Plasma-treated monatomic catalyst, method for production thereof and use of catalyst
By treating metal oxide supports and catalytically active materials of precious metals under O2 conditions, surface peroxyl species and nanoclusters are formed, which solves the problem of insufficient activity and stability of existing catalysts in alkyne hydrogenation and CO oxidation reactions. Achieve efficient catalytic effect.
Patent Information
- Application Number
- CN202280091991.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-30
- Filing Date
- 2022-12-22
- Publication Date
- 2024-10-01
AI Technical Summary
Existing catalysts have insufficient activity and selectivity in alkyne hydrogenation and CO oxidation reactions, and are unstable under high temperatures and reducing environments. Traditional support materials cannot effectively anchor small metal clusters or single-atom catalysts.
Catalytically active materials including metal oxide carriers and atomically dispersed noble metals are used, prepared through non-thermal plasma treatment under O2 conditions, to form surface peroxyl species and metal oxide nanoclusters to improve catalytic activity and stability.
It achieves excellent catalytic activity and stability at low reaction temperatures, and improves the efficiency and selectivity of alkyne hydrogenation and CO oxidation reactions.
Smart Images

Figure CN118742385A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a catalytically active material, its preparation and the use of the catalytically active material. Background Art
[0002] The catalytic selective hydrogenation of alkynes to olefins is an industrially important reaction. For example, the hydrogenation of acetylene to ethylene is a key process for removing acetylene from the ethylene feedstock for polyethylene production, because the catalysts used for polyethylene production are poisoned by the acetylene in the ethylene feedstock. Catalysts based on nanoparticles containing noble metals such as Pt and Pd are used in the hydrogenation of alkynes. For example, the use of intermetallic Pt / Ga nanoparticles is reported in EP 2 060 323 A1.
[0003] The catalytic oxidation of CO to CO2 is of great significance to the pollution control in the automotive industry. Known noble metals (such as Pt, Pd, Rh and Au) are particularly active in catalyzing CO oxidation reactions. Because noble metals are expensive, CO oxidation catalysts usually contain highly dispersed noble metal nanoparticles supported on metal oxides. For example, EP 0 602 865 A1 relates to CeO2 as a carrier material for catalysts. Compared with this nanoparticle catalyst, single atom catalysts (single atom catalyst, SAC) are generally considered to have advantages because they maximize the efficiency of noble metals. Because catalysis is a surface reaction process, using smaller metal particles can save costs and / or produce better catalytic selectivity / activity.
[0004] However, as described in US2021 / 0016256 A1, smaller metal particles, clusters or single atoms are not thermodynamically stable and are typically sintered to form larger particles during the catalytic reaction, especially at elevated temperatures and in a reducing environment. Typical inert refractory support materials (e.g., SiO2, Al2O3, etc.) have been used as high surface area supports, but generally do not strongly anchor small metal clusters or single metal atoms. In this context, US2021 / 0016256 A1 proposes a method for synthesizing a nanocomposite catalyst using small clusters and nanoparticles of reducible oxides (CeOx, FeOx, NbOx, etc.) deposited on an inert refractory support material, the inert refractory support material being selected from silica, alumina, magnesia, zirconia, cordierite, mullite, perovskite, or any combination thereof. One or more atoms of Pt, Au, Pd, etc. are deposited onto this "nanocomposite" via strong electrostatic adsorption (SEA) from aqueous solution. The synthesis of nanocomposite catalysts requires a calcination step in air at, for example, 400°C or 600°C.
[0005] US2021 / 0016256 A1 claims to synthesize 0.05wt% Pt1 / CeOx-SiO2 or 0.05wt% Pd1 / CeOx-SiO2 single atom catalysts. Increasing the Pt loading to 2wt.% leads to the formation of Pt clusters and nanoparticles.
[0006] Therefore, there is a need for SACs with high metal loadings, which not only exhibit excellent activity and selectivity but are also stable under catalytically relevant conditions.
[0007] Technical issues
[0008] An object of the present invention is to provide a catalytically active material which can be effectively used for the oxidation of CO. Another object is to provide a catalytically active material suitable for the oxidation of CO which exhibits high activity and / or stability in this reaction.
[0009] According to another aspect, the object of the present invention is to provide a catalytically active material that can be effectively used for the hydrogenation of alkynes. Another object is to provide a catalytically active material suitable for the hydrogenation of alkynes, which catalytically active material exhibits high activity, high selectivity and / or stability in this reaction.
[0010] According to a further aspect, it is an object of the present invention to provide a simple and efficient process for the preparation of such catalytically active materials which enables appropriate use. Summary of the invention
[0011] The present inventors have found that the above-mentioned problems are solved by the following embodiments.
[0012] [1] A catalytically active material comprising
[0013] A support comprising a metal oxide, and
[0014] A noble metal is atomically dispersed on the surface of the carrier, wherein
[0015] The metal oxide is selected from TiO2, CeO2, ZnO, SnO2, Ga2O3, In2O3, ZrO2 and Fe2O3,
[0016] The noble metal is selected from Pt, Pd, Rh and Au, and
[0017] The catalytically active material is obtainable by a method comprising the following steps: a non-thermal plasma treatment in the presence of O2.
[0018] [2] The catalytically active material according to [1], wherein
[0019] The number of noble metal atoms normalized to the surface area of the catalytically active material is 3.0×10 12 at / cm 2 Up to 8.0×10 14 at / cm 2 , preferably 3.0×10 12 at / cm 2 Up to 4.0×10 14 at / cm 2 , more preferably 6.0×10 12 at / cm 2 Up to 2.0×10 14 at / cm 2 .
[0020] [3] The catalytically active material according to [1] or [2], wherein
[0021] The relative intensity of the noble metal in oxidation state X relative to the total intensity of the noble metal in all oxidation states in the catalytically active material, as measured by X-ray photoelectron spectroscopy, is 50% or more, preferably 75% or more, wherein
[0022] For Pt and Pd, X is 2+; for Rh and Au, X is 3+.
[0023] [4] The catalytically active material according to any one of [1] to [3], wherein
[0024] When measured under the following conditions, the infrared absorption spectrum measured for the catalytically active material shows a peak at 2085 cm -1 Up to 2120cm -1 The absorption band in the range of , which does not change when the material is heated from 300K to 500K:
[0025] (1) exposing the catalytically active material in the reaction cell to a reaction mixture consisting of 1% CO and 5% O2 balanced to 1 bar by Ar,
[0026] (2) heating the catalytically active material to 500 K at a rate of 60 K / min and reacting the mixture at 500 K and 1 bar for 5 min;
[0027] (3) cooling the reaction mixture and catalytically active material to 300K,
[0028] (4) Remove the reaction mixture from the reaction unit and apply 10 -9 The following ultrahigh vacuum (UHV) conditions,
[0029] (5) Spectra were recorded in UHV at 300K without additional exposure to CO,
[0030] (6) increasing the temperature to 500 K at a rate of 60 K / min and recording spectra at 320 K, 360 K, 400 K, 440 K, 480 K, and 500 K, and
[0031] (7) Compare the absorption maxima in the spectra recorded at the respective temperatures.
[0032] [5] The catalytically active material according to any one of [1] to [4], wherein the metal oxide and the noble metal are selected from the following material combinations:
[0033] a metal oxide selected from TiO2 and CeO2, and
[0034] Noble metals from Pt and Pd, of which
[0035] The metal oxide is preferably CeO2 and the noble metal is preferably Pt.
[0036] [6] The catalytically active material according to any one of [1] to [5], wherein
[0037] The carrier is in the form of particles, such as a powder.
[0038] [7] The catalytically active material according to [6], wherein
[0039] The support is composed of a metal oxide.
[0040] [8] The catalytically active material according to [6] or [7], wherein
[0041] The powder support has an average particle diameter of 10 nm to 50 nm as measured by scanning transmission electron microscopy, and is preferably a CeO2 powder support.
[0042] [9] The catalytically active material according to any one of [6] to [8], wherein
[0043] The catalytically active material consists of a carrier and a noble metal.
[0044]
[10] The catalytically active material according to any one of [1] to [5], wherein
[0045] The carrier is in the form of a film.
[0046]
[11] The catalytically active material according to
[10] , wherein
[0047] The carrier is composed of a substrate and clusters supported on the substrate.
[0048] The substrate and the clusters comprise the same metal oxide, and
[0049] The average diameter of the clusters determined by scanning tunneling microscopy is 2.0 nm or less, preferably 1.5 nm or less.
[0050]
[12] The catalytically active material according to
[11] , wherein the substrate and the clusters are composed of the same metal oxide.
[0051]
[13] Use of the catalytically active material according to any one of [1] to
[12] in the catalytic oxidation of CO to CO2, wherein, preferably, the catalytically active material is used as follows:
[0052] A gas mixture comprising CO and O2 is reacted in the presence of a catalytically active material at a pressure of 0.8 to 2.0 bar and at a reaction temperature of 323 K to 573 K, wherein
[0053] The CO content in the gas mixture is less than 5% by volume,
[0054] The content of O2 in the gas mixture is 2% by volume or more and 25% by volume or less, and
[0055] The CO / O2 molar ratio is preferably 2.0 or less.
[0056]
[14] Use of the catalytically active material according to any one of [1] to
[12] in the catalytic hydrogenation of alkynes, wherein, preferably, the catalytically active material is used as follows:
[0057] A gas mixture comprising an alkyne and H2 is reacted in the presence of a catalytically active material at a pressure of 0.8 to 2.0 bar and a temperature of 323 K to 573 K, wherein
[0058] The content of alkynes in the gas mixture is less than 10% by volume,
[0059] The molar ratio of alkyne to H2 in the gas mixture is less than 1, and
[0060] The alkyne is preferably a C2-C5 alkyne, more preferably a C2-C3 alkyne.
[0061]
[15] A method for producing a catalytically active material according to any one of [6] to [9], the method comprising the following steps:
[0062] (1) Providing a precursor for a catalytically active material, the catalytically active material comprising
[0063] a support in particulate form comprising a metal oxide, and
[0064] The precious metal on the surface of the carrier,
[0065] (2) calcining a precursor for a catalytically active material in the presence of O2, and
[0066] (3) Non-thermal plasma treatment of a calcined precursor for a catalytically active material in the presence of O2.
[0067]
[16] The method according to
[15] , wherein step (1) is selected from the following steps (1a) and (1b):
[0068] (1a) depositing a noble metal onto a support, preferably from an aqueous solution of a salt of the noble metal, wherein preferably the support consists of a metal oxide, and
[0069] (1b) Co-precipitating a noble metal and a metal oxide from an aqueous solution containing a salt of the noble metal and the metal oxide.
[0070]
[17] The method according to
[15] or
[16] , wherein the non-thermal plasma treatment is carried out at a pressure below 20 mbar and an O2 content of more than 5 volume %.
[0071]
[18] A method for producing the catalytically active material described in any one of
[10] to
[12] , the method being selected from method A and method B,
[0072] Method A comprises the following steps:
[0073] (1) providing a metal oxide film support,
[0074] (2) performing a non-thermal plasma treatment in the presence of O2 to obtain a plasma-treated metal oxide film support, and
[0075] (3) depositing the noble metal onto the plasma-treated metal oxide film support in the gas phase, preferably by physical vapor deposition of the noble metal atoms;
[0076] Method B comprises the following steps
[0077] (1) providing a metal oxide film support,
[0078] (2) depositing a noble metal onto a metal oxide film support from a solution containing the noble metal, and
[0079] (3) non-thermal plasma treatment in the presence of O2;
[0080] Among them, it is preferred to -6 mbar to 1×10 -5 The non-thermal plasma treatment is carried out under a pressure of O 2 of mbar.
[0081] Insofar as the present description refers to preferred embodiments / features (including all degrees of preference), combinations of these preferred embodiments / features shall also be considered disclosed insofar as these combinations make technical sense.
[0082] In the present text, the use of the terms "comprising" or "including" is to be understood as also being disclosed as a stricter embodiment, insofar as this makes technical sense, as the term "consisting of".
[0083] If preferred upper and lower limits are stated for certain features, this should be understood to disclose any combination of upper and lower limits.
[0084] In the following, depending on the context, the term "catalytically active material" may also be replaced by "catalyst". BRIEF DESCRIPTION OF THE DRAWINGS
[0085] Figure 1 Schematic diagram of the apparatus used for O2-plasma treatment of samples in film form (A) and particle form (B).
[0086] Figure 2.(Left side) Low energy electron diffraction (LEED) patterns (measured at 81 eV) of the “CeO2-plasma” film carrier of Reference Example 4, the “CeO2-step” film carrier of Reference Example 3, the “CeO2-red” film carrier of Reference Example 2, and the “CeO2(111)” film carrier of Reference Example 1 (from top to bottom).
[0087] (Right) X-ray photoemission spectra (XPS) of Pt 4f obtained for the Pt / CeO2-plasma sample of Example 1, the Pt / CeO2-step sample of Comparative Example 3, the Pt / CeO2-red sample of Comparative Example 2, and the Pt / CeO2(111) sample of Comparative Example 1 before and after CO oxidation reaction (10 mbar CO, 50 mbar O2, equilibrated from He to 1 bar, 523 K) (from top to bottom). -9 The XPS of Pt 4f before reaction was measured after annealing at 523 K in an ultra-high vacuum (UHV) at a pressure of mbar.
[0088] Figure 3 . XPS spectra of Pt 4f, Ce 3d and O1s of the Pt / CeO2(111) film sample according to Comparative Example 1: (i) measured at 300K after the Pt deposition step; (ii) measured during the UHV annealing step immediately after reaching a temperature of 523K; (iii) after UHV annealing at 523K for 5 min; (iv) after CO oxidation reaction. (v) XPS spectrum of Ce 3d normalized to the peak intensity at 882 eV. The region where the spectrum changes is highlighted with a grey box. Ce 3d is shown near the spectrum. 3+ The relative content of .
[0089] Figure 4 . XPS spectra of Pt 4f, Ce 3d and O1s of the Pt / CeO2-red film sample according to Comparative Example 2: (i) measured at 300K after the Pt deposition step; (ii) measured during the UHV annealing step immediately after reaching a temperature of 523K; (iii) after UHV annealing at 523K for 5 min; (iv) after CO oxidation reaction. (v) XPS spectrum of Ce 3d normalized to a peak intensity of 882 eV. The region where the spectrum changes is highlighted with a grey box. Ce 3d is shown near the spectrum. 3+ The relative content of .
[0090] Figure 5. XPS spectra of Pt 4f, Ce 3d and O1s of the Pt / CeO2-step film sample according to Comparative Example 3: (i) measured at 300K after the Pt deposition step; (ii) measured during the UHV annealing step immediately after reaching a temperature of 523K; (iii) after UHV annealing at 523K for 5 min; (iv) after CO oxidation reaction. (v) XPS spectrum of Ce 3d normalized to a peak intensity of 882 eV. The region where the spectrum changes is highlighted with a grey box. Ce 3d is shown near the spectrum. 3+ The relative content of .
[0091] Figure 6 . XPS spectra of Pt 4f, Ce 3d and O1s of the Pt / CeO2-plasma film sample according to Example 1: (i) measured at 300K after the Pt deposition step; (ii) measured during the UHV annealing step immediately after reaching a temperature of 523K; (iii) after UHV annealing at 523K for 5 min; (iv) after CO oxidation reaction. (v) XPS spectrum of Ce 3d normalized to a peak intensity of 882 eV. The region where the spectrum changes is highlighted with a grey box. Ce 3d is shown near the spectrum. 3+ The relative content of .
[0092] Figure 7 (a) STM images of a CeO2(111) film support according to Reference Example 1 and (b), (c) STM images of a CeO2-plasma film support according to Reference Example 4, each measured in UHV at 523K. (d) Topography profile along the line marked in the STM image (C). (e) XPS spectra of O1s of the CeO2-plasma film support according to Reference Example 4 measured under normal (upper spectrum) and glancing (lower spectrum) emission. (f) Binding energy shifts of peroxy-O atoms (open symbols) and surface O atoms of CeO2 (filled symbols) at the surface of CeO2, referenced to lattice O atoms in bulk CeO2 (zeroed), calculated for each of the CeO2(111), CeO2(110) and CeO2(100) surfaces. The latter are abundant and dominate in the experimental spectra. The shaded area highlights the experimentally measured BE shift. The inset shows a top-down view of the topmost layer in the Density Functional Theory (DFT) optimized structure, containing 1 / 4 monolayer of peroxide species on the (111), (110), and (100) surfaces.
[0093] Figure 8Schematic representation of the pristine (100), (110), (100), and (100)-4O surfaces of CeO2 viewed from the top (above), and of the peroxide species formed on the same surfaces of CeO2 by reaction with oxygen radicals (below). Oxygen-oxygen bond lengths are annotated.
[0094] Fig. 9 Schematic diagram of the (111), (110), (100), and (100)-4O surfaces of CeO2 viewed from the top, with a monolayer peroxide coverage of 0.5 with diagonal-wise and row-wise arrangement of peroxide species.
[0095] Fig.10 .Infrared reflection-absorption spectra (IRAS) measured in ultra-high vacuum for (a) the (annealed) Pt / CeO2(111) film sample according to Comparative Example 1 and (b) the (annealed) Pt / CeO2-plasma film sample with CO adsorption according to Example 1.
[0096] Fig.11 . XPS spectra of (a) Pt 4f and (b) O 1s of the (annealed) Pt / CeO2-plasma film sample according to Example 1 and the (annealed) Pt / CeO2-sputtered film sample according to Comparative Example 4.
[0097] Fig.12 (a) CO oxidation rates measured for the "Pt / CeO2-plasma" film sample according to Example 1 and the "Pt / CeO2(111)" film sample according to Comparative Example 1, and their comparison with the "CeO2-plasma" and "CeO2(111)" film samples. (b) XPS spectra of Pt 4f measured for the "Pt / CeO2-plasma film" sample according to Example 1 and the "Pt / CeO2(111) film" sample according to Comparative Example 1 after CO oxidation reaction.
[0098] Fig.13(a) CO oxidation rates measured for the plasma-treated Pt / CeO2 powder catalyst according to Example 2 and the pristine Pt / CeO2 powder catalyst according to Comparative Example 5, and their comparison with the "CeO2-plasma" and "CeO2" powder samples. Aberration-corrected scanning transmission electron microscopy (STEM) images of the plasma-treated Pt / CeO2 powder catalyst according to Example 2 before (b) and after (c) CO oxidation reaction at 523°C. Some Pt single atoms are highlighted with circles.
[0099] Fig.14 XPS spectra of Pt 4f of (a) the plasma-treated Pt / CeO2 powder catalysts according to Examples 2 to 4 and (b) the pristine Pt / CeO2 powder catalysts according to Comparative Examples 5 to 7 measured after 3 h of CO oxidation reaction at 523 K.
[0100] Fig.15 Aberration-corrected STEM images of (a) the original Pt / CeO2 powder catalyst according to Comparative Example 6, (b) the plasma-treated Pt / CeO2 powder catalyst according to Example 3, (c) the original Pt / CeO2 powder catalyst according to Comparative Example 7, and (d) the plasma-treated Pt / CeO2 powder catalyst according to Example 4 measured after 3 h of CO oxidation reaction at 523 K. Pt single atoms are highlighted with dashed circles and PtO x Clusters are highlighted with solid circles.
[0101] Fig.16 (a) Raman spectra observed for the original CeO2 support according to Reference Example 5 (denoted as "CeO2-calcined") and the plasma-treated CeO2 support according to Reference Example 6 (denoted as "CeO2-plasma"). (b) Raman spectra observed for the original Pt / CeO2 catalyst according to Comparative Example 5 (denoted as "Pt / CeO2-calcined") and the plasma-treated Pt / CeO2 catalyst according to Example 2 (denoted as "Pt / CeO2-plasma"). All spectra were normalized to 465 cm -1 The maximum of the main peak at is shown and is vertically offset for clarity.
[0102] Fig.17. Ethylene production rates observed for the plasma-treated Pt / CeO2 powder catalyst according to Example 2 ("Pt / CeO2-pla(sma)"), the original Pt / CeO2 powder catalyst according to Comparative Example 5 ("Pt / CeO2-cal(cined)"), the Pt-free, calcined CeO2 powder support according to Reference Example 5 ("CeO2-cal(cined)"), and the plasma-treated CeO2 powder support according to Reference Example 6 ("CeO2-pla(sma)").
[0103] Fig.18 .XPS spectra of Pt 4f measured for the Pt / CeO2-plasma film sample according to Example 1, the Pt / CeO2(111) film sample according to Comparative Example 1, the Pt / TiO2-plasma film sample according to Example 5, and the Pt / TiO2(110) film sample according to Comparative Example 8 after UHV annealing at 523K for 5 minutes.
[0104] Fig.19 .Schematic representation of the reconstruction of CeO2(111) film leading to the formation of CeO2 nanoclusters while reducing the film thickness.
[0105] Fig. 20 .Robustness analysis of the final input parameters used in the thermal model calculations.
[0106] Fig.21 Schematic representation of the energetically most favorable optimized structures of Pt atoms adsorbed on the (111), (110), (100), and (100)-4O surfaces of CeO2 with different peroxide coverages ranging from 0 (denoted as “Pris”) to 1.0 monolayer (denoted as “1.0”), all viewed from the top.
[0107] Fig. 22 .Schematic representation of the stepped (112)b, (210), (211)a, (211)b, (221), (310), (311)a, and (311)b surfaces of CeO2 and adsorbed Pt atoms, which are used to approximate the edge energies used in the thermodynamic model of ceria nanoparticle formation and consider alternative binding sites for single atomic Pt.
[0108] Fig.23 .(a) For the CeO2 nanoparticle / film model composite system (Ce 178 O 356(a) Schematic diagram of Pt atoms adsorbed on different sites (shown in the middle). The adsorption energies (in eV; referenced to bulk Pt) are shown near the structure. (b) Schematic diagram of optimized geometries for CO adsorption on Pt single atoms at the CeO2 nanoparticle / boundary and (100)-4O (denoted as “Pt-4O”) as well as (100)-3O (denoted as “Pt-3O”) and (100)-2O (denoted as “Pt-2O”). The Pt-3O and Pt-2O sites are generated by removing one or two ligand oxygen atoms from Pt-4O. The adsorption energies of CO (in eV) are shown.
[0109] Fig.24 Schematic diagram of Pt bound at the boundary and (100)-4O, and Pt bound at (100)-3O and (100)-2O sites derived from the (100)-4O site, and the calculated adsorption energy of CO (in eV) for the CeO2 nanoparticle / slab model system.
[0110] Fig.25 Schematic illustration of the interaction of Pt atoms with CeO2(111) film supports and CeO2-plasma film supports. Pt forms small clusters upon deposition on CeO2(111) surfaces that aggregate into larger Pt nanoparticles at elevated temperatures (top row). Plasma treatment of CeO2(111) surfaces in the presence of O2 generates peroxospecies and induces surface reconstruction, leading to small ceria nanoparticles (bottom row) that act as anchoring centers either directly upon Pt adsorption or through surface migration of peroxo-stabilized Pt single atoms. DETAILED DESCRIPTION
[0111] I. Catalytically active materials
[0112] The catalytically active material of the present invention comprises a support containing a metal oxide and a noble metal dispersed atomically on the surface of the support. The support comprises a metal oxide, and the metal oxide is selected from TiO2, CeO2, ZnO, SnO2, Ga2O3, In2O3, ZrO2 and Fe2O3. The noble metal is selected from Pt, Pd, Rh and Au. The catalytically active material is obtainable by a method comprising the following steps: non-thermal plasma treatment is performed under the condition of the presence of O2. The method includes, for example, the step of subjecting the support comprising a metal oxide and the noble metal on its surface to non-thermal plasma treatment under the condition of the presence of O2. In an alternative, the support comprising a metal oxide is subjected to non-thermal plasma treatment before the noble metal is deposited on the surface of the support.
[0113] By "atomically dispersed", we understand the presence of individual noble metal atoms on the support surface, which can be detected by commonly used analytical techniques, such as extended X-ray absorption fine structure (EXAFS), infrared spectroscopy (IR) or STEM. Analysis using STEM will be further described in the experimental part. For the avoidance of doubt, if not otherwise stated, the term "atom" is used in the specification and claims to cover both neutral (oxidation state = 0) and charged (ionic, e.g. oxidized) noble metal atoms.
[0114] The form of the carrier is not particularly limited. The carrier may be in the form of, for example, particles (eg, powder) or a film.
[0115] The present invention is characterized in that the catalytically active material is obtainable by a method comprising the following steps: performing a non-thermal plasma treatment in the presence of O2.
[0116] In one embodiment, the catalytically active materials of the present invention exhibit a chromatic asymmetry centered at 815 to 845 cm -1 Raman spectroscopy can be performed according to the method described in the examples. Without being bound by theory, the center is between 815 and 845 cm -1 The Raman bands in the range are believed to be due to the surface peroxides (O2 2- ) species.
[0117] In one embodiment, the catalytically active material of the present invention exhibits an additional O1s XPS signal at a binding energy that is 1.2 eV to 2.0 eV, preferably 1.5 eV to 1.7 eV higher than the binding energy of the main signal of oxygen in the metal oxide in the support. XPS analysis can be performed according to the method described in the Examples. The additional XPS signal can be observed as a shoulder of the main signal. Without being bound by theory, the additional XPS signal is believed to be attributed to the surface peroxide groups (O2 2- ) species, preferably surface peroxide species formed on the surface of the metal oxide during the non-thermal plasma treatment. For example, in the case of a CeO2 support, the XPS signal of O1s of the original (untreated with plasma) CeO2 appears at 529.2 eV, while the XPS signal of O1s of the surface peroxide species appears at 530.8 eV.
[0118] In one embodiment, the non-thermal plasma treatment in the presence of O2 results in the formation of metal oxide nanoclusters at the surface of the support. As determined by scanning tunneling microscopy (STM), the average diameter of the metal oxide nanoclusters can be 2.0 nm or less, preferably 1.5 nm or less; see further description below. STM measurements can be performed as described in the Examples.
[0119] In one embodiment, the catalytically active material of the present invention exhibits two or more of the characteristics described in the above embodiments.
[0120] According to the present invention, the support includes a metal oxide at the support surface, and the metal oxide is selected from TiO2, CeO2, ZnO, SnO2, Ga2O3, In2O3, ZrO2 and Fe2O3. These metal oxides are generally referred to as reducible metal oxides. Reducible metal oxides are capable of losing oxygen atoms from their crystal structure at relatively low energy, which results in the formation of oxygen vacancies and a decrease in the oxidation number of metal atoms in the reducible metal oxide, such as from Ce 4+ To Ce 3+ The metal oxide is preferably selected from TiO2, CeO2, SnO2, Ga2O3, In2O3 and Fe2O3, more preferably TiO2, CeO2 and In2O3, and most preferably CeO2.
[0121] Since the support includes a reducible metal oxide, the catalytically active material of the present invention can exhibit excellent catalytic activity and stability, and the CO oxidation reaction can be carried out at a relatively low reaction temperature. Without being bound by theory, it is believed that metal oxide nanoclusters are formed on the support surface after plasma treatment in the presence of O2, and the atomically dispersed noble metal interacts strongly with the metal oxide. It is believed that this interaction allows charge transfer and the presence of oxygen atoms bridging the noble metal and the metal oxide, and excellent stability and excellent catalytic activity can be obtained even at low reaction temperatures.
[0122] Another benefit of using a specific reducible metal oxide (rather than, for example, SiO ) as a carrier is that reducible oxides (such as CeO itself) can also contribute to the catalytic activity in the reaction to be catalyzed, particularly if the reducible metal oxide has been treated with plasma. In a preferred embodiment, CeO clusters are produced during the plasma treatment of CeO carriers, so metal atoms (e.g., Pt atoms) interact with the CeO carriers (when compared with, for example, SiO ) that are also activated. In addition, the data provided in the examples show that even in the absence of noble metals (such as Pt), CeO carriers can also be activated by plasma treatment. This discovery can be attributed to the formation of small CeO clusters with higher surface density, and may also be the formation of peroxide surface species, such as on the formed CeO clusters. These discoveries can be transferred to other reducible metal oxides and noble metals used in the present invention.
[0123] The catalytically active material according to the present invention comprises a noble metal atomically dispersed on the surface of a support, wherein the noble metal is selected from Pt, Pd, Rh and Au. Preferably, the noble metal is selected from Pt and Pd. Further preferably, the noble metal is Pt.
[0124] The combination of metal oxide and noble metal is not particularly limited. According to a preferred embodiment, the metal oxide is selected from TiO2 and CeO2, and the noble metal is selected from Pt and Pd, and the combination of CeO2 and Pt is more preferred.
[0125] The number of noble metal atoms normalized to the surface area of the catalytically active material (surface density, Ns) is not particularly limited, and is preferably at least 3.0×10 12 at / cm 2 , more preferably at least 6.0×10 12 at / cm 2 , more preferably at least 1.2×10 13 at / cm 2 . N S The upper limit is 8.0×10 14 at / cm 2 and can be, for example, 4.0×10 14 at / cm 2 , 2.0×10 14 at / cm 2 , 1.0×10 14 at / cm 2 8.0×10 13 at / cm 2 , 6.0×10 13 at / cm 2 , or 4.0×1013 at / cm 2 Any combination of the above upper and lower limits is an embodiment of the present invention. Therefore, N S It can be, for example, 3.0×10 12 at / cm 2 Up to 8.0×10 14 at / cm 2 , 3.0×10 12 at / cm 2 Up to 4.0×10 14 at / cm 2 , 3.0×10 12 at / cm 2 Up to 2.0×10 14 at / cm 2 , 6.0×10 12 at / cm 2 Up to 8.0×10 14 at / cm 2 , and 6.0×10 12 at / cm 2 Up to 4.0×10 14 at / cm 2 Ns is preferably 3.0×10 12 at / cm 2 Up to 8.0×10 14 at / cm 2 In the range of 3.0×10 12 at / cm 2 Up to 4.0×10 14 at / cm 2 In the range of 6.0×10 12 at / cm 2 Up to 2.0×10 14 at / cm 2 In the examples section, the determination of N is given. S method.
[0126] Preferably, at least a portion of the noble metal has a specific oxidation state X. The specific oxidation state X of the noble metal may be caused by a strong interaction with the metal oxide in the support. When the noble metal is Pt or Pd, the specific oxidation state X is 2+. When the noble metal is Rh or Au, the specific oxidation state X is 3+. As measured by X-ray photoelectron spectroscopy (XPS), the relative intensity of the noble metal having a specific oxidation state relative to the total intensity of the noble metals in all oxidation states is preferably 50% or more, more preferably 75% or more, further preferably 80% or more, and particularly preferably 90% or more. For example, if the noble metal is Pt, relative to Pt 0 , Pt2+ and Pt 4+ (i.e., the total intensity of all oxidation states observed), Pt 2+ The relative intensity of will be determined by the XPS spectrum of Pt 4f. The detailed determination method is given in the Examples section.
[0127] Preferably, the infrared reflection-absorption spectrum (IRAS) measured for the catalytically active material shows a peak at 2085 cm-1 when measured under the following conditions: -1 Up to 2120cm -1 The absorption band in the range of , which does not change when the material is heated from 300K to 500K:
[0128] (1) exposing the catalytically active material in the reaction unit to a reaction mixture consisting of 1% CO and 5% O2 at 1 bar (balanced by Ar),
[0129] (2) heating the catalytically active material to 500 K at a rate of 60 K / min and reacting the mixture at 500 K and 1 bar for 5 min;
[0130] (3) cooling the reaction mixture and catalytically active material to 300K,
[0131] (4) Remove the reaction mixture from the reaction unit and apply 10 -9 The following ultrahigh vacuum (UHV) conditions,
[0132] (5) Spectra were recorded in UHV at 300K without additional exposure to CO,
[0133] (6) increasing the temperature to 500 K at a rate of 60 K / min and recording spectra at 320 K, 360 K, 400 K, 440 K, 480 K, and 500 K, and
[0134] (7) Compare the absorption maxima in the spectra recorded at the respective temperatures.
[0135] For any catalytically active material of the present invention, there is a -1 Up to 2120cm -1 The corresponding absorption band is within the range and can be easily determined by a person skilled in the art. In the case of Pt / CeO2, Fig.10 As shown, the corresponding band (i.e., its absorption maximum) is located at 2110 cm -1 ±1cm -1 Place.
[0136] According to the present invention First embodiment The carrier is present in the form of particles and can be formed into powder, for example. The shape of these particles is not particularly limited and can be selected from ellipsoidal, cubic and spherical.
[0137] According to a first embodiment of the present invention, the average particle size of the carrier is not limited, preferably 10nm to 1μm, more preferably 10nm to 500nm, further preferably 10nm to 100nm, particularly preferably 10nm to 50nm, most preferably 10nm to 30nm. As described in the experimental section, the average particle size of the carrier can be determined by STEM, by measuring the diameter of 20 arbitrarily selected particles and calculating their average value. The longest visible axis of the particle is taken as the "diameter". If the accuracy of the measurement is to be further increased, 100 arbitrarily selected particles can be used for measurement. If several particles form aggregates, the diameter of the primary particle is taken for measurement.
[0138] According to a first embodiment of the present invention, the support is preferably composed of a metal oxide selected from the group consisting of TiO2, CeO2, ZnO, SnO2, Ga2O3, In2O3, ZrO2 and Fe2O3. According to a preferred aspect of the first embodiment of the present invention, the catalytically active material is preferably composed of a metal oxide support and at least partially atomically dispersed noble metals. According to another preferred aspect of the first embodiment of the present invention, the catalytically active material is preferably composed of a metal oxide support and noble metals, wherein more than 50%, more than 75%, more than 80%, or more than 90% of the noble metals are atomically dispersed.
[0139] XPS can be used to measure the percentage of atomically dispersed noble metals. Specifically, as described above, the relative intensity of the noble metal with a particular oxidation state X relative to the total intensity of the noble metal in all oxidation states can be used as a feature indicating the percentage of atomically dispersed noble metals. For example, when the noble metal is Pt, it can be determined based on the Pt 2+ The percentage of atomically dispersed Pt was determined from the relative intensity relative to the total intensity of Pt in all oxidation states. 0 and Pt 4+ can be attributed to metallic Pt and PtO2 clusters, respectively.
[0140] STEM can also be used to measure the percentage of atomically dispersed noble metals. Specifically, 100 STEM images (enlarged to, for example, 10 nm x 10 nm) that clearly show noble metal species (atomically dispersed noble metals and clusters containing more than two noble metals) are randomly selected, and the percentage of atomically dispersed noble metals is determined for each STEM image, and then averaged. In the STEM image, the noble metal species can be brighter than the carrier.
[0141] The percentage of atomically dispersed noble metal is preferably determined by XPS.
[0142] According to the first embodiment of the present invention, the surface density Ns of the noble metal is preferably 3.0×10 12 at / cm 2 Up to 4.0×10 14 , more preferably 3.0×10 12 at / cm 2 Up to 2.0×10 14 at / cm 2 , more preferably 3.0×10 12 at / cm 2 to 1.0×10 14 at / cm 2 , even more preferably 6.0×10 12 at / cm 2 to 1.0×10 14 at / cm 2 .
[0143] According to the present invention Second embodiment , the carrier is in the form of a film. The membrane carrier can be arranged on a substrate (base material). In one embodiment, the substrate provides a planar area on which the membrane carrier can be grown, for example, by growing a metal component of a reducible oxide by vapor deposition on an oxidized surface of the substrate. The substrate is not particularly limited as long as it does not adversely affect the catalytically active material. For example, a substrate made of metal, alloy or ceramic can be used. Examples of metals used as substrates include, but are not limited to, Ru, Cu and Al, etc. The metal used as a substrate can be a single crystal, and examples thereof include Ru (0001) single crystal and Cu (111) single crystal. Examples of alloys used as substrates include, but are not limited to, steel and brass, etc. Examples of ceramics used as substrates include, but are not limited to, aluminum oxide, silicon dioxide (silica) and silicon carbide, etc. Those skilled in the art can select a substrate suitable for the reaction conditions to which the catalytically active material is exposed.
[0144] According to a second example of the present invention, the thickness of the film carrier is not particularly limited, preferably 5nm to 50nm, more preferably 10nm to 20nm. For example, the thickness of the metal oxide film can be determined by XPS by measuring the attenuation of the XPS signal of the substrate on which the metal oxide film is provided. For example, if the metal oxide film is arranged on a Ru substrate, the attenuation of the Ru 3d signal in the XPS energy spectrum can be measured to determine the thickness of the metal oxide film carrier. Similarly, if a Cu substrate is used, the attenuation of the Cu 2p signal in the XPS energy spectrum can be measured. Similarly, if a steel substrate is used, the attenuation of the Fe 2p signal in the XPS energy spectrum can be measured. Those skilled in the art can appropriately select the signal generated by the element in the substrate and measure its attenuation to determine the thickness of the metal oxide film. The detailed information of the measuring method is given in the embodiment section.
[0145] According to the second embodiment of the present invention, the surface density Ns of the noble metal is preferably 3.0×10 12 at / cm 2 Up to 4.0×10 14 at / cm 2 , more preferably 6.0×10 12 at / cm 2 Up to 4.0×10 14 at / cm 2 , more preferably 1.2×10 13 at / cm 2 Up to 2.0×10 14 at / cm 2 .
[0146] According to a second embodiment of the present invention, the carrier may be composed of a substrate and a cluster supported on the substrate, the substrate and the cluster comprising the same metal oxide. Preferably, the substrate and the cluster are composed of the same metal oxide group. The average diameter of the cluster may be less than 2.0 nm, preferably less than 1.5 nm, as determined by STM according to the following items: by drawing a profile curve along a straight line corresponding to a length of 10 nm; measuring the distance between two adjacent minima; multiplying the measured value by a correction factor of 0.5 and recording the obtained value as the diameter; repeating the measurement for 20 arbitrarily selected surface areas showing coverage by metal oxide clusters; and calculating the average value. The detailed method is given in the Examples section.
[0147] The number of metal oxide clusters on the metal oxide substrate and the number normalized to the surface area of the metal oxide substrate (surface cluster density) are not particularly limited. The surface cluster density is preferably at least 0.05 clusters / nm 2 , more preferably at least 0.08 clusters / nm 2 , more preferably at least 0.10 clusters / nm2 , and most preferably at least 0.12 clusters / nm 2 The surface cluster density can be determined by STM by counting the number of metal oxide clusters present in an arbitrarily selected area. The detailed method is given in the Examples section.
[0148] According to a preferred aspect of the second embodiment of the present invention, the catalytically active material preferably includes a noble metal, for example more than 50%, more than 75%, more than 80%, or more than 90% of the noble metal is atomically dispersed. The percentage of atomically dispersed noble metal can be determined as described above for the first embodiment.
[0149] The catalytically active materials of the present invention are particularly suitable for the oxidation of CO and the selective hydrogenation of alkynes (eg, acetylene hydrogenation). The catalytically active materials of the present invention may also be suitable for other catalytic reactions, including, for example, water-gas shift reactions, steam reforming, and the oxidation of natural gas.
[0150] The catalytically active materials of the present invention exhibit excellent stability and activity, which is also reflected by suitably low initial reaction temperatures in target reactions such as CO oxidation and selective alkyne hydrogenation. These properties appear to be related, at least in part, to the atomic dispersion of the noble metal on the surface of the metal oxide clusters. Available experimental evidence further suggests that this atomic dispersion and / or the noble metal loading (measured in at / cm 2 The uniformity of the catalytically active material can be improved by the inventive method for producing the catalytically active material as described below.
[0151] II. Method for producing catalytically active materials
[0152] The method for producing a catalytically active material according to a first embodiment of the present invention may comprise the following steps:
[0153] (1) Providing a precursor for a catalytically active material, the catalytically active material comprising
[0154] a support in particulate form comprising a metal oxide, and
[0155] The precious metal on the surface of the carrier,
[0156] (2) calcining a precursor for a catalytically active material in the presence of O2, and
[0157] (3) Non-thermal plasma treatment of a calcined precursor for a catalytically active material in the presence of O2.
[0158] At the end of step (1), the noble metal may be present on the surface of the support in elemental form (oxidation state = 0) or as a noble metal compound (e.g. a noble metal salt). The method for providing the precursor of the catalytically active material is not particularly limited, and step (1) is preferably selected from the following steps (1a) and (1b):
[0159] (1a) depositing a noble metal onto a support, and
[0160] (1b) Co-precipitating a noble metal and a metal oxide from an aqueous solution containing a salt of the noble metal and the metal oxide.
[0161] The method for depositing the noble metal onto the support according to step (1a) is not particularly limited, and examples thereof include physical vapor deposition, chemical vapor deposition, and deposition from an aqueous solution of a noble metal salt. Preferably, the noble metal is deposited onto the support from an aqueous solution of a noble metal salt, and known methods such as strong electrostatic adsorption (SEA) and impregnation may be appropriately used. Deposition is preferably performed so that the noble metal deposition can be controlled according to the surface density of metal atoms on the support. In step (1a), the support is preferably composed of a metal oxide.
[0162] The salt of the noble metal is not particularly limited. Examples of the salt of the noble metal include, but are not limited to, tetraamine platinum (II) nitrate, tetraamine platinum (II) chloride, platinum (II) acetylacetonate, tetraamine palladium (II) nitrate, tetraamine palladium (II) chloride, rhodium (III) acetylacetonate, tetrachloroaurate hydrogen (III), gold (III) chloride, to name a few.
[0163] As used herein, the term "calcining" or "calcination" refers to the thermal treatment of a solid under dry conditions, in the presence of O2, at elevated temperatures. As used herein, the phrase "dry" means that no additional water is introduced into the atmosphere in which the calcination is performed. For example, calcination in air is understood to be performed under dry conditions.
[0164] The calcination of the precursor for the catalytically active material is preferably carried out at a temperature of 573 K to 973 K, more preferably at 623 K to 873 K, and further preferably at 673 K to 823 K. The calcination is preferably carried out under conditions where the O2 concentration is 5% by volume or more, more preferably 10% by volume or more. For example, air can be used as a source of O2.
[0165] The calcined precursor for the catalytically active material is subjected to a non-thermal plasma treatment in the presence of O2. Prior to ignition of the plasma, the pressure is preferably reduced to below 40 mbar, more preferably below 20 mbar. The pressure during the non-thermal plasma treatment is preferably below 40 mbar, more preferably below 20 mbar. The non-thermal plasma treatment is preferably carried out in an inert gas at an O2 concentration of 5% by volume or more, more preferably of 80% or more, more preferably of 100% (pure oxygen). The inert gas may be selected from N2, He, Ne and Ar, among others.
[0166] The non-thermal plasma treatment can be carried out in a static atmosphere or under a gas flow, the latter being preferred. When the non-thermal plasma treatment is carried out under a gas flow, it is preferred that the calcined precursor for the catalytically active material is blown (suspended) by the gas flow during the non-thermal plasma treatment.
[0167] The source of non-thermal plasma is not limited, and examples include inductively coupled plasma, capacitively coupled plasma, DC glow discharge, microwave plasma, radio frequency plasma, cold plasma jet, and dielectric barrier discharge plasma. The source of non-thermal plasma is preferably microwave plasma or radio frequency plasma.
[0168] When the source of the non-thermal plasma is microwave plasma, the anode voltage of the plasma source is preferably 0.2 kV to 2 kV, and the emission current is preferably 0.1 μA to 1 μA.
[0169] When the source of the non-thermal plasma is radio frequency plasma, the power of the radio frequency plasma generator is preferably 20W to 300W.
[0170] The duration of the non-thermal plasma treatment can be appropriately adjusted as required, and is generally 1 to 300 minutes, preferably 5 to 180 minutes, more preferably 10 to 120 minutes, and further preferably 30 to 90 minutes.
[0171] The method for producing a catalytically active material according to the second embodiment of the present invention may be selected from the following method A and method B.
[0172] Method A comprises the following steps:
[0173] (1) providing a metal oxide film support,
[0174] (2) performing a non-thermal plasma treatment in the presence of O2 to obtain a plasma-treated metal oxide film support, and
[0175] (3) Depositing the noble metal onto the plasma-treated metal oxide film support in the gas phase, preferably by physical vapor deposition of the noble metal atoms.
[0176] Method B comprises the following steps:
[0177] (1) providing a metal oxide film support,
[0178] (2) depositing a noble metal onto a metal oxide film support from a solution containing the noble metal, and
[0179] (3) Non-thermal plasma treatment in the presence of O2.
[0180] The method for providing the metal oxide film support is not particularly limited, and any method available in the art can be used. The method for providing the metal oxide film may include molecular beam epitaxy, laser ablation, chemical vapor deposition, and sol-gel methods, etc. In one embodiment, the metal oxide film is provided on a substrate, as explained above in conjunction with the second embodiment of the present invention.
[0181] In step (2) of method A and step (3) of method B, the non-thermal plasma treatment is carried out in the presence of O2. The non-thermal plasma treatment is preferably carried out at 1×10 -6 mbar to 1×10 -2 mbar, more preferably 1×10 -6 mbar to 1×10 -4 , more preferably 1×10 -6 mbar to 1×10 -5 During the non-thermal plasma treatment, the partial pressure of O2 is preferably 1×10 -6 mbar to 1×10 -2 , more preferably 1×10 -6 mbar to 1×10 -4 mbar, more preferably 1×10 - 6 mbar to 1×10 -5 In one embodiment, the non-thermal plasma treatment is preferably carried out in 100% O2 at the above pressures.
[0182] Non-thermal plasma treatment can be performed in a static atmosphere or under a gas flow.
[0183] The source of the non-thermal plasma is not particularly limited, and examples include inductively coupled plasma, capacitively coupled plasma, DC glow discharge, microwave plasma, radio frequency plasma, cold plasma jet, and dielectric barrier discharge plasma. The source of the non-thermal plasma is preferably microwave plasma or radio frequency plasma.
[0184] When the source of the non-thermal plasma is microwave plasma, the anode voltage of the plasma source is preferably 0.2 kV to 2.0 kV, more preferably 0.5 kV to 1.5 kV, and the emission current is preferably 0.1 μA to 1.0 μA.
[0185] When the source of the non-thermal plasma is radio frequency plasma, the power of the radio frequency plasma generator is preferably 20W to 300W.
[0186] The duration of the non-thermal plasma treatment can be appropriately adjusted as required, and is generally 1 to 300 minutes, preferably 5 to 180 minutes, more preferably 10 to 120 minutes, and further preferably 30 to 90 minutes.
[0187] According to step (3) of method A, the method for depositing the noble metal on the plasma-treated metal oxide film support in the gas phase is not particularly limited, and examples thereof include physical vapor deposition and chemical vapor deposition, with physical vapor deposition being preferred. According to step (2) of method B, the method for depositing the noble metal on the plasma-treated metal oxide film from a solution containing the noble metal is not particularly limited, and examples thereof include deposition from an aqueous solution of a noble metal salt as a precursor. When the noble metal is deposited from an aqueous solution, the method and materials described in the method for producing a catalytically active material according to the first embodiment of the present invention can be applied.
[0188] According to the method described herein, it can be assumed that all the deposited noble metal is present on the surface of the metal oxide support and the metal oxide clusters. Therefore, a high catalytic activity of the catalytically active material can be obtained using a small amount of noble metal.
[0189] III. Catalytic oxidation of CO
[0190] The catalytically active material of the present invention can be suitably used for the catalytic oxidation of CO to CO 2 (also referred to as catalytic oxidation).
[0191] In the catalytic oxidation of CO to CO2, a reaction gas mixture including CO and O2 reacts in the presence of a catalytically active material to generate CO2. The pressure of the reaction gas mixture is not particularly limited and may be 0.8 bar to 2.0 bar, preferably 0.8 bar to 1.5 bar, more preferably 0.9 bar to 1.2 bar.
[0192] The reaction temperature for catalytic oxidation is not particularly limited, and may be 323K to 573K, preferably 353K to 523K, more preferably 353K to 473K.
[0193] The composition of the reaction gas mixture is not particularly limited as long as it includes CO and O2. The CO content in the reaction gas mixture may be, for example, 5% by volume or less, preferably 3% by volume or less, and more preferably 2% by volume or less. The O2 content in the reaction gas mixture may be 2% by volume or more and 25% by volume or less, preferably 5% by volume or more and 20% by volume or less. The molar ratio CO / O2 of the reaction gas mixture is preferably 2.0 or less, more preferably 1.0 or less, further preferably 0.5 or less, and most preferably 0.2 or less.
[0194] IV. Catalytic Hydrogenation of Alkynes
[0195] The catalytically active material of the present invention can be suitably used for catalytic hydrogenation of alkynes to olefins (also referred to as "catalytic hydrogenation"). The alkynes used in the catalytic hydrogenation are preferably C2-C5 alkynes, more preferably C2-C3 alkynes.
[0196] In the catalytic hydrogenation of alkynes to alkenes, a reaction gas mixture comprising alkynes and H2 reacts in the gas phase in the presence of a catalytically active material to produce alkenes. For example, when acetylene (acetylene) is used as the alkyne, ethylene (ethylene) is produced as the product (olefin).
[0197] The pressure of the reaction gas mixture is not particularly limited, and may be 0.8 bar to 2.0 bar, preferably 0.8 bar to 1.5 bar, more preferably 0.9 bar to 1.2 bar.
[0198] The reaction temperature of the catalytic hydrogenation is not particularly limited, and may be 323K to 573K, preferably 323K to 523K, and more preferably 353K to 473K.
[0199] The composition of the reaction gas mixture is not particularly limited as long as it includes alkynes and H2. The content of alkynes in the reaction gas mixture may be, for example, 10% by volume or less, preferably 5% by volume or less, and more preferably 3% by volume or less. For example, the content of H2 in the reaction gas mixture may be 3% by volume or more, 5% by volume or more, and 10% by volume or more. The molar ratio H2 / alkyne is preferably 1.0 or more, more preferably 2.0 or more.
[0200] Example
[0201] Hereinafter, the present invention will be described in more detail with reference to Examples. However, the present invention is not limited to the following Examples.
[0202] Analytical methods
[0203] Scanning tunneling microscopy (STM) analysis - average diameter and number of metal oxide clusters; and low energy electron diffraction Low-energy electron diffraction analysis (LEED) - Surface order in membrane supports
[0204] The STM measurements were performed at a sample voltage of 3.8 V and a constant tunneling current of 30 pA.
[0205] In order to determine the Average diameter , a profile curve was drawn along a straight line corresponding to a length of 10 nm. In the profile curve, the distance between two adjacent minima was measured, and the measured value was multiplied by a correction factor of 0.5 to correct for the tip / cluster convolution effect. The corrected value obtained was recorded as the diameter. The diameter was measured for 20 arbitrarily selected metal oxide clusters, and the average value was calculated.
[0206] In order to determine the surface density of metal oxide clusters in the recorded STM images, i.e. the number of metal oxide clusters normalized to the surface area of the metal oxide substrate, the number of metal oxide clusters in an arbitrarily selected 100 nm × 100 nm area was counted. This measurement was repeated in four different sample points, i.e., measurements were performed in a total of five different sample points. The average value was taken as the "density of metal oxide clusters".
[0207] Low energy electron diffraction (LEED) analysis was performed on the same instrument and a LEED pattern was recorded at 81 eV.
[0208] Scanning transmission electron microscopy (STEM) analysis - average diameter of metal oxide particles in powder
[0209] STEM images were recorded on a JEOL JEM ARM200F probe / image correction TEM (JEOL Ltd) at 200 kV.
[0210] The average diameter of the metal oxide particles (e.g., CeO2 particles) of the metal oxide powder support was determined by measuring the diameters of 20 randomly selected particles and calculating the average thereof. In the case where the STEM image showed a non-spherical shape for the selected particles, the longest axis was taken as the diameter.
[0211] X-ray Photoelectron Spectroscopy (XPS) - Elemental composition in catalytically active materials (films) and chemical analysis of elements at the surface Chemical (oxidation) state
[0212] The relative intensity of a noble metal having a specific oxidation state (X) relative to the total intensity of noble metals in all oxidation states is measured by XPS. In the case where the noble metal is Pt, the specific oxidation state is 2+. In addition, in the case where the catalytically active material is a membrane, the number of noble metals per unit surface area of the catalytically active material, N, is measured by XPS. S (at / cm 2). XPS spectra were measured using a Phoibos 150 analyzer (SPECS Ltd.) using an Al Kα X-ray source (hν = 1486.6 eV). Spectral analysis (background subtraction and deconvolution) was performed using CasaXPS software (commercially available from Casa Software LLC; version 2.3.18), and the measured spectra were subjected to background subtraction using a Shirley background. In the case of Pt / CeO2 film samples, core level spectra of Pt 4f, Ce 3d, and O1s were recorded at pass energies of 25 eV, 50 eV, and 50 eV, respectively. The technician is able to select the core level of the target element and attribute the binding energy to the oxidation state by using common knowledge. For example, binding energy lists (such as the NIST X-ray Photoelectron Spectroscopy Database) are common knowledge to those skilled in the art.
[0213] The Pt spectrum was deconvoluted using CasaXPS software. Background subtraction was performed in the range of 68 eV to 80 eV for each Pt spectrum. The spectrum was deconvoluted using Gaussian / Lorentzian lineshapes. The maximum value of the full-width half maximum (FWHM) of each peak was set to 2.0 eV. 2+ The relative intensity of the peak at 72.6 eV is calculated relative to the Pt 4f 7 / 2 The signal is expressed as a percentage of the total peak area.
[0214] Measurement of Metal Oxide Film Thickness
[0215] The thickness of the metal oxide film prepared on the substrate (e.g., CeO2 film) deposited on Ru(0001) single crystal was determined by XPS based on the attenuation of the most intense signal from the substrate (e.g., Ru 3D signal) compared to the signal of the substrate before deposition of the CeO2 film.
[0216] Raman spectroscopy - identification of surface peroxide species
[0217] Raman spectroscopy is a technique used in TM Raman microscopy was performed on a Renishaw microscope with a 532 nm excitation laser. For each sample, measurements were performed at five different sample points. Three scans were collected at each sample point and the average value was recorded. The acquisition time for each scan was 20 seconds. The spectra were normalized to the main peak of the carrier (e.g. 465 cm for CeO2). -1 F 2g Peak). The normalized spectra recorded at five different sample points were averaged.
[0218] N2 physical adsorption analysis (BET specific surface area)
[0219] The specific surface area of the catalytically active material in particle form (powder) was determined by the BET method based on the N2 adsorption isotherm. The N2 physical adsorption measurements were carried out on an ASAP 2020PLUS (Micromeritics Instrument Corporation).
[0220] The number of noble metal atoms (N) normalized to the surface area of the catalytically active material (particle) S ), unit is at / cm 2
[0221] For catalytically active materials in particle form, the surface density of single atoms (ie, the number of noble metal atoms normalized to the surface area of the catalytically active material (N S )) is based on the specific surface area (m 2 / g to cm 2 The amount is calculated from the amount of noble metal present in the aqueous solution (g / g) and the amount (g converted to at). If the noble metal is deposited by an impregnation technique, the total amount of noble metal atoms present in the aqueous solution (in g) can be used for the calculation if the deposition is quantitative. Otherwise, the amount depends on the yield achieved.
[0222] Calculation of O 1s binding energy
[0223] The binding energy of the O1s level at the surface is calculated by density functional theory (DFT) in the final state approximation and with reference to the O1s signal oxygen in the bulk (2×2×2) supercell of ceria. Details on DFT are given in the following sections.
[0224] Targeting CO oxidation reactions on catalytically active materials in membrane form
[0225] The reactivity measurements were performed in a high pressure cell (SPECS HPC 20) connected to the main UHV analysis chamber. The catalytically active material was heated through a quartz window by a halogen lamp outside the chamber. The reaction mixture consisted of 10 mbar CO, 50 mbar O2 and was balanced to 1 bar by He. The gas composition in the reactor was analyzed by gas leakage through a quartz microcapillary into a quadrupole mass spectrometer (QMS, MKS Instruments). Starting from room temperature, the temperature of the catalytically active material was gradually increased in increments of 50 K and the production of CO2 was monitored with the QMS. In experiments aimed at testing the stability of atomically dispersed noble metals in the catalytically active material in CO oxidation reactions, the sample was heated to 523 K at a rate of 1 K / S and kept under reaction conditions for 10 min, after which the sample was cooled to 300 K and evacuated before being transferred to the analysis chamber for post-characterization.
[0226] Infrared reflection-absorption spectroscopy (IRAS)
[0227] IRAS measurements on catalytically active materials in film form were performed using a Bruker 66ivs FTIR spectrometer in a UHV chamber (reaction volume 1 L) with a "high pressure" cell for exposing the sample to a gas mixture at near atmospheric pressure.
[0228] The IRAS spectra of CO adsorption were measured by following the following steps:
[0229] (1) Cooling the catalytically active material to 200K under UHV,
[0230] (2) Inject CO into 10 -6 mbar for 100 s, and then pump CO out to 10 -9 Below mbar,
[0231] (3) Recording IRAS spectra
[0232] (4) heating the catalytically active material to 500 K at 60 K / min in UHV and cooling to 200 K, and
[0233] (5) Repeat steps (2) to (4) twice.
[0234] IRAS measurements were also performed on the catalytically active material after exposure to a 1 bar reaction mixture consisting of 1% CO and 5% O2, balanced by Ar.
[0235] The measurement is performed as follows:
[0236] (1) exposing the catalytically active material in the reaction unit to a reaction mixture,
[0237] (2) heating the catalytically active material to 500 K at a rate of 60 K / min and reacting at 500 K for 5 min,
[0238] (3) Cooling the catalytically active material to 300K,
[0239] (4) Remove the reaction mixture from the reaction unit and apply 10 -9 UHV conditions below mbar,
[0240] (5) Spectra were recorded at 300K under UHV without additional exposure to CO,
[0241] (6) The temperature of the catalytically active material was increased to 500 K at a heating rate of 60 K / min and spectra were recorded at 320 K, 360 K, 400 K, 440 K, 480 K and 500 K.
[0242] CO oxidation on granular catalytically active materials
[0243] The reactivity of the catalytically active material (powder) in the CO oxidation reaction was measured in a tubular packed bed reactor. The gas phase composition was analyzed by QMS (Hiden 20). The catalytically active material was screened to less than 75 μm and 1 part by mass of the catalytically active material was physically mixed with 4 parts by mass of silica gel. The resulting mixture (5 parts by mass) was then mechanically mixed with 1 part by mass of acid-purified SiO2 and loaded into a glass tube reactor. The CO oxidation reaction rate was measured at steady state, in a mixture of 1% CO and 20% O2 (He balance) at 1 bar, at temperatures (stepwise increase) of 373K, 383K, 403K, 423K, 443K and 473K, for at least 1 h at each temperature.
[0244] Hydrogenation of alkynes on granular catalytically active materials
[0245] The reactivity of the catalytically active material in the form of particles (powder) in the hydrogenation of alkynes was measured in a tubular packed bed reactor, using acetylene as the alkyne. The gas phase composition was analyzed by QMS (Hiden 20). The catalytically active material was sieved to less than 75 μm and loaded into a glass tube reactor without dilution. The rate of hydrogenation of alkynes was measured at steady state, in a mixture of 1% C2H2 and 5% H2 (Ar balance) at 1 bar, at temperatures (increased stepwise) of 373, 393, 413, 433, 453 and 473 K, and hydrogenated for 12 h at each temperature. The average ethylene production rate observed during the hydrogenation reaction (lasting 12 h at each temperature) was recorded as the hydrogenation rate of acetylene.
[0246] Pt / CeO2 film samples
[0247] Reference Example 1: Preparation of CeO2(111) membrane carrier
[0248] The experiments were performed in an ultrahigh vacuum (UHV) chamber equipped with low energy electron diffraction (LEED), X-ray photoelectron spectroscopy (XPS) and scanning tunneling microscopy (STM), all from SPECS Ltd. Stoichiometric ordered CeO2(111) films were grown on Ru(0001) single crystals. The Ru(0001) single crystals (9 mm diameter, 1.5 mm thickness, from MaTeck Ltd.) were mounted on a stainless steel sample holder with a 9 mm diameter hole to heat the sample from the back using an electron beam from a W filament. A K-type thermocouple was spot welded to the edge of the crystal. The surface of the Ru(0001) was heated at 1000 K, 10 -6The precipitate was oxidized in 10 mbar of O2 using an electron beam assisted evaporator (Focus EMT3) at 90 K. -6 Ce was vapor deposited onto the oxidized Ru(0001) surface from a Mo crucible filled with Ce (99.9%, Sigma Aldrich) in an amount corresponding to the formation of 4 to 5 monolayers (ML) of CeO2(111) in mbar O2. Subsequently, the temperature of Ru(0001) was increased at a rate of 1 K / s and maintained at 673 K during the deposition of further CeO2 layers. The sample was then heated at 1000 K, 10 -6 The thickness of the prepared CeO2(111) film was about 5 nm. The prepared sample was denoted as "CeO2(111)".
[0249] Reference Example 2: Preparation of CeO2-red membrane carrier
[0250] The reduced CeO was prepared by UHV annealing of CeO2(111) film at 1200K for 5 min. 2-x (111) surface (hereafter referred to as “CeO2-red”).
[0251] Reference Example 3: Preparation of CeO2-ladder membrane carrier
[0252] A CeO2(111) surface rich in monoatomic steps (denoted as “CeO2-steps”) was prepared according to the procedures described in detail in Nat. Commun. 7 (2016) 10801.
[0253] In particular, it was obtained by depositing 0.3 monolayer (ML) of Ce on a CeO2(111) film and subsequently oxidizing it at 673 K. This resulted in the formation of small ML-high islands. This homoepitaxy of CeO2 on CeO2 produced sharply aligned samples with a high step density.
[0254] Reference Example 4: Preparation of CeO2-plasma film carrier
[0255] The CeO2(111) film was treated with oxygen plasma using a microwave plasma generator with a temperature of 7×10 -6 A commercial plasma source (Osprey, from Oxford Scientific, Figure 1 A), the anode voltage was 1 kV, and the emission current was 0.5 μA. The prepared sample is called "CeO2-plasma".
[0256] Example 1: Preparation of Pt / CeO2-plasma film samples
[0257] Pt was deposited onto the CeO2-plasma film from a Pt rod using an electron beam assisted evaporator (Omicron EMT3). To reduce metal aggregation during deposition at room temperature, Pt was intentionally deposited at a low metal flux, i.e., 0.03 ML / min as determined by a quartz microbalance (McVac), where 1.0 ML of Pt corresponds to one Pt atom per CeO2(111) surface unit cell, i.e., 7.9×10 14 Pt atoms / cm 2 During deposition, the sample was biased at the same potential as the Pt rod. The amount of Pt was controlled to be 0.20 ML by XPS through analysis of the Pt 4f signal intensity. The resulting sample was denoted as "Pt / CeO2-plasma".
[0258] UHV annealing was then applied to the resulting "Pt / CeO2-plasma" sample. The sample was exposed to UHV, heated to 523K at a ramp rate of 120K / min, and kept at 523K in UHV for 5min, then cooled at a cooling rate of 60K / min. The resulting sample is denoted as "annealed-Pt / CeO2-plasma".
[0259] The obtained annealed -Pt / CeO2-plasma film catalyst exhibited the following characteristics. The average diameter of CeO2 clusters measured by STM was about 1.0 nm. The number of Pt atoms on the sample surface (surface density, Ns) was 1.6×10 14 at / cm 2 As measured by XPS, Pt 2+ Relative to Pt in catalytically active materials 0 , Pt 2+ and Pt 4+ The relative intensity of the total intensity is 100%. The number of CeO2 clusters normalized to the surface area of the CeO2 substrate was 0.15 clusters / nm by STM measurement. 2 .
[0260] Comparative Example 1: Preparation of Pt / CeO2(111) film sample
[0261] Pt was deposited on the CeO2(111) film prepared in Reference Example 1 in the same manner as in Example 1. The resulting sample was denoted as "Pt / CeO2(111)". UHV annealing was applied to Pt / CeO2(111) in the same manner as in Example 1. The resulting sample was denoted as "Annealed-Pt / CeO2(111)".
[0262] Comparative Example 2: Preparation of Pt / CeO2-red film sample
[0263] In the same manner as described in Example 1, Pt was deposited onto the CeO2-red film prepared in Reference Example 1. The resulting sample was denoted as "Pt / CeO2-red". In the same manner as described in Example 1, UHV annealing was applied to Pt / CeO2(111). The resulting sample was denoted as "Annealed-Pt / CeO2-red".
[0264] Comparative Example 3: Preparation of Pt / CeO2 step film sample
[0265] In the same manner as described in Example 1, Pt was deposited onto the CeO2-step film prepared in Reference Example 1. The resulting sample was denoted as "Pt / CeO2-step". In the same manner as described in Example 1, UHV annealing was applied to Pt / CeO2(111). The resulting sample was denoted as "annealed-Pt / CeO2-step".
[0266] Comparative Example 4: Preparation of Pt / CeO2 sputtered film samples
[0267] First, a CeO2 (111) support was prepared in the same manner as described in Reference Example 1. Then, the support was heated at 300K with 1 keV Ar + The CeO2(111) film was ion bombarded for 5 min to roughen its surface. Due to the preferential sputtering of the lighter O atoms, the surface was significantly reduced as determined by XPS. To reoxidize the ceria surface, the film was exposed to 10 -6 mbar of O2. The support thus produced is called "CeO2-sputtered".
[0268] Subsequently, 0.2 ML of Pt was deposited on this "CeO2-sputtered" support in the same manner as described in Example 1. The resulting sample was denoted "Pt / CeO2-sputtered". In the same manner as in Example 1, UHV annealing was applied to Pt / CeO2(111). The resulting sample was denoted "Annealed Pt / CeO2-sputtered".
[0269] Evaluation of results
[0270] The results obtained for the membrane samples are discussed below.
[0271] Figure 2The XPS spectra of Pt4f obtained for the (annealed) Pt / CeO2 samples of Example 1 and Comparative Examples 1-3 are shown, and the XPS spectra of Pt4f before and after the CO oxidation reaction described above in a reaction mixture consisting of 10 mbar CO and 50 mbar O2 (balanced to 1 bar by He) at 523 K are measured. All samples before the reaction were annealed in UHV at 523 K in order to distinguish between thermal effects and reaction-induced effects. Figures 3 to 6 A complete XPS data set of Pt 4f, Ce 3d, and O1s levels is shown.
[0272] First, the results of Comparative Example 1 are discussed. Upon deposition, the Pt species in Pt / CeO2(111) is characterized by a binding energy (BE) of 71.8 eV, indicating the formation of small Pt metal clusters ( Figure 3 ). The peak shift to a lower BE (71.4 eV) in the annealed -Pt / CeO2(111) sample indicates the sintering of Pt metal clusters during UHV annealing. The spectrum obtained after CO oxidation reaction consists of several valence states determined by deconvolution. The 71.1 eV valence state is associated with larger metal nanoparticles (NPs), indicating further Pt sintering under the reaction conditions. The other two signals centered at 74.2 eV and 72.7 eV, respectively, are assigned to Pt in 4+ and 2+ oxidation states.
[0273] XPS spectra of Ce 3d and O1s measured for the CeO2(111) support according to Reference Example 1 and the Pt / CeO2(111) sample according to Comparative Example 1 ( Figure 3 ) showed no significant difference before and after Pt deposition measured at 300 K. Compared with Pt / CeO2(111), the Ce content in the annealed Pt / CeO2(111) sample 3+ The relative content of CeO2(111) increases slightly, indicating that Pt induces partial ceria reduction upon UHV annealing at 523 K. After CO oxidation in an O-rich atmosphere, the Ce 3d spectrum is fully restored. The O1s signal at 529.3 eV indicates that there are no additional valence states associated with adsorbates (typically hydroxyls and carbonates) before and after Pt deposition, i.e., in the CeO2(111) support and Pt / CeO2(111) samples, because the stoichiometric CeO2(111) surface is essentially inert to residual gases in the UHV background at 300 K. However, after CO oxidation, a considerable signal appears at 531.8 eV, which can be attributed to the adsorption of exogenous CO2 (and possibly water) on the bare ceria support at "high" pressure.
[0274] like Figure 2 As shown in Figure 2, the surface of the CeO2-red film support of Reference Example 2 exhibits a complex (√7×√7)-R19.1° LEED pattern, which is assigned to the long-range ordering of O vacancies at the surface. Unlike the stoichiometric CeO2(111) support of Reference Example 1, this surface readily reacts with trace amounts of water in the UHV background, resulting in an additional weak O1s signal from the surface hydroxyl groups at 532.0 eV ( Figure 4 ). In the Pt / CeO2-red sample of Comparative Example 2, outside the Pt metal atoms constituting the small clusters (BE at 71.6 eV), some Pt atoms are in the 2+ oxidation state (at 72.8 eV). However, in the annealed-Pt / CeO2-red sample, the Pt 2+ The signal disappears at UHV, while Pt 0 The signal increases in intensity compared to Pt / CeO2-red, so that the spectrum becomes almost identical to that observed on stoichiometric CeO2 surfaces ( Figure 2 ). After CO oxidation, the Pt in the annealed -Pt / CeO2-red sample is almost exclusively in the Pt 2+ state (72.8eV), contributing a small amount of Pt 4+ (74.2eV), and Pt 0 The state shifted to 71.1 eV. Again, this result can be explained by the formation of relatively large Pt nanoparticles after oxidation. At the same time, since an O2-rich mixture was used in the CO oxidation reaction, the ceria surface became completely oxidized (no Ce was detected). 3+ )( Figure 4 ).
[0275] Turning to Comparative Example 3, in the Pt / CeO2-step sample, the Pt atoms are partially in the 2+ and metallic states (BE is 72.8 eV and 71.9 eV, respectively, see Figure 5 ). Different from Comparative Example 1, after UHV annealing, in the annealed Pt / CeO2-step sample, Pt 2+ The species are thermally stable and remain on the surface except for small metal clusters that sinter during annealing (corresponding to a BE shift from 71.9 eV to 71.7 eV). After CO oxidation, no metallic Pt atoms were found on the surface, only Pt 2+ and Pt 4+ Species.
[0276] As shown above, in Comparative Examples 1-3, Pt deposition always forms Pt nanoparticles upon UHV annealing. A certain amount of thermally stable Pt was found in the annealed -Pt / CeO2-stepped samples. 2+The species can be explained by the strong adsorption of Pt single atoms at the step edges. When exposed to CO oxidizing atmosphere, the metal clusters are oxidized, resulting in 4+ and 2+ states, although their ratio depends on the size of the initial particles. In oxidizing atmosphere, it has been documented that Pt 4+ and Pt 2+ The formation of the species is usually attributed to PtO2 / PtO clusters or thin PtOx oxide films on large Pt nanoparticles.
[0277] at last, Figure 2 The LEED pattern obtained for the CeO2-plasma film support according to Reference Example 4 is shown. This sample is substantially different from the samples of Reference Examples 1-3, as no long-range order is observed. From the XPS spectrum of the Pt 4f of the Pt / CeO2-plasma sample, it can be seen that, starting from the "deposited" sample, even in the CO oxidation reaction at near atmospheric pressure, the Pt / CeO2 exists only in the 2+ state ( Figure 2 and Figure 6 ).
[0278] In order to clarify the reason for the excellent stability of Pt on the annealed-CeO2 plasma surface, the film morphology was studied by STM. STM images ( Figure 7 b to Figure 7 c) shows that the formation of CeO2 clusters with a diameter of about 1.0 nm is randomly distributed on the surface of the CeO2-plasma carrier of Reference Example 4, so that the initial film morphology showing terraces separated by monoatomic steps can still be recognized. Figure 7 Such CeO2 clusters were not observed in the CeO2(111) support of a). The STM results also explain the lack of long-range order observed by LEED (see Figure 2 ).
[0279] Importantly, CeO2-plasma carrier and Pt / CeO2-plasma samples ( Figure 7 The XPS spectrum of O1s in e) shows a prominent shoulder at 530.8 eV, which cannot be attributed to exogenous hydroxyl groups and / or carbonates, and shows a relatively high BE of about 531.8 eV ( Figures 3 to 5). The signal is shifted by 1.6 eV relative to the main peak at 529.2 eV and increases with increasing plasma exposure time. In addition, the intensity of the signal increases when measured under glancing emission, to which the surface is more sensitive. All these findings indicate the formation of new oxygen species that are not present on the other CeO2 film supports used in Comparative Examples 1-3. DFT calculations based on stoichiometric atomic O adsorption on CeO2 (111) surfaces and the corresponding BE shift of the O1s energy level ( Figure 7 f, see below), the signal at 530.8 eV is assigned to the surface peroxide O2 2- ( Figures 8 to 9 ). Table 1 lists the PBE+U core-level binding energies (in eV) of oxygen species on the CeO2 surface for different peroxide coverages. The values given correspond to average results, since in each case all oxygen atoms located in the surface layer are sampled. The values are always referred to the simulated O1s signal of oxygen atoms in a (2 × 2 × 2) supercell of the ceria bulk phase. For 0.5 ML, two different geometric arrangements of the peroxide groups are possible (in Fig. 9 In the example above, the diagonal direction is represented as “diag” and “row”).
[0280] [Table 1]
[0281]
[0282] IRA spectroscopy was used to identify the Pt species formed on the CeO2-plasma film using CO as a probe molecule. The CO IRAS results of the (annealed) Pt / CeO2-plasma sample of Example 1 and the (annealed) Pt / CeO2(111) sample of Comparative Example 1 are discussed. No adsorbed CO was found on the bare ceria surface under the conditions studied.
[0283] For the Pt / CeO2(111) sample of Comparative Example 1, at 200K( Fig.10 a) under CO (at 10 -6 mbar) on Pt deposited on an ordered CeO2(111) surface resulted in the adsorption of 2087 and 2024 cm -1 The IRAS band centered at about 2060 cm -1 After UHV annealing at 500 K and re-exposure to CO, the first two signals disappear, while the 2060 cm -1 The latter can be attributed to the stretching vibration of CO adsorbed on the low-coordination sites on the metallic Pt nanoparticles mainly located at the step edges, as shown previously by STM. Correspondingly, the 2087 and 2024 cm--1 The bands belong to CO adsorbed on structurally ill-defined Pt clusters and aggregates, as its formation is influenced by the limited diffusion rate of surface ad-atoms at these relatively low temperatures.
[0284] In contrast, for the Pt / CeO2-plasma sample of Example 1, after Pt deposition, the CO adsorbed on the Pt species formed on the CeO2-plasma surface was 2104 cm -1 A single band is shown at Fig.10 b) For CO adsorbed on the sample heated to 500 K under UHV, the band is significantly narrowed and red-shifted (to 2095 cm -1 ). After multiple thermal flashes to 500 K, the spectrum is fully reproduced, indicating that the Pt species has good thermal stability, which is completely consistent with the XPS data. For the powder Pt SAC confirmed by high-resolution electron microscopy, the IR band is very similar to the IR band reported in the literature. However, after thermal flash to 700 K, this band disappears, indicating that Pt atoms become inaccessible to CO. However, please note that the IRAS spectrum on metal-supported oxide films follows the selection rule, so only vibrations related to dipole changes perpendicular to the metal surface can be detected. Therefore, CO molecules oriented parallel to the Ru(0001) surface under the ceria film are not visible in the IRAS spectrum.
[0285] The two systems (Example 1 and Comparative Example 1) were also studied with IRAS after exposure to a reaction mixture consisting of 1% CO and 5% O2 (balanced by Ar) at 1 bar in a "high pressure" cell. After 5 min of reaction at 500 K and cooling of the sample to room temperature, the cell was evacuated and the IRAS spectra were recorded in UHV at 300 K without additional exposure to CO. Interestingly, the spectra showed a peak at ~2110 cm for both systems. -1 There is a similar band at 2070 cm-1 observed on annealed -Pt / CeO2(111). -1 The weak and broad band at can be attributed to CO traces located at the edges of the metallic Pt nanoparticles, see above). However, during the slow heating of the sample to 500 K, the spectrum shows a different behavior. Fig.10 a), 2113cm -1 The band gradually shifts to lower wavenumbers (shifted by 10 cm -1), whose integrated intensity slightly decreases, indicating partial desorption of CO. This spectral change and its peak position are characteristic for CO adsorbed on the O-pre-covered Pt surface and can be explained by dipole-dipole interactions between adjacent CO molecules adsorbed by partially oxidized Pt nanoparticles initially formed before the reaction. The formation of relatively large metallic Pt nanoparticles on CeO2(111) can also explain the high signal intensity of the IRAS band due to the image charge effect. In contrast, for the annealed-Pt / CeO2-plasma of Example 1, the 2110 cm-1 peak observed on the annealed-Pt / CeO2-plasma surface during sample heating to 500 K was -1 The weaker band at remains unchanged ( Fig.10 b). Although this band completely disappears upon heating to 700 K and cannot be observed upon CO exposure at room temperature, it reappears after a second CO oxidation reaction (not shown in this paper). Based on these comparative XPS and IRAS studies, it can be concluded that Pt deposited on the plasma-treated CeO2 surface forms single atoms that remain stable in the reaction atmosphere, although its coordination to the ceria surface may be affected by the CO oxidation reaction.
[0286] Based on the structural characterization of the CeO2-plasmon surface by LEED and STM, one can assume that the enhanced Pt stability originates from the surface roughness, which inhibits the diffusivity of Pt adatoms and, therefore, their aggregation. To verify this concept, the Pt adatoms were synthesized at 300 K by irradiating the surface with 1 keV Ar + The ordered CeO2(111) film was ion bombarded for 5 minutes to produce a rough CeO2 surface. In Comparative Example 4, the obtained "CeO2-sputtered" support was used to prepare a (annealed-)Pt / CeO2-sputtered sample.
[0287] From the XPS spectrum of Pt 4f ( Fig.11 a) It can be seen that the Pt in the Pt / CeO2-sputtered sample of Comparative Example 4 produces Pt species that are mainly present in the 2+ state, but a considerable amount of Pt is also found to be in the metallic state (at 71.5 eV), which is likely to be Pt nanoparticles. Fig.11 As shown in Figure 2, a significantly higher intensity is observed for the 530.8 eV signal in the O1s spectrum of the Pt / CeO2-plasma sample of Example 1 compared to the Pt / CeO2-sputtered sample of Comparative Example 4. The results indicate that the plasma treatment of the CeO2 support produces more "O-rich" sites to stabilize Pt single atoms.
[0288] Finally, the activity of the annealed-Pt / CeO2-plasma sample of Example 1 was compared with the activity of the annealed-Pt / CeO2(111) sample of Comparative Example 1 in the CO oxidation reaction. The steady-state CO2 production rate for the catalysts of Example 1 and Comparative Example 1 was measured at different increasing sample temperatures in a high-pressure cell filled with 10 mbar CO and 50 mbar O2 and balanced to 1 bar by He. The results are Fig.12 As shown in a. It can be seen that the annealed-Pt / CeO2-plasma sample of Example 1 exhibits a higher CO2 production rate than the annealed-Pt / CeO2(111) sample of Comparative Example 1.
[0289] Pt / CeO2 powder catalyst
[0290] Reference Example 5: Preparation of original CeO2 powder carrier
[0291] With high specific surface area (50m 2 CeO2 powder with 0.1747 W / g was purchased from US Research Nanomaterials (Cat. No. US3037) and used as received.
[0292] Comparative Example 5: Preparation of original Pt / CeO2 powder catalyst
[0293] Powdered Pt / CeO2 samples were synthesized via strong electrostatic adsorption (SEA) method. High purity (99.995%) tetraammineplatinum(II)nitrate (TAPN) (Sigma-Aldrich, No. 482293) was used as a Pt precursor, and ammonium hydroxide (28% to 30% aqueous solution) was purchased from Acros Organics. The original Pt / CeO2 powder catalyst was obtained by the following steps.
[0294] 1) 1 g of cerium dioxide was crushed, sieved to powder finer than 75 μm, and then added to a deionized water solution mixed with NH 4 OH at pH 9 to prepare a carrier solution.
[0295] 2) 10 mg of TAPN was dissolved in 5 mL of deionized water to obtain a TAPN aqueous solution, and 300 μL of the obtained solution was added to 25 mL of NH4OH solution at pH 9. The obtained solution (25.3 mL) was slowly added to the carrier solution through a burette, and this process took about 3.5 hours.
[0296] 3) The solution obtained in step 2) was dried in a rotary vacuum evaporator (343K, 110 rpm).
[0297] 4) The dried catalyst was calcined in a muffle furnace at 723 K in air at a heating rate of 10 K / min for 4 h, and then cooled to room temperature.
[0298] Example 2: Preparation of Plasma-treated Pt / CeO2 Powder Catalyst
[0299] First, a raw Pt / CeO2 powder catalyst was prepared in the same manner as in Comparative Example 5. The raw Pt / CeO2 powder catalyst was then subjected to O2 plasma treatment in the following manner to obtain a plasma-treated Pt / CeO2 powder sample.
[0300] The O2-plasma treatment was carried out in an apparatus consisting of a glass tube with a frit, a funnel-shaped glassware, a mechanical pump, a radio frequency plasma generator and a high voltage power supply. Figure 1 B provides a schematic diagram of the apparatus for O2-plasma treatment. The glass tube is wrapped with a Cu mesh connected to a high voltage power supply. The frit can hold the calcined powder while allowing the gas to blow out from the bottom. A funnel-shaped glassware is connected to the top of the tube, and the other 3 outlets of the funnel-shaped glassware are connected to a pressure gauge, a mechanical pump, and a tungsten rod for grounding. The tungsten rod extends to the bottom of the glass tube, thereby achieving a uniformly distributed plasma.
[0301] The plasma is generated by a 20-60kHz high voltage power supply (PVM500). The peak voltage is measured with an oscilloscope with a high voltage probe, and the plasma power is the product of the square root of the mean square (RMS) voltage and the RMS current, which are measured by a multimeter. The power and frequency output of the powder power supply are adjusted until a plasma with the desired power is formed.
[0302] The conditions of O2 plasma treatment are as follows:
[0303] 1) Introduce the original Pt / CeO2 powder catalyst into a glass tube (between 100 and 300 mg), and evacuate the glass tube to below 20 mPa.
[0304] 2) Oxygen flows out from the bottom of the tube, and the flow rate is set to 20 mL / min by a mass flow controller (MFC).
[0305] 3) The powdered sample begins to float in the turbulent flow.
[0306] 4) Ignite the plasma. Adjust the power output and frequency of the power supply to achieve the target power of 200W.
[0307] 5) The plasma treatment time is 1 hour.
[0308] Reference Example 6: Preparation of CeO2 powder carrier treated with plasma
[0309] By subjecting the CeO 2 nanoparticles of Reference Example 5 to an O 2 plasma treatment in the same manner as in Example 2, a plasma-treated CeO 2 powder support was prepared.
[0310] Example 3 and Example 4
[0311] First, a raw Pt / CeO2 powder catalyst was prepared in the same manner as described in Comparative Example 5, except that the amount of TAPN dissolved in 5 mL of deionized water in step 2) was changed as shown in Table 2 below. Then, the raw Pt / CeO2 powder catalyst was subjected to O2-plasma treatment in the same manner as in Example 2 to prepare a plasma-treated Pt / CeO2 powder catalyst.
[0312] Comparative Examples 6 and 7:
[0313] The original Pt / CeO2 powder catalyst was produced in the same manner as described in Comparative Example 5, with the only difference that in Comparative Examples 4 and 5, the amount of TAPN solution added to 25 mL of NH4OH solution in step 2) was changed as shown in the following Table 2. In Example 4 and Comparative Example 7, 20 mg of TAPN was dissolved in 10 mL of deionized water to prepare a TAPN aqueous solution.
[0314] [Table 2]
[0315] Example No. Add TAPN solution <![CDATA[Pt / CeO2(wt.%)]]> Example 2 300μL 0.05 Example 3 3.0mL 0.5 Example 4 6.0mL 1.0 Comparative Example 5 300μL 0.05 Comparative Example 6 3.0mL 0.5 Comparative Example 7 6.0mL 1.0
[0316] Due to the impregnation preparation method adopted, it can be assumed that all deposited Pt atoms are located on the surface of the CeO2 support and CeO2 clusters of the prepared catalytically active material. The surface density Ns of the nanoparticles of Pt atoms in the catalytically active material is shown in Table 3.
[0317] [Table 3]
[0318] <![CDATA[Pt / CeO2(wt.%)]]> <![CDATA[Surface density of Pt (at / cm 2 )]]> Example 2 0.05 <![CDATA[3.1×10 12 ]]> Example 3 0.5 <![CDATA[3.1×10 13 ]]> Example 4 1.0 <![CDATA[6.2×10 13 ]]> Comparative Example 5 0.05 <![CDATA[3.1×10 12 ]]> Comparative Example 6 0.5 <![CDATA[3.1×10 13 ]]> Comparative Example 7 1.0 <![CDATA[6.2×10 13 ]]>
[0319] Evaluation of results
[0320] Fig.13a shows the CO2 production rate measured for the Pt / CeO2 powder samples of Example 2 and Comparative Example 5. It can be seen that the plasma-treated Pt / CeO2 powder catalyst of Example 2 exhibits a higher CO2 production rate than the original Pt / CeO2 catalyst of Comparative Example 5.
[0321] Fig.13 b and Fig.13 c shows the STEM images of the plasma-treated Pt / CeO2 catalyst of Example 2 before and after CO oxidation reaction at 523K.
[0322] Fig.14 Examples 2-4 ( Fig.14 a) and Comparative Examples 5-7 ( Fig.14 b) XPS spectrum of Pt 4f of Pt / CeO2 powder catalyst. When the Pt loading is above 0.5wt%, both the original and plasma-treated Pt / CeO2 powder samples show PtO2 clusters, such as Pt 4+ However, the Pt on the plasma-treated Pt / CeO2 catalyst 4+ Species content ( Fig.14 a) Pt on the original Pt / CeO2 catalyst 4+ The content of species is small ( Fig.14 b), which indicates a better atomic-level distribution of Pt.
[0323] Fig.15 The plasma treated Pt / CeO2 catalysts of Examples 3 and 4 ( Fig.15 a and Fig.15 c) and the original Pt / CeO2 catalysts of Comparative Examples 6 and 7 ( Fig.15 b and Fig.15 d). The pristine Pt / CeO2 catalyst exhibits fewer Pt single atoms in favor of the formation of small oxidized clusters (PtO2). It is difficult to detect Pt on CeO2 on the pristine Pt / CeO2 sample measured after CO oxidation compared to the plasma-treated Pt / CeO2 sample. Without being bound by theory, it is speculated that this is due to the formation of PtO2 clusters on the pristine Pt / CeO2 catalyst (consistent with XPS). In STEM, more Pt single atoms were found in the plasma-treated Pt / CeO2 sample, indicating a better distribution of Pt atoms, which is consistent with the XPS results.
[0324] Fig.16a shows the Raman spectra of the pristine CeO2 support of Reference Example 5 and the plasma-treated CeO2 support of Reference Example 6. The 465 cm -1 The Raman band is attributed to F in the bulk CeO2 2g The plasma treated CeO2 support shows a -1 Without being bound by theory, it is assumed that 831 cm -1 The band at is attributed to the surface peroxide (O2 2- ) species.
[0325] Fig.16 b shows the Raman spectra of the original Pt / CeO2 catalyst of Comparative Example 4 and the plasma-treated Pt / CeO2 catalyst of Example 2. Both Raman spectra are normalized to the 2g Model 465cm -1 Compared with the original Pt / CeO2 catalyst, the plasma-treated Pt / CeO2 catalyst has a main band at 831 cm -1 Therefore, it is speculated that the O2 plasma treatment on the Pt / CeO2 catalyst promotes the formation of surface peroxide species.
[0326] Fig.17 The ethylene production rates measured for the Pt / CeO2 powder samples of Example 2 and Comparative Example 5 are shown. It can be seen that the plasma-treated Pt / CeO2 powder catalyst of Example 2 exhibits a higher ethylene production rate than the original (calcined) Pt / CeO2 powder catalyst of Comparative Example 5.
[0327] Pt / TiO2 film samples
[0328] Reference Example 7: Preparation of TiO2 (110) carrier
[0329] TiO2(110) single crystals were purchased from SurfaceNet. The surface of the TiO2(110) single crystal was cleaned by a cycle of ion sputtering-oxygen annealing treatment (which is well known and documented in the literature (Diebold et al., Surface Science, 1995, 331-333 (PART B), 845-854)) until no contamination was detected by XPS to obtain a clean TiO2(110) single crystal.
[0330] Reference Example 8: Preparation of TiO2-plasma film carrier
[0331] The oxygen plasma treatment of the cleaned TiO2 (110) single crystal of Reference Example 7 was performed in the same manner as in Reference Example 4. The obtained sample was denoted as "TiO2-plasma".
[0332] Example 5: Preparation of Pt / TiO2-plasma film samples
[0333] The Pt / TiO2-plasma sample was obtained in the same manner as in Example 1, except that Pt was deposited on the TiO2-plasma film support.
[0334] Comparative Example 8: Preparation of Pt / TiO2(110) film sample
[0335] The Pt / TiO2(110) sample was obtained in the same manner as in Example 5, except that Pt was deposited on a clean TiO2(110) membrane support. Therefore, no plasma treatment was performed.
[0336] Evaluation of results
[0337] Fig.18 The XPS spectra of Pt 4f obtained for the Pt / TiO2 samples of Example 5 and Comparative Example 8 are shown. The Pt in the Pt / TiO2-plasma sample is almost exclusively in the 2+ oxidation state, as indicated by the XPS signal at 72.8 eV. This indicates that the Pt in the Pt / TiO2-plasma sample is present in a single atomic form. The Pt / TiO2 sample shows a significant signal at 71.6 eV, which is attributed to the Pt 0 And it shows that clusters or nanoparticles of metallic Pt are formed.
[0338] Theoretical model research
[0339] The studies presented herein describe mechanistic considerations regarding embodiments of the invention. They should not be construed as describing actual conditions or limiting the scope of the invention, but may be used to illustrate the same.
[0340] Reference Example 9
[0341] (Calculation method)
[0342] The calculations were performed using the Vienna Ab initio Simulation Package (VASP, version 5.4.4) with the generalized gradient functional of Perdew, Burke and Ernzerhof (PBE). The core electrons were treated with the projector-augmented wave (PAW) method, while the valence electrons were extended with a plane wave with a basis set cutoff of 500 eV. An additional Hubbard correction (DFT+U) was applied to the Ce (4f) band, followed by a field-valid U parameter correction of 4.5 eV by Dudarev et al. (Phys. Rev. B, 1998, 57, 1505-1509).
[0343] The optimization of bulk ceria has been The theoretical lattice parameters of the (111), (110), and (100) surfaces are simulated using (2×2) plates. Accordingly, the stepped surface is prepared as a (1×2) supercell. At least vacuum. The bottom layers of the slab (about half of the total) were kept in an optimized bulk position while the upper layers were allowed to relax. Dipole correction along the surface normal was used throughout. Sampling of the Brillouin zone was performed using a k-point grid at the center of G with a grid spacing of approximately When the absolute force acting on each atom drops below , the atomic positions are assumed to converge. Spin polarization is taken into account when necessary. Starting from the pre-optimized original surface, the peroxide formation energies and adsorption energies of Pt and CO are obtained by stepwise structural relaxation. For the ceria nanoparticle / plate composite model, we used the initial octahedral nanoparticles, followed the well-known Wulff-construction structure and applied several cuts to ensure the stoichiometry of CeO2. The resulting ceria nanoislands are fixed on 9 atomic layers of CeO2(111)-(7×7) plates. The entire system consists of 178 cerium atoms and 356 oxygen atoms (film-Ce 147 O 294 ; Nanoparticle-Ce 31 O 62 ), and the total expansion is Due to the large cell size, the optimization is performed at the Gamma point.
[0344] The CO vibrational frequencies were estimated by applying small step-wise displacements of the relevant platinum, carbon and oxygen atoms (Vasp-Tag NFREE=2). Due to the high computational cost, a modified version of the nanoparticle / plate composite system was used, retaining only the surface layer of the lower plate and keeping the Pt fixed. Reference calculations have shown that the deviations caused by this approximation remain below 10 cm -1 , validating the approach. Furthermore, in the case of extended low-index surfaces, higher precision was applied by setting the Vasp-tag PREC to Accurate. Finally, all frequencies were scaled by reference to theoretical and experimental values for molecular CO (see Table 4). Table 4 shows the CO adsorption on extended low-index ceria surfaces (referenced to gaseous single-atom Pt), CO-adsorption on single-atom Pt, and the corresponding CO vibrational frequencies (in cm -1 Based on the experimental value obtained for CO in the gas phase (2143 cm -1 ) and theoretical value (2125cm -1 ), the calculated vibration frequency was calibrated using a scaling factor of 1.008.
[0345] [Table 4]
[0346]
[0347] The plasma was simulated as isolated oxygen atoms (radicals). The binding energy of the O1s level at the surface was calculated under the final state approximation and with reference to the O1s signal of oxygen in the ceria bulk phase (2×2×2) supercell.
[0348] (discuss)
[0349] To understand the principle behind the formation of ceria nanoparticles observed by STM (see Figure 7 a to Figure 7 c), a thermodynamic model was considered under the assumption that the material forming the ceria nanoparticles came from the top CeO2(111) layer of the sample ( Fig.19). Therefore, the ceria film becomes thinner, while the total number of ceria formula units remains unchanged during the reconstruction process (Ce atoms are not sputtered by relatively light O atoms in the plasma). The ceria nanoparticles are approximated as hemispheres of aligned growth of the underlying film, and the surface energies calculated for the extended surfaces with different peroxide coverage using high Miller index surfaces (Tables 5 to 9), as well as the step energy and corner energy (Tables 10 to 11) are used. Depending on the input parameters, the diameter of the ceria nanoparticles is between 3 and 11 nm ( Fig. 20 ), i.e., larger than what is observed experimentally. Nevertheless, these thermodynamic considerations suggest that, in addition to the possible bombardment effect of energetic O atoms in the plasma, the oxygen plasma facilitates the surface reconstruction and formation of ceria nanoparticles on the initially flat film. The increase in surface area leads to a large number of local surface structures that can stabilize oxygen radicals via peroxide groups, while the exposure of other crystal planes on ceria nanoparticles besides (111) simultaneously requires more exothermic reaction energy to form peroxides.
[0350] [Table 5]
[0351]
[0352] [Table 6]
[0353]
[0354] [Table 7]
[0355]
[0356] [Table 8]
[0357]
[0358] [Table 9]
[0359]
[0360] [Table 10]
[0361]
[0362] [Table 11]
[0363]
[0364] As expected, peroxide species affected the Pt adsorption on the CeO2 surface (Table 12 and Fig.21). For example, Pt atoms bind to peroxide-covered (111) surfaces 1-2 eV stronger than to pristine CeO2(111), depending on the peroxide coverage. For (110) surfaces the effect is smaller (average energy gain of about 0.6 eV), while for (100) surfaces the peroxide species even weaken the Pt binding. Among the surfaces studied, the strongest Pt adsorption was observed for the (100)-4O coordination environment. Interestingly, the presence of peroxide groups did not have any favorable effect on Pt binding at this site. Pt adsorption was also investigated for stepped surfaces ( Fig. 22 ). Although the 4O-coordination environment of the square plane, especially for the (210) and (310) surfaces, can again provide sites for strongly exothermic Pt adsorption (Table 12), these step surfaces show rather high surface energies and are therefore thermodynamically unstable. Table 13 shows the adsorption energies (in eV) of Pt single atoms adsorbed on clean and peroxide-covered CeO2 surfaces in the most stable structure as a function of the peroxide coverage (1 ML corresponds to one peroxide group per (1×1) surface unit cell). At the 0.5 ML coverage for the (2×2) plate used in the calculations, two peroxide groups allow two inequivalent geometric arrangements: 1) along the unit vector (labeled "r" = row direction); and 2) diagonally to the unit vector ("d" = diagonal). The energies are referenced to the corresponding ceria surface and Pt bulk. Negative values indicate exothermic adsorption and unfavorable Pt aggregation (formation of Pt-Pt bonds).
[0365] [Table 12]
[0366]
[0367] [Table 13]
[0368]
[0369] Secondly, the interaction between Pt single atoms and ceria nanoparticles formed on the CeO2(111) surface as shown by STM was investigated. For this purpose, a model system consisting of ceria clusters fixed on an extended CeO2(111)-(7×7) plate was constructed. The particle size was compatible with the experimentally measured size (i.e., about 1.0 nm, see Figure 7 ), and accordingly the entire structure was optimized by DFT ( Fig.23 a, middle). Apparently, new Pt adsorption sites are formed at the boundaries between the nanoparticles and the surrounding (111) terraces. The adsorption energies (E adsThe (Pt) (0.57 eV) is much lower than that of the clean and peroxide-covered (111) surfaces (2.80 eV and 1.3-1.6 eV, respectively, Table 13). However, the (100)-4O sites exposed at the vertices of the ceria nanoparticles exhibit the most thermodynamically favorable Pt adsorption sites (E ads (Pt) = -1.76 eV). Depending on their position on the ceria nanoparticles, the coordination environment of the adsorbed Pt atoms is chemically different from that of their symmetrically equivalent counterparts on the extended ceria surface. In particular, at the (100)-4O site, the difference amounts to 0.9 eV (i.e., -1.76 eV and -0.85 eV on the nanoparticle apex and the corresponding extended surface, respectively).
[0370] The nanoparticle / terrace boundaries and square planar “nanopocket” Pt binding sites of this system were also studied for CO adsorption. Fig.23 b. Fig.24 ). CO is not adsorbed on Pt in the (100)-4O site (E ads (CO) = 0.11 eV), while CO adsorption is exothermic for Pt at the nanoparticle / CeO2 (111) boundary (E ads (CO) = -0.86 eV). However, at this site, the CO molecule is oriented almost parallel to the metal support surface and is therefore not visible to IRAS due to the metal selection rule mentioned above. Both findings could explain the very low intensity of the IRAS band on the “deposited” Pt / CeO2-plasma surface compared to that observed in the Pt / CeO2(111) system ( Fig.10 ). For the latter, calculations performed on Pt adatoms on the pristine CeO2(111) surface yield E ads (CO) = -2.14 eV, and the CO frequency is 2093 cm -1 , which is consistent with the 2087 cm- -1 The bands match ( Fig.10 For Pt adsorbed on 0.25 and 0.5 ML peroxide-covered CeO2(111) surfaces, the CO binding energy increases to −2.33 and −2.62 eV, respectively, and the CO frequency shifts to 2081 and 2080 cm-1, respectively. -1 However, the 2104 cm -1The IRAS bands at can be assigned to single Pt atoms adsorbed on bare and / or peroxide-covered CeO2(111) surfaces. After UHV annealing at 500K, these atoms may migrate to stronger binding boundaries and nanocavity sites where they only weakly adsorb CO, resulting in a significant decrease in signal intensity, such as Fig.10 As shown in b.
[0371] In an attempt to determine the nature of the strongly bound CO adsorbed species remaining on the Pt / CeO2-plasma surface after the reaction, several structures derived from Pt / nanocavity sites by sequential removal of O atoms from Pt-4O coordination as a result of their reaction with CO were calculated. Fig.23 The resulting structures, denoted as Pt-3O and Pt-2O in b, exhibit exothermic CO adsorption with energies of −2.00 eV and −0.82 eV, respectively. Therefore, the Pt-3O structure appears to be a likely candidate for the CO observed by IRAS for the post-reacted Pt / CeO2 plasma sample.
[0372] Based on the above observations, the overall effect of plasma treatment on the surface structure of Pt / CeO2(111) is reasonable, e.g. Fig.25 As shown. It is speculated that the plasma treatment leads to two modifications of the ceria surface: 1) morphological, apparently nanostructuring leading to the formation of ceria nanoparticles; and 2) chemical, through the formation of surface peroxides. During Pt deposition, metal atoms can be directly attached to ceria nanoparticles or adsorbed on the peroxide-covered CeO2(111) surface in between, where they form separate strongly bound complexes with the surface peroxide groups, rather than the original CeO2(111) film surface, where Pt atoms diffuse on the surface and aggregate into Pt nanoparticles. With increasing temperature, the Pt atoms trapped by the peroxide groups on the (111) terraces may further migrate to the numerous ceria nanoparticles surrounding and occupying sites at the particle / terrace boundaries and nanocavities. Therefore, the peroxide-covered CeO2(111) surface can firstly prevent Pt aggregation during deposition and secondly serve as a reservoir for Pt single atoms on ceria nanoparticles. Therefore, the morphology and chemical modification of the ceria surface, as well as the synergistic effect between them, may be beneficial to obtain high-density stable Pt single atoms.
Claims
1. A catalytically active material, comprising: a support comprising a metal oxide, and A noble metal, the noble metal being dispersed atomically on the surface of the carrier, wherein The metal oxide is selected from TiO2, CeO2, ZnO, SnO2, Ga2O3, In2O3, ZrO2 and Fe2O3, The noble metal is selected from Pt, Pd, Rh and Au, and The catalytically active material is obtainable by a method comprising the following steps: performing a non-thermal plasma treatment in the presence of O2.
2. The catalytically active material according to claim 1, wherein The number of noble metal atoms normalized to the surface area of the catalytically active material is 3.0 × 10 12 at / cm 2 Up to 8.0×10 14 at / cm 2 , preferably 3.0×10 12 at / cm 2 Up to 4.0×10 14 at / cm 2 , more preferably 6.0×10 12 at / cm 2 Up to 2.0×10 14 at / cm 2 .
3. The catalytically active material according to claim 1 or 2, wherein The relative intensity of the noble metal in oxidation state X relative to the total intensity of the noble metal in all oxidation states in the catalytically active material as measured by X-ray photoelectron spectroscopy is 50% or more, preferably 75% or more, wherein For Pt and Pd, X is 2+, and for Rh and Au, X is 3+.
4. The catalytically active material according to any one of claims 1 to 3, wherein When measured under the following conditions, the infrared absorption spectrum measured for the catalytically active material shows an absorption peak at 2085 cm -1 Up to 2120cm -1 An absorption band in the range of , which does not change when the material is heated from 300K to 500K: (1) exposing the catalytically active material in the reaction unit to a reaction mixture consisting of 1% CO and 5% O2 balanced to 1 bar by Ar, (2) heating the catalytically active material to 500 K at a rate of 60 K / min and reacting the mixture at 500 K and 1 bar for 5 min, (3) cooling the reaction mixture and the catalytically active material to 300K, (4) removing the reaction mixture from the reaction unit and applying 10 -9 Ultra-high vacuum conditions below mbar, (5) Spectra were recorded in ultrahigh vacuum at 300 K without additional exposure to CO, (6) increasing the temperature to 500 K at a rate of 60 K / min and recording spectra at 320 K, 360 K, 400 K, 440 K, 480 K, and 500 K, and (7) Compare the absorption maxima in the spectra recorded at the respective temperatures.
5. The catalytically active material according to any one of claims 1 to 4, wherein The metal oxide and the noble metal are selected from the following combinations: The metal oxide is selected from TiO2 and CeO2, and The noble metal is selected from Pt and Pd, wherein The metal oxide is preferably CeO2 and the noble metal is preferably Pt.
6. The catalytically active material according to any one of claims 1 to 5, wherein The carrier is in the form of particles, such as a powder.
7. The catalytically active material according to claim 6, wherein The support is composed of the metal oxide.
8. The catalytically active material according to claim 6 or 7, wherein The powder carrier has an average particle diameter of 10 nm to 50 nm as measured by scanning transmission electron microscopy, and the powder carrier is preferably a CeO2 powder carrier.
9. The catalytically active material according to any one of claims 6 to 8, wherein The catalytically active material is composed of the support and the noble metal.
10. The catalytically active material according to any one of claims 1 to 5, wherein The support is in the form of a film.
11. The catalytically active material according to claim 10, wherein The carrier is composed of a substrate and clusters supported on the substrate. The substrate and the clusters include the same metal oxide, and The average diameter of the clusters as determined by scanning tunneling microscopy is 2.0 nm or less, preferably 1.5 nm or less.
12. The catalytically active material according to claim 11, wherein The substrate and the clusters are composed of the same metal oxide.
13. Use of the catalytically active material according to any one of claims 1 to 12 in the catalytic oxidation of CO to CO2, wherein Preferably, the catalytically active material is used as follows: In the presence of the catalytically active material, a gas mixture comprising CO and O2 is reacted at a pressure of 0.8 to 2.0 bar and a reaction temperature of 323K to 573K, wherein The content of CO in the gas mixture is less than 5% by volume, The content of O2 in the gas mixture is greater than 2% by volume and less than 25% by volume, and The molar ratio of CO / O2 is preferably 2.0 or less.
14. Use of the catalytically active material according to any one of claims 1 to 12 in the catalytic hydrogenation of alkynes, wherein: Preferably, the catalytically active material is used as follows: In the presence of the catalytically active material, a gas mixture comprising an alkyne and H2 is reacted at a pressure of 0.8 to 2.0 bar and a temperature of 323K to 573K, wherein The content of the alkyne in the gas mixture is less than 10% by volume, The molar ratio of the alkyne to H2 in the gas mixture is less than 1, and The alkyne is preferably a C2-C5 alkyne, more preferably a C2-C3 alkyne.
15. A method for producing a catalytically active material according to any one of claims 6 to 9, the method comprising the following steps: (1) providing a precursor for the catalytically active material, the catalytically active material comprising a support in particulate form, the support comprising a metal oxide, and The noble metal on the surface of the carrier, (2) calcining a precursor for the catalytically active material in the presence of O2, and (3) non-thermal plasma treatment of a calcined precursor for the catalytically active material in the presence of O2.
16. The method according to claim 15, wherein: The step (1) is selected from the following steps (1a) and (1b): (1a) depositing the noble metal onto the support, preferably from an aqueous solution of a salt of the noble metal, wherein preferably the support consists of the metal oxide, and (1b) Co-precipitating the noble metal and the metal oxide from an aqueous solution containing a salt of the noble metal and the metal oxide.
17. The method according to claim 15 or 16, wherein: The non-thermal plasma treatment is performed at a pressure below 20 mbar and an O2 content above 5% by volume.
18. A method for producing a catalytically active material according to any one of claims 10 to 12, said method being selected from method A and method B, The method A comprises the following steps: (1) providing a metal oxide film support, (2) performing a non-thermal plasma treatment in the presence of O2 to obtain a plasma-treated metal oxide film support, and (3) depositing a noble metal onto the plasma-treated metal oxide film support in the gas phase, preferably by physical vapor deposition of noble metal atoms; The method B comprises the following steps: (1) providing a metal oxide film support, (2) depositing the noble metal onto the metal oxide film support from a solution containing the noble metal, and (3) non-thermal plasma treatment in the presence of O2; The preferred -6 mbar to 1×10 -5 The non-thermal plasma treatment is performed under a pressure of 02 mbar.
Citation Information
Patent Citations
Monatomic material, preparation method and application thereof
CN110252347A
Universal method for preparing supported metal monoatoms / metal nanoparticles
CN110694616A
Catalyst for ethylene reaction produced by acetylene selective hydrogenation and its preparing method
CN1511634A
RF non-thermal plasma techniques for catalyst development to improve process efficiencies
US20080161182A1
Cited By
Green synthesis method and application of Pt monatomic catalyst
CN119657131A
Ruthenium-based VOCs catalyst with nano island structure and preparation method of ruthenium-based VOCs catalyst
CN121490758A