is ethylene glycol dimethyl ether.

[0066] This embodiment is applicable to a method for preparing an ether-based electrolyte based on an ionic liquid for a high-voltage lithium metal battery greater than 4V, comprising the following steps:

[0067] Step (1), drying the lithium salt, ionic liquid and additive separately at 70° C. for 24 hours;

[0068] Step (2), The molecular sieve was placed in a muffle furnace and activated at 500°C for 24 hours. The molecular sieves were added to the ether solvent and allowed to stand for 7 days;

[0069] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0070] Example 4

[0071] Ionic liquid-based ether electrolytes for high-voltage lithium metal batteries greater than 4 V, including lithium salts, additives and solvents;

[0072] The lithium salt is lithium bis(fluorosulfonyl)imide, with a final concentration of 1.2 mol / L;

[0073] The additives are lithium nitrate, lithium difluorophosphate and lithium difluorooxalate borate, and the final concentration of the additives is 0.3 mol / L (the final concentrations of lithium nitrate, lithium difluorophosphate and lithium difluorooxalate borate are all 0.1 mol / L); the solvent is a mixed solvent of an ionic liquid and an ether solvent, with a volume ratio of 1:6.

[0074] The ionic liquid is 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt.

[0075] The ether solvent is ethylene glycol dimethyl ether.

[0076] This embodiment is applicable to a method for preparing an ether-based electrolyte based on an ionic liquid for a high-voltage lithium metal battery greater than 4V, comprising the following steps:

[0077] Step (1), drying the lithium salt, ionic liquid and additive separately at 70° C. for 24 hours;

[0078] Step (2), The molecular sieve was placed in a muffle furnace and activated at 450°C for 16 h. The molecular sieves were added to the ether solvent and allowed to stand for 5 days;

[0079] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0080] Example 5

[0081] An ether-based electrolyte based on an ionic liquid suitable for a high-voltage lithium metal battery greater than 4V, characterized in that it comprises a lithium salt, an additive and a solvent;

[0082] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the final concentration is 1 mol / L;

[0083] The additives are lithium nitrate (0.005 mol / L), lithium difluorophosphate (0.005 mol / L) and lithium difluorooxalate borate (0.01 mol / L), and the total final concentration of the additives is 0.02 mol / L;

[0084] The solvent is a mixed solvent of an ionic liquid and an ether solvent, with a volume ratio of 1:1.

[0085] The ionic liquid is 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt.

[0086] The ether solvent is ethylene glycol dimethyl ether.

[0087] This embodiment is applicable to a method for preparing an ether-based electrolyte based on an ionic liquid for a lithium metal battery with a high voltage greater than 4V, comprising the following steps:

[0088] Step (1), drying the lithium salt, ionic liquid and additive at 70° C. for 10 hours;

[0089] Step (2), The molecular sieve was placed in a muffle furnace and activated at 350°C for 24 hours. The molecular sieves were added to the ether solvent and allowed to stand for 3 days;

[0090] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0091] Example 6

[0092] An ether-based electrolyte based on an ionic liquid suitable for a high-voltage lithium metal battery greater than 4V, characterized in that it comprises a lithium salt, an additive and a solvent;

[0093] The lithium salt is lithium bis(fluorosulfonyl)imide, with a final concentration of 1.5 mol / L;

[0094] The additives are lithium nitrate (0.2 mol / L), lithium difluorophosphate (0.2 mol / L) and lithium difluorooxalate borate (0.2 mol / L), and the total final concentration of the additives is 0.5 mol / L;

[0095] The solvent is a mixed solvent of ionic liquid and ether solvent, with a volume ratio of 1:10.

[0096] The ionic liquid is 1-ethyl-3-methylimidazolium tetrafluoroborate.

[0097] The ether solvent is ethylene glycol dimethyl ether.

[0098] This embodiment is applicable to a method for preparing an ether-based electrolyte based on an ionic liquid for a lithium metal battery with a high voltage greater than 4V, comprising the following steps:

[0099] Step (1), drying the lithium salt, ionic liquid and additive at 100° C. for 24 hours;

[0100] Step (2), The molecular sieve was placed in a muffle furnace and activated at 500°C for 10 h. The molecular sieves were added to the ether solvent and allowed to stand for 7 days;

[0101] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0102] Example 7

[0103] An ether-based electrolyte based on ionic liquids suitable for high-voltage lithium metal batteries greater than 4V includes 1 mol / LLiFSI, 0.3 mol / L LiNO3, 0.05 mol / L LiDFOB, and the solvent is 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) and ethylene glycol dimethyl ether (DME); the volume ratio of 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) to ethylene glycol dimethyl ether (DME) is 1:1.

[0104] The method for preparing the ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V described in this embodiment comprises the following steps:

[0105] Step (1), drying the lithium salt, ionic liquid and additive separately at 70° C. for 10 hours;

[0106] Step (2), The molecular sieve was placed in a muffle furnace and activated at 350°C for 10 h. The molecular sieves were added to the ether solvent and allowed to stand for 3 days;

[0107] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0108] Example 8

[0109] An ether-based electrolyte based on ionic liquids suitable for high-voltage lithium metal batteries greater than 4V includes 1mol / LLiFSI, 0.3mol / L LiNO3, 0.1mol / L LiDFOB, and the solvent is 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) and ethylene glycol dimethyl ether (DME); the volume ratio of 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) to ethylene glycol dimethyl ether (DME) is 1:1.

[0110] The method for preparing the ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V described in this embodiment comprises the following steps:

[0111] Step (1), drying the lithium salt, ionic liquid and additive separately at 100° C. for 15 hours;

[0112] Step (2), The molecular sieve was placed in a muffle furnace and activated at 500°C for 24 hours. The molecular sieves were added to the ether solvent and allowed to stand for 7 days;

[0113] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0114] Example 9

[0115] An ether-based electrolyte based on ionic liquids suitable for high-voltage lithium metal batteries greater than 4V includes 1 mol / LLiFSI, 0.3 mol / L LiNO3, 0.05 mol / L LiDFOB, and the solvent is 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) and ethylene glycol dimethyl ether (DME); the volume ratio of 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) to ethylene glycol dimethyl ether (DME) is 1:5.

[0116] The method for preparing the ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V described in this embodiment comprises the following steps:

[0117] Step (1), drying the lithium salt, ionic liquid and additive separately at 80° C. for 20 hours;

[0118] Step (2), The molecular sieve was placed in a muffle furnace and activated at 400°C for 16 h. The molecular sieves were added to the ether solvent and allowed to stand for 5 days;

[0119] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0120] Example 10

[0121] An ether-based electrolyte based on ionic liquid suitable for high-voltage lithium metal batteries greater than 4V, including 1 mol / LLiFSI, 0.3 mol / L LiNO3, 0.05 mol / L LiPO2F2, and the solvent is 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt (PP14TFSI) and ethylene glycol dimethyl ether (DME); the volume ratio of 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt (PP14TFSI) to ethylene glycol dimethyl ether (DME) is 1:1.

[0122] The method for preparing the ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V described in this embodiment comprises the following steps:

[0123] Step (1), drying the lithium salt, ionic liquid and additive separately at 90° C. for 25 hours;

[0124] Step (2), The molecular sieve was placed in a muffle furnace and activated at 450°C for 18 h. The molecular sieves were added to the ether solvent and allowed to stand for 6 days;

[0125] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0126] Embodiment 11

[0127] An ether-based electrolyte based on ionic liquid suitable for high-voltage lithium metal batteries greater than 4V, including 1 mol / LLiFSI, 0.3 mol / L LiNO3, 0.1 mol / L LiPO2F2, and the solvent is 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt (PP14TFSI) and ethylene glycol dimethyl ether (DME); the volume ratio of 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt (PP14TFSI) to ethylene glycol dimethyl ether (DME) is 1:1.

[0128] The method for preparing the ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V described in this embodiment comprises the following steps:

[0129] Step (1), drying the lithium salt, ionic liquid and additive separately at 85° C. for 20 hours;

[0130] Step (2), The molecular sieve was placed in a muffle furnace and activated at 420°C for 30 h. The molecular sieves were added to the ether solvent and allowed to stand for 4 days;

[0131] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0132] Example 12

[0133] An ether-based electrolyte based on ionic liquid suitable for high-voltage lithium metal batteries greater than 4V, including 1 mol / LLiFSI, 0.3 mol / L LiNO3, 0.05 mol / L LiPO2F2, and the solvent is 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt (PP14TFSI) and ethylene glycol dimethyl ether (DME); the volume ratio of 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt (PP14TFSI) to ethylene glycol dimethyl ether (DME) is 1:5.

[0134] The method for preparing the ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V described in this embodiment comprises the following steps:

[0135] Step (1), drying the lithium salt, ionic liquid and additive separately at 75° C. for 12 h;

[0136] Step (2), The molecular sieve was placed in a muffle furnace and activated at 380°C for 36 hours. The molecular sieves were added to the ether solvent and allowed to stand for 5 days;

[0137] Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

[0138] Comparative Example 1

[0139] The ether-based electrolyte of this comparative example includes the following components: 1 mol / L LiFSI, and the solvent is ethylene glycol dimethyl ether (DME).

[0140] Preparation process: According to the above ratio, LiFSI and DME are mixed and stirred until all materials are completely dissolved.

[0141] Comparative Example 2

[0142] The ether-based electrolyte of this comparative example includes the following components: 1 mol / L LiFSI, and a solvent selected from ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.

[0143] Preparation process: According to the above ratio, LiFSI, EC, and DEC are mixed and stirred until all materials are completely dissolved.

[0144] Performance Test:

[0145] The electrolytes in Examples 7-12 and the electrolytes and batteries in Comparative Examples 1-2 were subjected to the following performance tests:

[0146] Performance Test 1: The electrolytes in Test Examples 7-12 and the electrolytes in Comparative Examples 1-2 were subjected to linear voltammetric scanning to test the electrochemical window of the samples. Figure 1 The linear voltammetric scan results of Example 7, Comparative Example 1 and Comparative Example 2 are shown. When the current density is 0.03 mA cm -2 Under the conditions, the electrochemical window results corresponding to each electrolyte are shown in Table 2 below.

[0147] Table 2

[0148] sample Electrochemical Window (V) Example 7 4.51 Example 8 4.62 Example 9 4.48 Example 10 4.41 Embodiment 11 4.47 Example 12 4.53 Comparative Example 1 3.69 Comparative Example 2 4.27

[0149] It can be seen from the above performance test 1 that in the electrolyte without adding ionic liquid, the electrochemical window of the ether-based electrolyte is less than 3.8V, and it is difficult to work under high voltage conditions higher than 4V. The electrochemical window of the electrolyte of the present invention is effectively widened and can be used with nickel-cobalt-manganese ternary positive electrode materials.

[0150] Performance Test 2: Li||Cu batteries were assembled with the electrolytes of the embodiment and the comparative example, that is, the positive electrode shell, the positive electrode (here the positive electrode is Cu foil), the separator and the electrolyte, the negative electrode (here the Li foil) and the negative electrode shell were sequentially stacked and assembled. The electrolyte of the embodiment showed good coulombic efficiency (CE), as shown in FIG. Figure 2 In addition, after 10 cycles of Li||Cu, the positive electrode was taken out for scanning electron microscopy characterization, as shown in Figure 3 As shown, the deposition morphology in the embodiment is dense and uniform, and there is no obvious dendrite formation. In contrast, the deposition morphology in the comparative example is loose and porous, and there is obvious dendrite formation, which indicates that the electrolyte has serious side reactions with the electrode material during the cycle, and the accumulation of a large number of side reaction products consumes active substances, causing the battery capacity to decay rapidly, and is accompanied by serious volume expansion and other problems, which poses a serious safety hazard.

[0151] Performance Test 3: Test the batteries in Examples 7-12 and the battery in Comparative Example 2 at 0.2C (1C = 180 mAhg -1 ) for one cycle, and then charge and discharge for 100 cycles at 3-4.3V with 1C current. Figure 4 As shown, the battery performance using the electrolyte in the embodiment shows good cycle stability, while the comparative example shows rapid capacity decay. The first discharge specific capacity of the battery and the capacity retention rate after 100 cycles of charge and discharge are shown in Table 3 below:

[0152] Table 3

[0153]

[0154] It can be seen from the above performance test 2 that the electrolyte in the present invention has a better cycle effect and a longer service life when used for batteries.

[0155] In summary, the present invention is applicable to an ether-based electrolyte based on an ionic liquid for a high-voltage lithium metal battery greater than 4V. The lithium salt and additives are mixed and added to an organic solvent and modified with an auxiliary ionic liquid, so that the ether electrolyte can be used in a high-voltage environment and exhibit good cycle performance, ensuring that a stable solid electrolyte interphase can be formed at the positive and negative electrodes of the battery under a high-voltage environment, avoiding continuous direct contact between the electrolyte and the positive or negative electrode of the battery, and improving the cycle performance and service life of the battery.

[0156] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. An ether-based electrolyte based on an ionic liquid suitable for a high voltage lithium metal battery greater than 4V, characterized in that: Including lithium salts, additives and solvents; The lithium salt is lithium bis(fluorosulfonyl)imide or lithium bis(trifluoromethanesulfonyl)imide, with a final concentration of 1-1.5 mol / L; The additive is at least one of lithium nitrate, lithium difluorophosphate and lithium difluorooxalate borate, and the total final concentration of the additive is 0.02-0.5 mol / L; The solvent is a mixed solvent of an ionic liquid and an ether solvent, with a volume ratio of 1:1-10.

2. The ether-based electrolyte based on ionic liquid suitable for high-voltage lithium metal batteries greater than 4V according to claim 1, characterized in that: The ionic liquid is 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide salt or 1-ethyl-3-methylimidazolium tetrafluoroborate.

3. The ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V according to claim 1, characterized in that: The ether solvent is ethylene glycol dimethyl ether.

4. The method for preparing an ether-based electrolyte based on an ionic liquid suitable for a lithium metal battery with a high voltage greater than 4V according to any one of claims 1 to 3, characterized in that: The steps include: Step (1), drying the lithium salt, ionic liquid and additive separately at 70-100° C. for at least 10 hours; Step (2), The molecular sieve is placed in a muffle furnace and activated at 350-500℃ for at least 10h; Add molecular sieves to ether solvent and let stand for 3-7 days; Step (3), mixing the lithium salt, additive, ionic liquid and ether solvent together until the lithium salt and additive are completely dissolved and mixed evenly, thereby obtaining an ether-based electrolyte based on ionic liquid suitable for a high-voltage lithium metal battery greater than 4V.

5. The method for preparing an ether-based electrolyte based on an ionic liquid suitable for a high-voltage lithium metal battery greater than 4V according to claim 4, characterized in that: In step (1), the drying time is 10h-24h.

6. Use of the ether-based electrolyte based on ionic liquid suitable for high-voltage lithium metal batteries with a voltage greater than 4V as claimed in any one of claims 1 to 3 in the preparation of high-voltage lithium metal batteries.

Citation Information

Patent Citations

  • Sulfuryl lithium battery electrolyte and lithium battery

    CN114725509A

  • Lithium ion battery electrolyte and preparation method and application thereof

    CN115295882A

  • Electrolyte and preparation method and application thereof

    CN115732760A

  • Novel amide electrolyte for lithium battery and preparation method thereof

    CN115966772A

  • High-voltage ether electrolyte for lithium metal battery

    CN116759650A