Spark plug
By setting specific pore distribution and seal design in the insulator of the spark plug, the problem of reduced thermal shock resistance of the insulator is solved, and the insulation endurance and thermal shock resistance are improved.
Patent Information
- Application Number
- CN202410356335.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-01
AI Technical Summary
The thermal shock resistance of the insulator of existing spark plugs may be reduced, affecting the insulation endurance.
Design a spark plug, in which an insulator is provided with an axial hole structure of a first hole and a second hole. The center electrode passes from the first hole through the second hole. The sealing member fixes the center electrode inside the insulator and uses specific pore distribution and The seal material design ensures the porosity and thermal expansion of the insulator. Specific measures include setting up a rectangular area in the cross section of the insulator, the ratio of the pore area to the total area is less than 5%, the average area of specific pores is less than 26.3 μm2, the number of pores with an area of 37 μm2 or more is less than 30, and the area is more than 51 μm2 The number of pores is more than 8, and the distance between these pores is more than 36.3μm.
It effectively improves the insulation endurance and thermal shock resistance of the insulator, ensuring the stability and mechanical strength in high temperature and high pressure environments.
Smart Images

Figure CN118739031A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a spark plug provided with an insulator. Background Art
[0002] Patent Document 1 discloses a related art in which abnormal grain growth of an insulator is suppressed in order to ensure the dielectric strength of a spark plug in which a center electrode is fixed to an insulator by a seal member disposed around the center electrode.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2022-190529 Summary of the invention
[0006] Problems to be solved by the invention
[0007] In the prior art, the thermal shock resistance of the insulator may be reduced.
[0008] The present invention has been made to solve this problem, and an object of the present invention is to provide a spark plug capable of ensuring insulation resistance and thermal shock resistance.
[0009] Means for solving problems
[0010] To achieve the object, the first aspect of the present invention is a spark plug comprising: an insulator having an axial hole formed by connecting a first hole and a second hole having a smaller diameter than the first hole via a connecting portion in the axial direction; a center electrode extending from the first hole through the second hole to the front end side; and a seal member arranged inside the insulator at the rear end side of the center electrode, wherein, in any cross section including the center line of the axial hole, when a rectangle is set in the insulator so that the front end of one of the long sides of a rectangle having an axial length of 1920 μm and a radial length of 510 μm is in contact with the front end of the first hole and the rear end of the long side is in contact with the first hole, the area of pores appearing in the rectangle accounts for 5% or less of the area of the rectangle. When a range is set in the insulator by dividing the rectangle into 20 equal parts by dividing the rectangle into two equal parts by dividing the rectangle into ten equal parts by dividing the rectangle into 20 equal parts, and 10 pores appearing in each range are selected in order from the pores with the largest area as specific pores, the average area of the specific pores is 26.3 μm 2 Below, the area of the specific pore is 37μm 2 The number of pores is less than 30 and the area is 51 μm 2 The number of pores is more than 8.
[0011] The second method is based on the first method, and the area of the specific pore is 37μm 2The distance between the above pores is 36.3 μm or more.
[0012] Effects of the Invention
[0013] The porosity of the rectangular portion of the insulator adjacent to the sealant, which has an axial length of 1920 μm and a radial length of 510 μm, is less than 5%. The average area of the pores appearing in the range of 20 equal parts of the rectangle is 26.3 μm, and the area of 10 specific pores selected from the largest to the smallest is 26.3 μm. 2 Below, the area of the specific pore is 37μm 2 The number of pores is less than 30, so the insulation resistance can be ensured. In addition, the area of the specific pores is 51μm 2 Since the number of the pores is 8 or more, the thermal shock resistance of the insulator can be ensured. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a one-side cross-sectional view of a spark plug according to an embodiment.
[0015] Figure 2 Yes Figure 1 II is a partially enlarged cross-sectional view of the spark plug.
[0016] Figure 3 This is a schematic diagram of a binary image in which a cross section of an insulator is magnified. DETAILED DESCRIPTION
[0017] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. Figure 1 This is a one-side cross-sectional view that combines an outer shape view and a full cross-sectional view with the center line X of the axial hole 12 of the spark plug 10 in one embodiment as the boundary. Figure 1 The lower side of the paper is referred to as the front end side of the spark plug 10, and the upper side of the paper is referred to as the rear end side of the spark plug 10 (in Figure 2 The spark plug 10 includes an insulator 11 and a center electrode 16.
[0018] The insulator 11 is a cylindrical component provided with an axial hole 12 extending along the axis O, and is made of ceramics such as alumina having excellent insulation and mechanical properties at high temperatures. In the present embodiment, the insulator 11 is an alumina-based sintered body. The axial hole 12 is connected from the rear end to the front end of the insulator 11 in the order of a first hole 13, a connecting portion 14, and a second hole 15. In the present embodiment, the first hole 13 and the second hole 15 are cylindrical surfaces with the same diameter throughout the entire length, and the connecting portion 14 is a conical surface whose diameter decreases as it moves toward the front end side. The connecting portion 14 can also be an annular plane perpendicular to the center line X of the first hole 13 and the second hole 15. The diameter of the second hole 15 is smaller than the diameter of the first hole 13.
[0019] A rod-shaped metal center electrode 16 is disposed in the axial hole 12 of the insulator 11. The center electrode 16 has a core material having excellent thermal conductivity buried in a base material. The base material is formed of an alloy mainly composed of Ni or a metal material composed of Ni. The core material is formed of copper or an alloy mainly composed of copper. The core material may be omitted. The center electrode 16 includes: a head 17 disposed in the first hole 13 and in contact with the connecting portion 14; and a leg 18 extending from the head 17 toward the front end side and disposed in the second hole 15. The head 17 and the leg 18 are integrally formed.
[0020] The terminal fitting 19 is a rod-shaped member connected to an ignition device (not shown), and is formed of a conductive metal material (such as low carbon steel). The front end side of the terminal fitting 19 is arranged in the first hole 13 of the insulator 11, and the rear end side of the terminal fitting 19 protrudes from the insulator 11. In the first hole 13 of the insulator 11, a seal 20, a resistor 21, and a seal 22 are arranged in order from the front end side between the center electrode 16 and the terminal fitting 19.
[0021] The seal 20 has the function of fixing the head 17 of the center electrode 16 to the insulator 11 and closing the first hole 13, and is arranged around the head 17. The seal 22 has the function of fixing the terminal fitting 19 to the insulator 11. The seals 20 and 22 have electrical conductivity, and contain glass particles and metal particles (Cu, Fe, etc.) at a ratio of about 1:1, for example. As the glass particles, materials such as B2O3-SiO2 system, BaO-B2O3 system, SiO2-B2O3-CaO-BaO system, etc. can be used. The thermal expansion coefficient of the seals 20 and 21 is between the thermal expansion coefficient of the ceramic insulator 11 and the thermal expansion coefficient of the metal center electrode 16.
[0022] The resistor 21 is a member for suppressing the radio noise generated during sparking. The resistor 21 is a mixture containing glass particles as a main component, ceramic particles other than glass, and a conductive material. As the material of the glass particles, for example, B2O3-SiO2 system, BaO-B2O3 system, SiO2-B2O3-CaO-BaO system and the like can be used. As the material of the ceramic particles, for example, TiO2, ZrO2 and the like can be used. As the conductive material, for example, non-metallic conductive materials such as carbon particles (carbon black, etc.), TiC particles, TiN particles, and metals such as Al, Mg, Ti, Zr and Zn can be used. Since the seals 20 and 22 are in contact with the resistor 21, the center electrode 16 and the terminal fitting 19 are electrically connected via the seals 20, 22 and the resistor 21.
[0023] The metal shell 23 is a substantially cylindrical member formed of a conductive metal material (e.g., low carbon steel). The metal shell 23 is disposed on the outer periphery of the insulator 11. The ground electrode 24 is a rod-shaped metal member (e.g., made of a nickel-based alloy) connected to the metal shell 23. A spark gap is formed between the ground electrode 24 and the leg portion 18 of the center electrode 16. A plurality of ground electrodes 24 may be connected to the metal shell 23.
[0024] Spark plug 10 is manufactured, for example, by the following method. First, center electrode 16 is inserted from first hole 13 of insulator 11. Center electrode 16 has head 17 disposed in first hole 13 and leg 18 disposed in second hole 15 in a state of being in contact with connection portion 14 of insulator 11.
[0025] Next, the raw material powder of the seal 20 is introduced from the first hole 13, and after the raw material powder is filled around the head 17 and at the rear end side of the first hole 13 relative to the head 17, the raw material powder is pre-compressed using a compression rod (not shown). Next, the raw material powder of the resistor 21 is filled on the raw material powder of the seal 20, and the raw material powder is pre-compressed using a compression rod. Finally, the raw material powder of the seal 22 is filled on the raw material powder of the resistor 21, and the raw material powder is pre-compressed using a compression rod.
[0026] The terminal fitting 19 is inserted from the rear end side of the first hole 13, and the front end of the terminal fitting 19 is brought into contact with the raw material powder of the seal 22. The terminal fitting 19 is then pressed in while being heated to a temperature higher than the softening point of the glass component contained in each raw material powder, for example, so that an axial load is applied to the raw material powder through the terminal fitting 19. Each raw material powder is compressed and sintered, and the seals 20 and 22 and the resistor 21 are manufactured in the first hole 13. Next, after the metal body 23 connected with the ground electrode 24 is assembled to the outer periphery of the insulator 11, the ground electrode 24 is bent, and a spark gap is set between the ground electrode 24 and the center electrode 16 to obtain the spark plug 10.
[0027] Figure 2 It is magnified Figure 1 The cross-sectional view of the portion II shown in FIG. 1 along the center line X of the axial hole 12 of the spark plug 10 shows the vicinity of the head 17 of the center electrode 16. A seal 20 is arranged around the head 17 of the first hole 13 arranged in the insulator 11. In the spark plug 10 installed in the engine (not shown), the heat of the combustion chamber is transmitted from the center electrode 16 (see FIG. 1 ). Figure 1 ) is transferred to the head 17 from the leg 18, and then to the seal 20 from the head 17. The thermal conductivity of the seal 20 is lower than that of the center electrode 16, so the thermal conductivity of the seal 20 becomes the speed limit of the thermal conduction, and the seal 20 is heated.
[0028] The head 17 is thicker than the leg 18, so the head 17 and the body metal part 23 (see Figure 1 ) is shorter than the distance between the leg portion 18 and the main body component 23. Therefore, the electric field between the head portion 17 and the main body component 23 is stronger than the electric field between the leg portion 18 and the main body component 23.
[0029] The seal 20 contains an alkali component derived from glass particles as a main component of the material. The insulator 11 composed of an alumina-based sintered body is excellent in resistance to alkali corrosion, but in the high-temperature and high-voltage environment where the spark plug 10 is installed in the engine, the alkali component penetrates through the pores of the insulator 11, which may cause a decrease in insulation resistance. In order to ensure insulation resistance, attention is paid to the pores of the portion of the insulator 11 adjacent to the seal 20.
[0030] A rectangle 25 for observing pores using a scanning electron microscope (SEM) is set in a portion of the insulator 11 adjacent to the seal 20. The lengths of the long sides 26 and 29 of the rectangle 25 are 1920 μm, and the lengths of the short sides 30 and 31 are 510 μm. The short sides 30 and 31 of the rectangle 25 are set along the radial direction of the insulator 11, and the long sides 26 and 29 are set along the axial direction of the insulator 11 in such a manner that the front end 27 of the long side 26 is connected to the front end of the first hole 13 and the rear end 28 of the long side 26 is connected to the first hole 13. The insulator 11 has a rounded corner at the intersection of the first hole 13 and the connecting portion 14, so the front end of the first hole 13 is the front end of the straight portion of the first hole 13 (the intersection of the rounded corner (curve) and the straight line).
[0031] Furthermore, 20 ranges 32 are set, which divide the rectangle 25 into 20 equal parts by dividing the short sides 30 and 31 of the rectangle 25 into two equal parts and dividing the long sides 26 and 29 into ten equal parts. The length of the short side extending in the axial direction of the range 32 is 192 μm, and the length of the long side extending in the radial direction is 255 μm. The size of the range 32 is equal to the size of one field of view observed using the SEM.
[0032] In order to obtain a SEM image of the cross section of the insulator 11 to calculate the area of the pores, the cross section of the insulator 11 is ground to a degree of accuracy that enables the shape of the pores appearing in the cross section to be determined. The surface roughness (Ra) of the ground insulator 11 is, for example, about 0.001 μm. In this embodiment, the acceleration voltage of the SEM is set to 20 kV, and the magnification of the SEM is set to 500 times.
[0033] After obtaining the SEM image in every 20 ranges 32, the image analysis is performed using a known image analysis software (e.g., WinROOF (registered trademark), manufactured by Mitani Shoji Co., Ltd.). In the image analysis, the size of the SEM image is corrected based on the scale marked on the SEM image, and then the SEM image is binarized. In the binarization process, the brightness (brightness) of each pixel of the SEM image is gray-scaled using a predetermined threshold value (e.g., threshold value 118). That is, the brightness of a pixel whose brightness is below the threshold is zero, and the brightness of a pixel whose brightness exceeds the threshold is "255". The intermediate grayscale is eliminated by gray-scale binarization of the pixels, thereby obtaining a binary image.
[0034] Figure 3 1 is a schematic diagram showing an enlarged binary image of the cross section of the insulator 11. Figure 3 In the figure, pores are represented by black, and the rest (ceramic particles and grain boundaries) are represented by white. Using the binary image of range 32, all pores (voids) contained in range 32 are extracted by a known image analysis method, and the area of each pore is calculated. The value (%) obtained by dividing the total area of all pores contained in 20 ranges 32 by the area of rectangle 25 is the porosity of insulator 11. The porosity of insulator 11 is less than 5%. This is to ensure the mechanical strength of insulator 11.
[0035] Next, for all the pores contained in the range 32, select 10 pores in order from the pore with the largest area. The 10 pores selected in order from the largest to the smallest area in each range 32 are called specific pores. There are 200 specific pores in the rectangle 25. The total area of the specific pores in each range 32 is calculated, and the average of the 20 ranges 32 is calculated. The total area of the specific pores calculated in each range 32 of the insulator 11, the average of the 20 ranges 32, that is, the total area of the 200 specific pores divided by 200 and rounded to the second decimal place, is 26.3μm 2 This is to limit the size of large pores (specific pores) that may cause insulation resistance to decrease due to the intrusion of alkali components, thereby reducing the intrusion of alkali components.
[0036] In addition, the distribution of specific pores was determined by a known image analysis method. The area of the specific pores in the insulator 11 was 37 μm 2 The number of pores is 30 or less. This is to limit the number of large pores that may cause the insulation resistance to decrease due to the intrusion of alkali components, thereby reducing the intrusion of alkali components. In addition, the area of the specific pores in the insulator 11 is 51 μm 2 The number of the pores is 8 or more. This is to ensure the number of particularly large pores and to ensure the thermal shock resistance of the insulator 11.
[0037] Furthermore, if Figure 3 As shown, the area of the specific pore is found to be 37 μm by a known image analysis method. 2 The distance L between the pores 33 and 34 is as follows. 2 In the case of the distance L between the pores 33 and 34 above, it is necessary not only to find the distance L between the pores existing in each range 32, but also to find the distance L between the pores existing in different ranges 32 across the adjacent positions of the range 32. The distance L of the insulator 11 is 36.3 μm or more. This is because the large pores that may cause the insulation resistance to decrease due to the invasion of alkali components are separated, thereby further reducing the invasion of alkali components.
[0038] An example of a method for producing the insulator 11 will be described. The insulator 11 is produced through the steps of slurry preparation, degassing, granulation, molding, grinding, and sintering. The steps will be described below in order.
[0039] The slurry preparation step is a step of preparing slurry by mixing raw material powder, a binder and a solvent. The raw material powder uses a powder of a compound that is converted into aluminum oxide by firing (hereinafter referred to as "Al compound powder") as a main component. As the Al compound powder, for example, aluminum oxide powder is used.
[0040] In the slurry making process, a pulverizing process for the purpose of mixing and pulverizing the raw material powder is carried out. The pulverizing process is carried out using a wet pulverizer using a ball mill or the like. The diameter of the jade used in the wet pulverizer is not particularly limited as long as it does not damage the purpose of the present invention, and is preferably more than 2 mm and less than 20 mm, more preferably more than 2 mm and less than 10 mm, and further preferably more than 2 mm and less than 6 mm. It is also possible to combine two or more pebbles with different diameters. Through such a pulverizing process, the deviation of the particle size (particle diameter) of the raw material powder is small, and it has a sharp particle size distribution. If such a raw material powder is used, then in the alumina-based sintered body obtained after sintering, the distribution and quantity of pores can be controlled, and the sintering density can be improved.
[0041] As long as the purpose of the present invention is not impaired, the particle size (particle size after crushing) of the Al compound powder (alumina powder, etc.) is not particularly limited, for example, it is preferably 1.5 μm or more, more preferably 1.7 μm or more, preferably 2.5 μm or less, and more preferably 2.0 μm or less. If the particle size of the Al compound powder is in such a range, the number of defects in the insulator is suppressed and a moderate sintering density is obtained. The particle size is a volume-based median particle size (D50) measured by a laser diffraction method (made by Nikkiso Co., Ltd., Microtrac particle size distribution measuring device, product name "MT-3000").
[0042] The Al compound powder is preferably prepared in such a manner that the Al compound powder is 90% by mass or more in terms of oxide when the mass (in terms of oxide) of the alumina-based sintered body after sintering is set to 100% by mass. It is more preferably 90% by mass or more and 98% by mass or less, and further preferably 90% by mass or more and 97% by mass or less. The raw material powder may also contain powders other than the Al compound powder as long as the purpose of the present invention is not impaired.
[0043] In order to improve the formability of the raw powder, a binder is added to the slurry. As such a binder, hydrophilic binders such as polyvinyl alcohol, aqueous acrylic resin, gum arabic, dextrin, etc. can be cited. They can be used alone or in combination of two or more. The amount of the binder is not particularly limited as long as it does not damage the purpose of the present invention. For example, relative to 100 parts by mass of the raw powder, it is mixed in a ratio of 1-10 parts by mass, preferably in a ratio of 3-7 parts by mass.
[0044] The solvent is used for the purpose of dispersing raw material powders, etc. Examples of the solvent include water and alcohol. They can be used alone or in combination of two or more. The amount of the solvent is not particularly limited as long as it does not impair the purpose of the present invention. For example, it is mixed in a ratio of 23-40 parts by mass, preferably 25-35 parts by mass, relative to 100 parts by mass of the raw material powder. Other ingredients other than the raw material powder, binder and solvent can be mixed in the slurry as needed. The slurry can be mixed using a known stirring and mixing device, etc.
[0045] The prepared slurry can be degassed as needed. In the degassed process, for example, a container containing the mixed (kneaded) slurry is placed in a vacuum degassing device, decompressed and placed in a low pressure environment, thereby removing bubbles contained in the slurry. By comparing the density of the slurry before and after degassed, the amount of bubbles in the slurry can be determined.
[0046] The granulation step is a step of making spherical granulated powder from a slurry containing raw material powder and the like. There is no particular limitation on the method of making granulated powder from the slurry as long as it does not impair the purpose of the present invention, and an example thereof may be a spray drying method. In the spray drying method, the slurry is spray-dried using a predetermined spray drying device to obtain granulated powder having a predetermined particle size. There is no particular limitation on the particle size of the granulated powder as long as it does not impair the purpose of the present invention, and for example, it is preferably 212 μm pass ≥ 95% or less, and more preferably 180 μm pass ≥ 95% or less.
[0047] The forming process is a process of forming the granulated powder into a predetermined shape using a forming die to obtain a formed body. The forming process is performed by rubber stamping, die stamping, etc. In the case of the present embodiment, the pressure (stamping pressure increase speed) applied to the forming die (for example, the inner rubber die and the outer rubber die of the rubber stamping machine) from the outer peripheral side is adjusted to rise in stages. In addition, it is preferably adjusted to a range of pressure higher than before (for example, more than 100 MPa). It should be noted that the upper limit of the pressure is not particularly limited as long as it does not impair the purpose of the present invention, and for example, it can be adjusted to less than 200 MPa.
[0048] The grinding process is a process of removing the machining allowance of the molded body obtained after the molding process, grinding the surface of the molded body, etc. In the grinding process, the machining allowance is removed, the surface of the molded body is ground, etc. by grinding with a resin bonded grinding wheel, etc. Through such a grinding process, the shape of the molded body is adjusted.
[0049] The firing step is a step of firing the molded body whose shape is adjusted by the grinding step to obtain an insulator. In the firing step, for example, the molded body is fired at 1450° C. to 1650° C. for 1 to 8 hours in an air atmosphere. After firing, the molded body is cooled to obtain an insulator 11 composed of an alumina-based sintered body.
[0050] [Example]
[0051] The present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.
[0052] (Insulator production)
[0053] Four insulators having the same basic structure as the insulator 11 of the spark plug 10 illustrated in the embodiment were manufactured from samples No. 1 to 17 using the same method as in the embodiment. The radial thickness of the front end of the first hole 13 of the insulator 11 is 3 mm. When the raw material powder is crushed by a wet pulverizer in the slurry preparation process, jade with a diameter of 2 mm and jade with a diameter of 6 mm are mixed in a ratio of 50% by mass and 50% by mass, respectively. The insulators of samples No. 2-8 are manufactured in the same manner as sample No. 1, except that the ratio of jade used when crushing the raw material powder in the slurry preparation process is appropriately changed.
[0054] In the insulator of sample No. 9, when the raw material powder was pulverized by a wet pulverizer in the slurry preparation process, jade with a diameter of 8 mm and jade with a diameter of 12 mm were mixed in a ratio of 50 mass % and 50 mass % respectively. Insulators of samples No. 10-15 and 17 were prepared in the same manner as sample No. 9, except that the ratio of jade used in pulverizing the raw material powder in the slurry preparation process was appropriately changed. Insulator of sample No. 16 was prepared in the same manner as sample No. 1, except that the amount of silica in the raw material powder was increased and the pressure in the forming process was made greater than the pressure in the forming process of the insulator of sample No. 1.
[0055] (Withstand voltage test)
[0056] Two samples of the spark plug 10 described in the embodiment were prepared using two insulators of each of the samples No. 1 to 17, four of which were prepared. One sample was subjected to a withstand voltage test specified in JIS B8031: 2006. After the ground electrode 24 was removed so that no discharge occurred between the center electrode 16 and the ground electrode 24, the metal shell 23 was tightened to a pressure chamber at a specified torque. After carbon dioxide was supplied to the pressure chamber to a pressure of about 5 MPa, the voltage applied between the terminal fitting 19 and the metal shell 23 of the sample was increased from 0 V at a rate of 0.1 kV / sec, and the dielectric breakdown voltage when the insulator 11 was penetrated was examined. The dielectric breakdown voltage was in the range of 40 kV to 42 kV.
[0057] Another sample was subjected to the conditions of removing the ground electrode 24 so as to prevent discharge between the center electrode 16 and the ground electrode 24, and further covering the front end of the insulator 11 with a heat-resistant insulating tube. The sample was placed in a heating furnace maintained at about 200°C, and a voltage of 35 kV was applied between the terminal fitting 19 and the metal shell 23 for 100 hours. This is to place the sample in an environment where the insulator 11 is easily corroded by the alkali component contained in the seal 20 disposed around the head 17 of the center electrode 16. The presence or absence of alkali corrosion can be determined by measuring the presence or absence of alkali metals such as Na and alkaline earth metals in the insulator 11 using an electron beam probe microanalyzer (EPMA).
[0058] After the sample was taken out of the heating furnace, the metal shell 23 was fastened to the pressure chamber at a specified torque according to the withstand voltage test specified in JIS B8031: 2006. After carbon dioxide was supplied to the pressure chamber to a pressure of about 5 MPa, the voltage applied between the terminal fitting 19 and the metal shell 23 of the sample was increased from 0 V at a rate of 0.1 kV / sec, and the dielectric breakdown voltage when the dielectric breakdown voltage penetrated the insulator 11 was examined. The samples with a dielectric breakdown voltage of 38 kV or more after alkali corrosion were judged as A, the samples with a dielectric breakdown voltage of 36 kV or more and less than 38 kV were judged as B, the samples with a dielectric breakdown voltage of 33 kV or more and less than 36 kV were judged as C, and the samples with a dielectric breakdown voltage of less than 33 kV were judged as D. The results are recorded in the insulation withstand voltage column of Table 1.
[0059] (Cross-sectional observation of insulator)
[0060] Each of the insulators 11 of the samples No. 1 to 17, each of which 4 pieces were produced, was cut at a position including the center line X of the axial hole 12. The cut surface of the insulator 11 was polished to a mirror surface, and the structure of the polished surface was observed using a SEM (JEM-IT 300LA, manufactured by JEOL Ltd.). Ten rectangular ranges 32 (long side length 255 μm, short side length 195 μm) whose short sides were connected to the first hole 13 of the insulator 11 were set, and 10 ranges 32 adjacent to the radial outer side of the 10 ranges 32 were set. After obtaining 20 SEM images corresponding to the 20 ranges 32, processing based on the image processing software WinROOF 2013 (Win ROOF is a registered trademark) was performed to calculate the ratio (porosity) of the total area of pores appearing in the entire 20 ranges 32 (rectangle 25) to the area of the rectangle 25. The porosity of the insulator 11 of the samples No. 1 to No. 17 was less than 5%.
[0061] By image analysis, 10 pores are selected from the pores with the largest area in order from all pores included in the range 32, and the total area of the selected 10 pores (specific pores) is calculated for each range 32, and the average of 20 ranges 32 is calculated (rounded to the second decimal place). The results are recorded in the "Area of specific pores" column of Table 1.
[0062] Through image analysis, the area of specific pores was found to be 37 μm 2 The number and area of pores above 51μm 2 The number of pores in the 20 ranges 32 is summed up to find the number of pores. The results are recorded in the "37μm" column of Table 1. 2 Pores above 51μm 2 The column for "pores above" is displayed.
[0063] Through image analysis, two specific pores appearing in rectangle 25 are selected, each with an area of 37 μm. 2 For the above pores, two pores with an area of 37 μm are selected. 2 For all combinations of the above pores, the distance L between the pores was determined. The shortest distance among all the distances L was recorded in the column "Distance between pores" in Table 1.
[0064] (Thermal shock test)
[0065] After the insulators 11 of sample No. 1-17 were stored in a thermostatic bath maintained at a predetermined temperature for 30 minutes, they were immediately immersed in water at 20°C for rapid cooling. The posture of the insulator 11 when immersed in water was set so that the center line X of the axial hole 12 of the insulator 11 was parallel to the water surface. The presence or absence of cracks in the insulator 11 taken out of the water was confirmed visually by applying a penetrant flaw detection liquid. The temperature of the thermostatic bath in which the insulator 11 was stored was increased from 150°C in units of 10°C until cracks were found in the insulator 11, and the temperature difference (critical temperature difference) between the temperature of the thermostatic bath and the water temperature (20°C) when cracks were found in the insulator 11 was investigated. Samples with a critical temperature difference of 210°C or more were judged as A, and samples with a critical temperature difference of less than 210°C were judged as D. The results are recorded in the thermal shock column of Table 1.
[0066] [Table 1]
[0067]
[0068] As shown in Table 1, the average area of specific pores is 26.3 μm 2 Below, the area is 37μm 2 The insulation resistance of samples No. 1-8 and No. 16, in which the number of pores was 30 or less, was judged as A or B. On the other hand, the average area of the specific pores was larger than 26.3 μm. 2 The insulation resistance of samples No. 11-15 and 17 was judged as D. In addition, even if the average area of the specific pores is 26.3 μm 2 Below, area 37μm 2 The insulation resistance of samples 9 and 10, which have more than 30 pores, was also judged as C. It can be seen that the average area of the specific pores of the insulator 11 is 26.3 μm 2 The following are the necessary conditions for determining insulation resistance A or B, with an area of 37μm 2 The above-mentioned condition that the number of pores is 30 or less is a sufficient condition for the dielectric strength determination A or B.
[0069] Area: 51 μm 2 The thermal shock properties of samples No. 1-12, 14, 15, and 17, which had 8 or more pores, were judged as A. On the other hand, the samples with an area of 51 μm 2The thermal shock properties of samples No. 13 and 16, which have 7 or less pores, were rated D. It can be seen that if the area is 51 μm 2 When there are 8 or more pores, the critical temperature difference of the insulator 11 can be increased, that is, the rapid cooling resistance is improved. It is considered that the pores relieve the tensile stress generated in the insulator 11 due to rapid cooling.
[0070] The insulation resistance of sample No. 1-8 was judged as A or B, and the thermal shock resistance was judged as A. Therefore, it can be seen that in order to ensure the insulation resistance and thermal shock resistance of the spark plug 10 used in a high temperature environment, the porosity of the insulator 11 is set to be less than 5% and the average area of the specific pores is set to 26.3 μm. 2 Below, area 37μm 2 The number of pores is less than 30 and the area is 51 μm 2 The above pores are effective when the number is 8 or more.
[0071] The insulation resistance and thermal shock resistance of sample No. 1-7 were both rated A. Therefore, it can be seen that in order to ensure insulation resistance and thermal shock resistance, the porosity of the insulator 11 is set to 5% or less and the average area of specific pores is set to 26.3 μm. 2 Below, area 37μm 2 There are less than 30 pores and the area is 51μm 2 There are more than 8 pores with an area of 37μm 2 It is particularly effective that the distance between the above pores is 36.3 μm or more.
[0072] The present invention has been described above based on the embodiment, but the present invention is not limited to the above embodiment, and it can be easily estimated that various modifications can be made without departing from the scope of the present invention. For example, the shape and size of the head 17 of the center electrode 16 are just examples and can be set appropriately.
[0073] In the embodiment, the spark plug 10 in which the resistor 21 is disposed in the insulator 11 is described, but the present invention is not necessarily limited to this. Of course, the structure of the embodiment can be applied to a spark plug that does not have a built-in resistor 21. This is because if the head 17 of the center electrode 16 is fixed by the seal 20, the same effects as those of the above-mentioned embodiment can be achieved.
[0074] In the embodiment, the spark plug 10 is described in which the ground electrode 24 is exposed to the combustion chamber when the spark plug 10 is installed in the engine (not shown), but it is not necessarily limited to this. Of course, the structure of the embodiment can be applied to a spark plug in which the ground electrode 24 is covered by a cap provided with a through hole (a spark plug in which a sub chamber is provided in the combustion chamber).
[0075] In the embodiment, the spark plug 10 that generates spark discharge between the center electrode 16 and the ground electrode 24 is described, but the present invention is not necessarily limited thereto. The structure of the embodiment can of course be applied to a spark plug that utilizes non-equilibrium plasma generated around the leg portion 18 of the center electrode 16 .
[0076] Description of Reference Numerals
[0077] 10 Spark plug
[0078] 11 Insulator
[0079] 12 Axis holes
[0080] 13. First Hole
[0081] 14Connection
[0082] 15 Second hole
[0083] 16 Center Electrode
[0084] 20 Seals
[0085] 25 Rectangle
[0086] 26 long side
[0087] 27 Front end of long side
[0088] 28 rear end of the long side
[0089] 30, 31 short side
[0090] 32 Range
[0091] X center line
Claims
1. A spark plug comprising: The insulator is provided with an axial hole, wherein the axial hole is formed by connecting a first hole and a second hole having a smaller diameter than the first hole via a connecting portion in the axial direction; a center electrode extending from the first hole through the second hole toward the front end side; and a seal member disposed inside the insulator on the rear end side of the center electrode, In any cross section containing the center line of the axial hole, When the rectangle is set in the insulator so that the front end of one of the long sides of the rectangle having an axial length of 1920 μm and a radial length of 510 μm is in contact with the front end of the first hole and the rear end of the long side is in contact with the first hole, The area of the pores in the rectangle accounts for less than 5% of the area of the rectangle. in, In the insulator, the short side of the rectangle is divided into two equal parts and the long side of the rectangle is divided into ten equal parts to divide the rectangle into 20 ranges, and 10 pores are selected from the pores with the largest area in each range as specific pores. In this case, The average area of the specific pores is 26.3 μm 2 the following, The area of the specific pore is 37 μm 2 The number of pores is less than 30 and the area is 51 μm 2 The number of pores is more than 8.