Positive active material and preparation method thereof, positive pole piece, secondary battery, battery module, battery pack and electric device
Patent Information
- Application Number
- CN202280092608.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-06-30
AI Technical Summary
Ternary cathode materials and lithium iron phosphate materials have problems with poor voltage resistance, conductivity and lithium ion diffusion properties in lithium-ion batteries, resulting in poor cycleability.
A double-layer carbon coating structure is adopted. The first carbon coating layer is coated on the surface of the cathode active material matrix, and the second carbon coating layer is coated on the surface of the first carbon coating layer, and lattice defects and lattice defects are introduced at the interface. The zigzag structure improves the lithium ion diffusion rate and the material's pressure resistance.
It significantly improves the voltage resistance and lithium ion diffusion performance of the positive active material, reduces the porosity of the battery and the amount of electrolyte injection, enhances the battery's capacity retention rate and reduces the battery impedance.
Smart Images

Figure CN118743052A_ABST
Abstract
Description
Positive electrode active material and preparation method thereof, positive electrode sheet, secondary battery, battery module, battery pack and electrical device Technical Field
[0001] The present application relates to the field of batteries, and in particular to a positive electrode active material and a preparation method thereof, a positive electrode sheet, a secondary battery, a battery module, a battery pack and an electrical device. Background Art
[0002] Ternary cathode materials are the mainstream materials for power lithium-ion batteries due to their high discharge platform and high energy density. However, the cyclic performance of ternary cathode materials is poor, mainly due to the decomposition of the electrolyte on the electrode surface under high potential and the dissolution of Ni, Mn, and Co elements. Lithium iron phosphate has the advantages of low price, good cyclic performance, and good safety, and is widely used in lithium-ion battery cathode materials. However, the tap density of lithium iron phosphate is low, so ternary cathode materials and lithium iron phosphate materials are generally mixed together to increase the bulk density of the positive electrode active material layer. However, when mixing slurries of different particle sizes, especially when nano-lithium iron phosphate is used as filler particles, lithium iron phosphate is not pressure-resistant, and has poor conductivity, dispersibility, and lithium ion diffusion properties, and cannot achieve the ideal combination of large and small particles. Although conventional carbon-coated lithium iron phosphate can improve the conductivity of electrons, the nano-lithium iron phosphate particles usually obtained still have the problems of easy agglomeration, poor lithium ion diffusion properties, and pressure resistance.
[0003] Summary of the Invention
[0004] Based on this, the present application provides a positive electrode active material having excellent pressure resistance, conductivity, dispersibility and lithium ion diffusivity.
[0005] In addition, the present application also provides a method for preparing a positive electrode active material, a positive electrode sheet, a secondary battery, a battery module, a battery pack and an electrical device.
[0006] According to a first aspect of the present application, a positive electrode active material is provided, comprising: a positive electrode active material substrate, a first carbon coating layer and a second carbon coating layer, wherein the first carbon coating layer is coated on the surface of the positive electrode active material substrate, and the second carbon coating layer is coated on the surface of the first carbon coating layer;
[0007] There is a lattice defect at the interface between the first carbon coating layer and the second carbon coating layer, and the second carbon coating layer has a jagged surface.
[0008] The aforementioned positive electrode active material comprises two layers of coating, one inner and one outer, on the surface of the positive electrode active material matrix. This double-layer structure prevents particle breakage of the positive electrode active material matrix, such as lithium iron phosphate particles, due to compression of the ternary particles during charge and discharge, thereby improving the pressure resistance of the positive electrode active material matrix. Lattice defects at the interface of the first and second carbon coating layers significantly improve the diffusion rate of lithium ions within the lattice. The unique serrated structure of the second carbon coating overcomes material fracture at the edges, improving pressure resistance while also better dispersing the positive electrode active material matrix particles and protecting them from aggregation during the reaction process.
[0009] Therefore, the above-mentioned positive electrode active material can be used in combination with the ternary positive electrode material. While reducing the porosity and the amount of electrolyte injection, it also has excellent conductivity and lithium ion diffusion performance, thereby reducing the injection coefficient while improving the battery capacity retention rate and reducing the battery impedance.
[0010] In some embodiments, the lattice defects include line defects. Line defects are dislocation lines in the lattice, which can be regarded as the result of local slippage of one part of the crystal relative to another part of the crystal in the lattice. The zigzag structure is obtained by calcining the alternating dislocations. By generating lattice defects in the crystal, the lithium ion diffusion coefficient and ionic conductivity are effectively increased, thereby reducing the Li+ transfer rate as the lithium ion migration rate increases. + Resistance during the deintercalation process.
[0011] In some embodiments, the second carbon coating layer has an atomically serrated surface. The unique serrated structure of the second carbon coating layer may result in atomic-level edges in the outermost carbon lattice, which can overcome material fracture issues that occur at the edges and better disperse the active particles, protecting them from aggregation during the reaction.
[0012] In some embodiments, at least one of the first carbon coating layer and the second carbon coating layer is a nitrogen-doped carbon layer. Providing the first and second carbon coating layers with nitrogen-doped carbon layers can, on the one hand, further improve their electrical conductivity, and on the other hand, the non-linear CNC bond angle facilitates the formation of a zigzag structure on the surface of the second carbon coating layer and the formation of lattice defects at the interface between the first and second carbon coating layers.
[0013] In some embodiments, the total thickness of the first carbon coating layer and the second carbon coating layer is 10 nm to 30 nm. If the total thickness of the first carbon coating layer and the second carbon coating layer is too thin or too thick, the conductivity of the coating layer will be affected, which is not conducive to electron transfer and ion diffusion.
[0014] In some embodiments, the thickness ratio of the first carbon coating layer to the second carbon coating layer is (1 to 10): (1 to 5). When the thickness of the first carbon coating layer is too low, on the one hand, it cannot achieve the effect of an electron conductor, and on the other hand, it cannot form lattice defects with the second carbon coating layer during the secondary calcination process, and the effect of improving lithium ion transmission cannot be achieved. On the contrary, when the thickness of the first carbon coating layer is too high, the path is too long, which will hinder the transmission rate of lithium ions from the first carbon coating layer into the positive electrode active material matrix, or directly cause the lithium ions to be deposited in the carbon coating layer, making it difficult for lithium ions to be released or embedded, thereby causing ineffective lithium ion diffusion.
[0015] In some embodiments, the positive electrode active material matrix includes at least one of lithium iron phosphate, lithium manganese phosphate, and lithium iron manganese phosphate. These positive electrode active materials suffer from low electronic conductivity and low lithium ion diffusion rates, which can be addressed by using the aforementioned coating layer.
[0016] In some embodiments, the volume average particle size Dv50 of the positive electrode active material matrix is 100 nm to 500 nm. A suitable particle size of the positive electrode active material matrix facilitates the use of the positive electrode active material matrix with other positive electrode materials, such as a ternary positive electrode material, to fully fill the excess pores of the ternary positive electrode material, thereby increasing the compaction density of the positive electrode sheet and reducing the consumption of electrolyte by the pores of the electrode sheet, thereby increasing the volume energy density of the battery.
[0017] According to a second aspect of the present application, a method for preparing a positive electrode active material is provided, comprising the following steps:
[0018] coating the surface of the positive electrode active material matrix with a first carbon source and performing a calcination to obtain a carbon-coated matrix;
[0019] coating a second carbon source on the surface of the carbon-coated substrate and performing secondary calcination;
[0020] The molecules of the first carbon source and the second carbon source both have a zigzag spatial structure.
[0021] The preparation method of the above-mentioned positive electrode active material coats the surface of the positive electrode active material matrix with a first carbon source and a second carbon source having a serrated molecular structure after calcination. The double-layer coating structure can prevent the positive electrode active material matrix, such as lithium iron phosphate particles, from being damaged due to the extrusion of ternary particles during charge and discharge, and improve the pressure resistance of the positive electrode active material matrix. In addition, the first carbon source is calcined twice, and the serrated structure at the interface of the inner and outer coating layers causes strain in the carbon lattice during the secondary calcination process, generating lattice defects, which greatly improves the diffusion rate of lithium ions inside the lattice. After calcination, the second carbon source with a serrated molecular structure forms a structure with a serrated surface, which can overcome the problem of material rupture occurring at the edge and can better disperse the active particles, protecting them from aggregation during the reaction process.
[0022] Therefore, the positive electrode active material prepared by the above method can be used in combination with the ternary positive electrode material. While reducing the porosity and the amount of electrolyte injection, it also has excellent conductivity and lithium ion diffusion performance, thereby improving the capacity retention rate of the battery and reducing the battery impedance while reducing the injection coefficient.
[0023] In some embodiments, both the first carbon source and the second carbon source include components having a conjugated molecular structure. The first carbon source and the second carbon source including components having a conjugated molecular structure can further improve the conductive characteristics of the coating layer, and thus improve the conductivity of the positive electrode active material.
[0024] In some embodiments, both the first carbon source and the second carbon source independently include at least one of polybenzylamine, polyaniline, polypyrrole, and polyethylene diamine. Taking polybenzylamine as an example, the structural formula of polybenzylamine is
[0025] -(A-B-A) n -,
[0026] where n is an integer, A includes at least one of an aromatic group and an alkenyl group, B includes an N atom, and 90° < bond angle of A-B-A < 180°.
[0027] In some embodiments, both the first carbon source and the second carbon source independently include at least one of polybenzylamine, polyaniline, polypyrrole, and polyethylene diamine. Taking polybenzylamine as an example, the polybenzylamine structural formula is It has an inherent twisted molecular chain, in which the benzene ring and the amino group are alternately connected in a non-linear manner to form a serrated molecular chain. This serrated structure may cause atomic-level edges and strain in the carbon lattice. During the second calcination process, the strain at the edge of the carbon lattice at the interface between the first carbon coating layer and the second carbon coating layer will induce distortion of the carbon lattice at high temperature, generating lattice defects, which greatly improves the diffusion rate of lithium ions inside the carbon lattice. In addition, the outermost atomic-level serrated structure can promote the stability of the material to reduce the damage to the electrode structure caused by the volume change of the material, which is beneficial to improving the cycle performance.
[0028] In some embodiments, the mass ratio of the first carbon source to the positive electrode active material matrix is (0.001-0.5):100.
[0029] In some embodiments, the mass ratio of the first carbon source to the positive electrode active material matrix is (0.003-0.2):100.
[0030] In some embodiments, the mass ratio of the first carbon source to the positive electrode active material matrix is (0.01-0.2):100.
[0031] By regulating the mass ratio of the first carbon source to the cathode active material matrix, the thickness of the first carbon coating layer is adjusted. When the thickness of the first carbon coating layer is too low, on the one hand, it cannot achieve the effect of electron conductor, and on the other hand, it cannot form lattice defects with the second carbon coating layer during the secondary calcination process, and the effect of improving lithium ion transmission cannot be achieved. Conversely, when the thickness of the first carbon coating layer is too high, the path is too long, which will hinder the transmission rate of lithium ions from the first carbon coating layer to the cathode active material matrix, or directly cause lithium ions to be deposited in the carbon layer, making it difficult for lithium ions to be released or embedded, resulting in ineffective lithium ion diffusion.
[0032] In some embodiments, the mass ratio of the first carbon source to the second carbon source is (1-10):(1-5). By adjusting the mass ratio of the first carbon source to the second carbon source and the thickness ratio of the first carbon coating layer to the second carbon coating layer, the tap density, electrical conductivity, and lithium ion diffusion coefficient of the positive electrode active material can be further improved.
[0033] In some embodiments, the temperatures of the primary calcination and the secondary calcination are each independently 200°C to 1000°C.
[0034] In some embodiments, the temperatures of the primary calcination and the secondary calcination are each independently 600°C to 800°C.
[0035] The calcination temperature affects the ion diffusivity and electrical conductivity of the positive electrode active material. A suitable calcination temperature can make the lattice defects at the interface between the first carbon coating layer and the second carbon coating layer more uniform, thereby improving the electrical properties of the coated positive electrode active material.
[0036] In some embodiments, the time of the primary calcination and the secondary calcination are each independently 1 hour to 10 hours.
[0037] In some embodiments, the time of the primary calcination and the secondary calcination are each independently 3 hours to 5 hours.
[0038] The calcination time also affects the ion diffusion rate and electrical conductivity of the positive electrode active material. An appropriate calcination time can make the lattice defects at the interface between the first carbon coating layer and the second carbon coating layer more uniform, thereby improving the electrical properties of the coated positive electrode active material.
[0039] In some embodiments, coating the first carbon source on the surface of the positive electrode active material matrix and coating the second carbon source on the surface of the carbon-coated matrix each independently include:
[0040] The monomers are mixed with the core material and ball-milled, and then a doping acid and an initiator are added to polymerize the monomers to form a carbon source coating the core material on the surface of the core material. The core material is the positive electrode active material matrix or the carbon-coated matrix, and the carbon source is the first carbon source or the second carbon source.
[0041] The first carbon source and the second carbon source are coated on the surface of the positive electrode active material matrix by mixing the monomer with the core material and initiating monomer polymerization. The prepared coating layer is denser, and when used to prepare a battery, the DCR DC resistance value is smaller, which is beneficial to improving the capacity value.
[0042] In some embodiments, the doping acid includes at least one of hydrochloric acid, sulfuric acid, and nitric acid.
[0043] In some embodiments, the initiator includes at least one of ammonium persulfate, potassium persulfate, and sodium persulfate.
[0044] In some embodiments, the molar ratio of the doping acid, the initiator, and the monomer is (1-3):(0.5-2.5):(1-5).
[0045] In some embodiments, during the process of coating the first carbon source on the surface of the positive electrode active material matrix and coating the second carbon source on the surface of the carbon-coated matrix, the steps of polymerizing the monomers each independently include:
[0046] The monomer, the core material, the doping acid and the initiator are reacted at 4° C. to 10° C. for 14 to 18 hours, and then washed and vacuum dried at 60° C. to 80° C. for 12 to 18 hours.
[0047] In some embodiments, coating the first carbon source on the surface of the positive electrode active material matrix and coating the second carbon source on the surface of the carbon-coated matrix each independently include:
[0048] The carbon source and the core material are mixed and ball-milled for 10 to 16 hours, then washed, and vacuum-dried at 60 to 80 degrees Celsius for 12 to 18 hours. The carbon source is the first carbon source or the second carbon source, and the core material is the positive electrode active material matrix or the carbon-coated matrix.
[0049] Directly mixing the first carbon source and the second carbon source with the core material is a simpler method.
[0050] In some embodiments, the positive electrode active material matrix includes at least one of lithium iron phosphate, lithium manganese phosphate, and lithium iron manganese phosphate. Lithium iron phosphate, lithium manganese phosphate, and lithium iron manganese phosphate as positive electrode materials suffer from low electronic conductivity and low lithium ion diffusion rate. The use of the aforementioned coating layer can improve these issues.
[0051] In some embodiments, the volume average particle size Dv50 of the positive electrode active material matrix is 100 nm to 500 nm. A suitable particle size of the positive electrode active material matrix facilitates the use of the positive electrode active material matrix with other positive electrode materials, such as a ternary positive electrode material, to fully fill the excess pores of the ternary positive electrode material, thereby increasing the compaction density of the positive electrode sheet and reducing the consumption of electrolyte by the pores of the electrode sheet, thereby increasing the volume energy density of the battery.
[0052] According to a third aspect of the present application, a positive electrode plate is provided, comprising:
[0053] a positive electrode current collector; and
[0054] A positive electrode active material layer, the positive electrode active material layer is located on at least one surface of the positive electrode current collector, and the positive electrode active material layer includes the positive electrode active material of the first aspect of the present application or the positive electrode active material prepared by the preparation method of the positive electrode active material of the second aspect of the present application.
[0055] In some embodiments, the positive electrode active material matrix includes at least one of lithium iron phosphate, lithium manganese phosphate, and lithium manganese iron phosphate, and the positive electrode active material layer further includes a ternary positive electrode material. By mixing the positive electrode active material with the ternary positive electrode material, the compaction density of the positive electrode plate is increased, and the consumption of electrolyte by the plate pores is reduced.
[0056] In some embodiments, the mass ratio of the positive electrode active material to the ternary positive electrode material is (0.1-20):100.
[0057] In some embodiments, the mass ratio of the positive electrode active material to the ternary positive electrode material is (0.1-10):100.
[0058] In some embodiments, the ratio of the volume average particle size Dv50 of the positive electrode active material to the volume average particle size Dv50 of the ternary positive electrode material is (0.1-20):100.
[0059] In some embodiments, the ratio of the volume average particle size Dv50 of the positive electrode active material to the volume average particle size Dv50 of the ternary positive electrode material is (0.1-12):100.
[0060] A suitable mass ratio of the positive electrode active material to the ternary positive electrode material and the Dv50 particle size ratio are conducive to fully filling the excess pores of the ternary positive electrode material, increasing the compaction density of the positive electrode sheet, reducing the consumption of electrolyte by the pores of the sheet, and thus improving the volumetric energy density of the battery. When the mass ratio of the positive electrode active material to the ternary positive electrode material is too low or the Dv50 particle size ratio is too high, the ternary positive electrode material will have a large number of pores, the particle stacking efficiency will be low, and the material distribution will be uneven. On the one hand, this pore space in the positive electrode sheet means that the electrolyte free in it has no contribution to the capacity. The additional weight of the electrolyte also reduces the energy density of the battery and increases the manufacturing cost of the battery cell. On the other hand, in ternary positive electrode materials such as high-nickel systems, the large amount of electrolyte in the pores can easily penetrate into the cracks of the ternary positive electrode material and react, further leading to a decline in battery performance. When the mass ratio of the positive electrode active material to the ternary positive electrode material is too high or the Dv50 particle size ratio is too low, the addition of a large number of positive electrode active material particles will affect the theoretical gram capacity of the ternary positive electrode material and reduce the capacity value.
[0061] In some embodiments, the porosity of the positive electrode sheet is 20% to 25%. The lower porosity of the positive electrode sheet is beneficial for increasing the compaction density of the positive electrode sheet, reducing the consumption of electrolyte by the pores of the sheet, and thus increasing the volume energy density of the battery.
[0062] According to a fourth aspect of the present application, a secondary battery is provided, comprising the positive electrode sheet according to the third aspect of the present application.
[0063] In some embodiments, the secondary battery has a filling coefficient of 2.1 g / Ah to 2.2 g / Ah.
[0064] Under the above filling coefficient, the capacity and cycle retention rate of the secondary battery are still high, but the amount of electrolyte used is reduced, which is conducive to improving the energy density of the battery.
[0065] According to a fifth aspect of the present application, a battery module is provided, comprising the secondary battery according to the fourth aspect of the present application.
[0066] According to a sixth aspect of the present application, a battery pack is provided, comprising the battery module of the fifth aspect of the present application.
[0067] According to a seventh aspect of the present application, an electrical device is provided, comprising at least one selected from the secondary battery of the fourth aspect of the present application, the battery module of the fifth aspect of the present application, and the battery pack of the sixth aspect of the present application.
[0068] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] In order to better describe and illustrate the embodiments or examples of the applications disclosed herein, reference may be made to one or more of the accompanying drawings. The additional details or examples used to describe the accompanying drawings should not be considered to limit the scope of the disclosed applications, the embodiments or examples currently described, and any of the best modes currently understood for these applications.
[0070] FIG1 is a schematic structural diagram of a positive electrode active material according to an embodiment of the present application;
[0071] FIG2 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0072] FIG3 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG2 ;
[0073] FIG4 is a schematic diagram of a battery module according to an embodiment of the present application;
[0074] FIG5 is a schematic diagram of a battery pack according to an embodiment of the present application;
[0075] FIG6 is an exploded view of the battery pack shown in FIG5 according to an embodiment of the present application;
[0076] 7 is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of the present application;
[0077] FIG8 is a scanning electron microscope image of the positive electrode active material prepared in Example 1 of the present application;
[0078] FIG9 is a HRTEM image of the positive electrode active material prepared in Example 1 of the present application;
[0079] FIG10 is a mapping diagram of the positive electrode sheet prepared in Example 1 of the present application;
[0080] FIG11 is a capacity cycle decay diagram of the lithium-ion batteries prepared in Example 1 and Comparative Example 1 of the present application.
[0081] Description of reference numerals:
[0082] 1. Battery pack; 2. Upper case; 3. Lower case; 4. Battery module; 5. Secondary battery; 5. Casing; 5. Electrode assembly; 5. Cover; 6. Electrical device. DETAILED DESCRIPTION
[0083] In order to make the purpose, technical solutions and advantages of this application more clear, the following further describes this application in detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit this application.
[0084] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application.
[0085] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0086] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0087] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0088] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0089] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0090] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0091] In the description of the embodiments of this application, the technical terms "first" and "second" are used only to distinguish different objects and should not be understood to indicate or imply relative importance or implicitly specify the quantity, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.
[0092] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0093] As described in the background technology, due to the problems that exist in both ternary cathode materials and lithium iron phosphate materials, ternary cathode materials and lithium iron phosphate materials are usually mixed together to increase the packing density of the positive electrode active material layer. However, when lithium iron phosphate is used as a filler particle, it still has problems such as poor pressure resistance, conductivity, dispersion, and lithium ion diffusion performance. Although conventional carbon layer-coated lithium iron phosphate can improve electronic conductivity, when lithium iron phosphate particles are used in combination with ternary cathode materials, their dispersion performance, conductivity, pressure resistance, and lithium ion diffusion performance are required to be higher, which is difficult to achieve with traditional carbon layer coating.
[0094] Based on this, the inventors of the present application have obtained the positive electrode active material of the present application with excellent pressure resistance, conductivity, dispersibility and lithium ion diffusivity through a large number of experiments.
[0095] Referring to FIG1 , a first aspect of the present application provides a positive electrode active material, comprising: a positive electrode active material substrate, a first carbon coating layer, and a second carbon coating layer, wherein the first carbon coating layer is coated on the surface of the positive electrode active material substrate, and the second carbon coating layer is coated on the surface of the first carbon coating layer;
[0096] There is lattice defect at the interface between the first carbon coating layer and the second carbon coating layer, and the second carbon coating layer has a jagged surface.
[0097] The aforementioned positive electrode active material comprises two layers of coating, one inner and one outer, on the surface of the positive electrode active material matrix. This double-layer structure prevents particle breakage of the positive electrode active material matrix, such as lithium iron phosphate particles, due to compression of the ternary particles during charge and discharge, thereby improving the pressure resistance of the positive electrode active material matrix. Lattice defects at the interface of the first and second carbon coating layers significantly improve the diffusion rate of lithium ions within the lattice. The unique serrated structure of the second carbon coating overcomes material fracture at the edges, improving pressure resistance and better dispersing the active positive electrode active material matrix particles, protecting them from aggregation during the reaction process.
[0098] Therefore, the above-mentioned positive electrode active material can be used in combination with the ternary positive electrode material. While reducing the porosity and the amount of electrolyte injection, it also has excellent conductivity and lithium ion diffusion performance, thereby reducing the injection coefficient while improving the battery capacity retention rate and reducing the battery impedance.
[0099] In some embodiments, the lattice defects include line defects. Line defects are dislocation lines in the lattice, which can be regarded as the result of local slip of one part of the crystal relative to another part of the crystal in the lattice. The zigzag structure is obtained by calcining the alternating dislocations. By generating lattice defects in the crystal, the lithium ion diffusion coefficient and ionic conductivity are effectively increased, thereby reducing the Li+ transfer rate as the lithium ion migration rate increases. + Resistance during the deintercalation process.
[0100] The serrated surface means that the surface of the second carbon coating layer is a non-smooth surface, and the carbon source molecules used to form the second carbon coating layer have a serrated spatial structure. The carbon source molecules form the second carbon coating layer with a serrated surface after calcination.
[0101] In some embodiments, the second carbon coating layer has an atomically serrated surface. The unique serrated structure of the second carbon coating layer may result in atomic-scale edges in the outermost carbon lattice, which can overcome material fracture at these edges and better disperse the active particles, protecting them from aggregation during the reaction. It will be appreciated that the serrated surface is not limited to the atomic level and can also have other dimensions. Atomic-level serrated surfaces can better disperse the active particles.
[0102] In some embodiments, a serrated surface refers to a surface having one or more triangular, circular, oval, or irregularly shaped teeth.
[0103] In some embodiments, the atomic-scale size is 0.1 nm to 1 nm.
[0104] In some embodiments, at least one of the first carbon coating layer and the second carbon coating layer is a nitrogen-doped carbon layer. Furthermore, both the first carbon coating layer and the second carbon coating layer are nitrogen-doped carbon layers. Providing the first carbon coating layer and the second carbon coating layer as nitrogen-doped coating layers can, on the one hand, further improve their electrical conductivity. On the other hand, the CNC bond angle is non-linear, which is conducive to forming a zigzag structure on the surface of the second carbon coating layer and forming lattice defects at the interface between the first carbon coating layer and the second carbon coating layer.
[0105] In some embodiments, the total thickness of the first carbon coating layer and the second carbon coating layer is 10 nm to 30 nm. In a specific example, the total thickness of the first carbon coating layer and the second carbon coating layer can be 10 nm, 12 nm, 15 nm, 18 nm, 20 nm, 22 nm, 25 nm, 28 nm, 30 nm, or a range consisting of any two of these values. Furthermore, the total thickness of the first carbon coating layer and the second carbon coating layer is 10 nm to 20 nm.
[0106] If the total thickness of the first carbon coating layer and the second carbon coating layer is too thin or too thick, the electrical conductivity of the coating layer will be affected, which is not conducive to electron transfer and ion diffusion.
[0107] In some embodiments, the thickness ratio of the first carbon coating layer to the second carbon coating layer is (1-10):(1-5). In a specific example, the thickness ratio of the first carbon coating layer to the second carbon coating layer is 1:1, 1:2, 1:3, 1:4, 1:5, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, or a range consisting of any two of these values.
[0108] Furthermore, the thickness ratio of the first carbon coating layer to the second carbon coating layer is 4:1 to 1:4. Further, the thickness ratio of the first carbon coating layer to the second carbon coating layer is 4:1 to 1:2. Further, the thickness ratio of the first carbon coating layer to the second carbon coating layer is 2:1 to 1:2.
[0109] When the thickness of the first carbon coating layer is too low, it fails to function as an electron conductor and cannot form lattice defects with the second carbon coating layer during the secondary calcination process, failing to improve lithium ion transport. Conversely, when the thickness of the first carbon coating layer is too high, the path is too long, which will hinder the transfer rate of lithium ions from the first carbon coating layer into the positive electrode active material matrix, or directly cause lithium ions to be deposited in the carbon coating layer, making it difficult for lithium ions to be released or embedded, resulting in ineffective lithium ion diffusion.
[0110] In some embodiments, the positive electrode active material matrix includes at least one of lithium iron phosphate (e.g., LiFePO4, also referred to as LFP), lithium manganese phosphate (e.g., LiMnPO4), and lithium manganese iron phosphate. In a specific example, the positive electrode active material matrix includes at least one of lithium iron phosphate with an olivine structure, lithium manganese phosphate with an olivine structure, and lithium manganese iron phosphate with an olivine structure. Lithium iron phosphate, lithium manganese phosphate, and lithium manganese iron phosphate as positive electrode active materials suffer from low electronic conductivity and low lithium ion diffusion rate. The use of the above-mentioned coating layer can improve these problems.
[0111] In some embodiments, the volume average particle size Dv50 of the positive electrode active material matrix is 100 nm to 500 nm. Dv50 refers to the particle size corresponding to 50% in the volume distribution. As an example, Dv50 can be conveniently measured using a laser particle size analyzer, such as the Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd. in the UK, with reference to GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method. In a specific example, the volume average particle size Dv50 of the positive electrode active material matrix is 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, or a range consisting of any two of these values.
[0112] Furthermore, the volume average particle size Dv50 of the positive electrode active material matrix is 200nm to 400nm. A suitable positive electrode active material matrix particle size is beneficial for fully filling the excess pores of the ternary positive electrode material when the positive electrode active material matrix is used in combination with other positive electrode materials, such as ternary positive electrode materials, thereby increasing the compaction density of the positive electrode sheet and reducing the consumption of electrolyte by the pores of the electrode sheet, thereby increasing the volume energy density of the battery.
[0113] A second aspect of the present application provides a method for preparing a positive electrode active material, comprising the following steps:
[0114] coating the surface of the positive electrode active material matrix with a first carbon source and performing a calcination to obtain a carbon-coated matrix;
[0115] coating a second carbon source on the surface of the carbon-coated substrate and performing secondary calcination;
[0116] The molecules of the first carbon source and the second carbon source both have a zigzag spatial structure.
[0117] The preparation method of the above-mentioned positive electrode active material coats the first carbon source and the second carbon source with a serrated spatial structure on the surface of the positive electrode active material matrix after calcination. The double-layer coating structure can prevent the positive electrode active material matrix, such as lithium iron phosphate particles, from being damaged due to the extrusion of ternary particles during charge and discharge, and improve the pressure resistance of the positive electrode active material matrix. In addition, the first carbon source undergoes two calcination processes. The serrated structure at the interface of the inner and outer coating layers causes strain in the carbon lattice during the secondary calcination process, generating lattice defects, which greatly improves the diffusion rate of lithium ions inside the lattice. The second carbon source with a serrated molecular structure forms a structure with a serrated surface after calcination, which can overcome the problem of material cracking at the edges and better disperse the active particles, protecting them from aggregating during the reaction process.
[0118] Therefore, the positive electrode active material prepared by the above method can be used in combination with the ternary positive electrode material. While reducing the porosity and the amount of electrolyte injection, it also has excellent conductivity and lithium ion diffusion performance, thereby improving the capacity retention rate of the battery and reducing the battery impedance while reducing the injection coefficient.
[0119] In some embodiments, both the first carbon source and the second carbon source include components with a conjugated molecular structure. For example, the molecular structures of the first carbon source and the second carbon source contain conjugated structures such as aromatic groups and alkenyl groups. The first carbon source and the second carbon source including components with a conjugated molecular structure can further improve the conductive properties of the coating layer, and thus improve the conductivity of the positive electrode active material.
[0120] In some embodiments, both the first carbon source and the second carbon source include materials having the following structure:
[0121] -(A-B-A) n -,
[0122] where n is an integer, A includes at least one of an aromatic group and an alkenyl group, B includes an N atom, and 90° < the bond angle of A-B-A < 180°. In a specific example, the bond angle can be measured by the single crystal X-ray diffraction method.
[0123] In some embodiments, the first carbon source and the second carbon source each independently include at least one of polybenzylamine, polyaniline, polypyrrole, and polyethylene diamine. It can be understood that the first carbon source and the second carbon source can be the same or different.
[0124] Taking polybenzylamine as an example, the structural formula of polybenzylamine is It has an inherently twisted molecular chain, in which benzene rings and amino groups are alternately connected in a nonlinear manner to form a zigzag molecular chain. This zigzag structure may lead to atomic-level edges and strain in the carbon lattice. During the second calcination process, the strain at the carbon lattice edge at the interface between the first carbon coating layer and the second carbon coating layer induces distortion of the carbon lattice at high temperature, greatly improving the diffusion rate of lithium ions within the carbon lattice. In addition, the outermost atomic-level zigzag structure can promote the stability of the material, thereby reducing the damage to the electrode structure caused by the material volume change, which is beneficial to improving the cycle performance.
[0125] In some embodiments, the mass ratio of the first carbon source to the positive electrode active material matrix is (0.001-0.5):100. In a specific example, the mass ratio of the first carbon source to the positive electrode active material matrix is 0.001:100, 0.005:100, 0.01:100, 0.02:100, 0.03:100, 0.04:100, 0.05:100, 0.06:100, 0.07:100, 0.08:100, 0.09:100, 0.1:100, 0.12:100, 0.15:100, 0.18:100, 0.2:100, 0.25:100, 0.3:100, 0.35:100, 0.4:100, 0.45:100, 0.5:100 or a range consisting of any two of these values.
[0126] Furthermore, the mass ratio of the first carbon source to the positive electrode active material matrix is (0.003-0.2):100. Further, the mass ratio of the first carbon source to the positive electrode active material matrix is (0.01-0.2):100. Further, the mass ratio of the first carbon source to the positive electrode active material matrix is (0.01-0.05):100.
[0127] By regulating the mass ratio of the first carbon source to the cathode active material matrix, the thickness of the first carbon coating layer is adjusted. When the thickness of the first carbon coating layer is too low, on the one hand, it cannot achieve the effect of electron conductor, and on the other hand, it cannot form lattice defects with the second carbon coating layer during the secondary calcination process, and the effect of improving lithium ion transmission cannot be achieved. Conversely, when the thickness of the first carbon coating layer is too high, the path is too long, which will hinder the transmission rate of lithium ions from the first carbon coating layer to the cathode active material matrix, or directly cause lithium ions to be deposited in the carbon layer, making it difficult for lithium ions to be released or embedded, resulting in ineffective lithium ion diffusion.
[0128] In some embodiments, the mass ratio of the first carbon source to the second carbon source is (1-10):(1-5). In a specific example, the mass ratio of the first carbon source to the second carbon source is 1:1, 1:2, 1:3, 1:4, 1:5, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, or a range consisting of any two of these values.
[0129] Furthermore, the mass ratio of the first carbon source to the second carbon source is 4:1 to 1:4. Furthermore, the mass ratio of the first carbon source to the second carbon source is 4:1 to 1:2. Furthermore, the mass ratio of the first carbon source to the second carbon source is 2:1 to 1:2.
[0130] By adjusting the mass ratio of the first carbon source to the second carbon source and the thickness ratio of the first carbon coating layer to the second carbon coating layer, the tap density, electrical conductivity and lithium ion diffusion coefficient of the positive electrode active material can be further improved.
[0131] In some embodiments, the temperature of the primary calcination and the secondary calcination is independently 200° C. to 1000° C. In a specific example, the temperature of the primary calcination and the secondary calcination is independently 200° C., 250° C., 300° C., 350° C., 400° C., 450° C., 500° C., 550° C., 600° C., 620° C., 650° C., 680° C., 700° C., 720° C., 750° C., 780° C., 800° C., 850° C., 900° C., 950° C., 1000° C., or a range consisting of any two of these values. It will be understood that the temperature of the primary calcination and the secondary calcination may be the same or different.
[0132] Furthermore, the temperatures of the primary calcination and the secondary calcination are each independently 600° C. to 800° C. The calcination temperature affects the ion diffusivity and electrical conductivity of the positive electrode active material. A suitable calcination temperature makes the lattice defects at the interface between the first carbon coating layer and the second carbon coating layer more uniform, thereby improving the electrical properties of the coated positive electrode active material.
[0133] In some embodiments, the time for the primary calcination and the secondary calcination is independently 1 hour to 10 hours. In a specific example, the time for the primary calcination and the secondary calcination is independently 1 hour, 2 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, or a range consisting of any two of these values. It will be understood that the time for the primary calcination and the secondary calcination can be the same or different.
[0134] Furthermore, the time for the first calcination and the second calcination is independently 3 hours to 5 hours. The calcination time also affects the ion diffusion rate and electrical conductivity of the positive electrode active material. An appropriate calcination time can make the lattice defects at the interface between the first carbon coating layer and the second carbon coating layer more uniform, thereby improving the electrical properties of the coated positive electrode active material.
[0135] In some embodiments, the heating rates during the primary calcination and the secondary calcination are each independently 1°C / min to 10°C / min. In a specific example, the heating rates during the primary calcination and the secondary calcination are each independently 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, or a range consisting of any two of these values.
[0136] In some embodiments, coating the first carbon source on the surface of the positive electrode active material matrix and coating the second carbon source on the surface of the carbon-coated matrix each independently include:
[0137] The monomers are mixed with the core material and ball-milled, and then the doping acid and initiator are added to polymerize the monomers to form a carbon source coating the core material on the surface of the core material. The core material is a positive electrode active material matrix or a carbon-coated matrix, and the carbon source is a first carbon source or a second carbon source.
[0138] The first carbon source and the second carbon source are coated on the surface of the positive electrode active material matrix by mixing the monomer with the core material and initiating monomer polymerization. The prepared coating layer is denser, and when used to prepare a battery, the DCR DC resistance value is smaller, which is beneficial to improving the capacity value.
[0139] The monomers and the core material are thoroughly mixed by ball milling the monomers and the core material.
[0140] In a specific example, the solvent used for ball milling includes at least one of water, ethanol, isopropyl ketone and acetone.
[0141] In a specific example, the time for ball milling the monomer and the core material is 10 hours to 16 hours. For example, the time for ball milling is 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, or a range consisting of any two of these values.
[0142] In some embodiments, the doping acid includes at least one of hydrochloric acid, sulfuric acid, and nitric acid. It is understood that the doping acids used in the process of coating the first carbon source on the surface of the positive electrode active material substrate and the process of coating the second carbon source on the surface of the carbon-coated substrate can be the same or different.
[0143] In some embodiments, the initiator comprises a persulfate. Furthermore, the initiator comprises at least one of ammonium persulfate, potassium persulfate, and sodium persulfate. It will be appreciated that the initiators used in coating the first carbon source on the surface of the positive electrode active material substrate and coating the second carbon source on the surface of the carbon-coated substrate may be the same or different.
[0144] In some embodiments, the molar ratio of the doping acid, initiator, and monomer is (1-3):(0.5-2.5):(1-5). It will be appreciated that the molar ratios of the doping acid, initiator, and monomer used in the process of coating the first carbon source on the surface of the positive electrode active material substrate and the process of coating the second carbon source on the surface of the carbon-coated substrate may be the same or different.
[0145] In some embodiments, in the process of coating the first carbon source on the surface of the positive electrode active material matrix and coating the second carbon source on the surface of the carbon-coated matrix, the steps of polymerizing the monomers each independently include:
[0146] The monomer, core material, doping acid and initiator are reacted at 4° C. to 10° C. for 14 to 18 hours, then washed and vacuum dried at 60° C. to 80° C. for 12 to 18 hours.
[0147] In a specific example, the reaction temperature of the monomer, core material, doping acid, and initiator is 4° C., 5° C., 6° C., 7° C., 8° C., 9° C., 10° C., or a range consisting of any two of these values. The reaction time of the monomer, core material, doping acid, and initiator is 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, or a range consisting of any two of these values.
[0148] In a specific example, the vacuum drying temperature is 60° C., 65° C., 70° C., 75° C., 80° C., or a range consisting of any two of these values. The vacuum drying time is 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, or a range consisting of any two of these values.
[0149] In a specific example, the washing is performed with anhydrous ethanol and deionized water, respectively.
[0150] In other embodiments, coating the first carbon source on the surface of the positive electrode active material matrix and coating the second carbon source on the surface of the carbon-coated matrix each independently include:
[0151] The carbon source and the core material are mixed and ball-milled for 10 to 16 hours, then washed and vacuum-dried at 60 to 80 degrees Celsius for 12 to 18 hours. The carbon source is the first carbon source or the second carbon source, and the core material is a positive electrode active material matrix or a carbon-coated matrix.
[0152] The coating method is simpler by directly mixing the first carbon source and the second carbon source with the core material.
[0153] The carbon source and the core material are ball-milled to fully mix the carbon source and the core material. In a specific example, the solvent used for ball milling includes at least one of water, ethanol, isopropyl ketone and acetone.
[0154] In a specific example, the washing is performed with anhydrous ethanol and deionized water, respectively.
[0155] In a specific example, the mixing ball milling time is 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, or a range consisting of any two of these values. The vacuum drying temperature is 60° C., 65° C., 70° C., 75° C., 80° C., or a range consisting of any two of these values. The vacuum drying time is 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, or a range consisting of any two of these values.
[0156] In some embodiments, the positive electrode active material matrix includes at least one of lithium iron phosphate, lithium manganese phosphate, and lithium iron manganese phosphate. These positive electrode active materials suffer from low electronic conductivity and low lithium ion diffusion rates, which can be addressed by using the aforementioned coating layer.
[0157] In some embodiments, the volume average particle size Dv50 of the positive electrode active material matrix is 100 nm to 500 nm. In a specific example, the volume average particle size Dv50 of the positive electrode active material matrix is 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, or a range consisting of any two of these values.
[0158] Furthermore, the volume average particle size Dv50 of the positive electrode active material matrix is 200nm to 400nm. A suitable matrix particle size is beneficial for the positive electrode active material matrix to fully fill the excess pores of the ternary positive electrode material when used in combination with other positive electrode materials, such as ternary positive electrode materials, thereby increasing the compaction density of the positive electrode sheet and reducing the consumption of electrolyte by the pores of the electrode sheet, thereby improving the volume energy density of the battery.
[0159] The third aspect of the present application provides a positive electrode plate, which includes a positive electrode collector and a positive electrode active material layer arranged on at least one surface of the positive electrode collector, and the positive electrode active material layer includes the positive electrode active material of the first aspect of the present application or the positive electrode active material prepared by the preparation method of the positive electrode active material of the second aspect of the present application.
[0160] In some embodiments, the positive electrode active material matrix includes at least one of lithium iron phosphate, lithium manganese phosphate and lithium manganese iron phosphate, and the positive electrode active material layer further includes a ternary positive electrode material, the molecular formula of the ternary positive electrode material is: LiNi x Co y Mn 1-x-y O2, x>0, y>0, or LiNi 0.8+a+b Co 0.15-a Al 0.05-b O2, 0≤a<0.15, 0≤b<0.05. For example, the ternary positive electrode material can be lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds, etc. In a specific example, lithium nickel cobalt manganese oxide can be LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 )wait.
[0161] By mixing the positive electrode active material with the ternary positive electrode material, the compaction density of the positive electrode plate is increased and the consumption of electrolyte by the plate pores is reduced.
[0162] In some embodiments, the mass ratio of the positive electrode active material to the ternary positive electrode material is (0.1-20): 100. In a specific example, the mass ratio of the positive electrode active material to the ternary positive electrode material is 0.1:100, 0.2:100, 0.5:100, 1:100, 1.5:100, 2:100, 2.5:100, 3:100, 3.5:100, 4:100, 4.5:100, 5:100, 6:100, 7:100, 8:100, 9:100, 10:100, 12:100, 15:100, 18:100, 20:100, or a range consisting of any two of these values.
[0163] Furthermore, the mass ratio of the positive electrode active material to the ternary positive electrode material is (0.1-10):100. Further, the mass ratio of the positive electrode active material to the ternary positive electrode material is (0.1-5):100. Further, the mass ratio of the positive electrode active material to the ternary positive electrode material is (0.1-3):100.
[0164] In some embodiments, the ratio of the volume average particle size Dv50 of the positive electrode active material to the ternary positive electrode material is (0.1-20): 100. In a specific example, the ratio of the volume average particle size Dv50 of the positive electrode active material to the ternary positive electrode material is 0.1:100, 0.2:100, 0.5:100, 1:100, 1.5:100, 2:100, 2.5:100, 3:100, 3.5:100, 4:100, 4.5:100, 5:100, 5.5:100, 6:100, 6.5:100, 7:100, 8:100, 9:100, 10:100, 12:100, 15:100, 18:100, 20:100, or a range consisting of any two of these values.
[0165] Furthermore, the ratio of the volume average particle size Dv50 of the positive electrode active material to the ternary positive electrode material is (0.1-12):100. Further, the ratio of the volume average particle size Dv50 of the positive electrode active material to the ternary positive electrode material is (0.1-10):100. Further, the ratio of the volume average particle size Dv50 of the positive electrode active material to the ternary positive electrode material is (1-10):100. Further, the ratio of the volume average particle size Dv50 of the positive electrode active material to the ternary positive electrode material is (3-7):100.
[0166] A suitable mass ratio of the positive electrode active material to the ternary positive electrode material and the Dv50 particle size ratio are conducive to fully filling the excess pores of the ternary positive electrode material, increasing the compaction density of the positive electrode sheet, reducing the consumption of electrolyte by the pores of the sheet, and thus improving the volumetric energy density of the battery. When the mass ratio of the positive electrode active material to the ternary positive electrode material is too low or the Dv50 particle size ratio is too high, the ternary positive electrode material will have a large number of pores, the particle stacking efficiency will be low, and the material distribution will be uneven. On the one hand, this pore space in the positive electrode sheet means that the electrolyte free in it has no contribution to the capacity. The additional weight of the electrolyte also reduces the energy density of the battery and increases the manufacturing cost of the battery cell. On the other hand, in ternary positive electrode materials such as high-nickel systems, the large amount of electrolyte in the pores can easily penetrate into the cracks of the ternary positive electrode material and react, further leading to a decline in battery performance. When the mass ratio of the positive electrode active material to the ternary positive electrode material is too high or the Dv50 particle size ratio is too low, the addition of a large number of positive electrode active material particles will affect the theoretical gram capacity of the ternary positive electrode material and reduce the capacity value.
[0167] In some embodiments, the porosity of the positive electrode sheet is 20% to 25%. In a specific example, the porosity of the positive electrode sheet is 20%, 21%, 21.2%, 21.4%, 21.6%, 21.8%, 22%, 22.1%, 22.2%, 22.4%, 22.6%, 22.8%, 23%, 24%, 25%, or a range consisting of any two of these values. Furthermore, the porosity of the positive electrode sheet is 21% to 23%. The above-mentioned low porosity of the positive electrode sheet is conducive to improving the compaction density of the positive electrode sheet, reducing the consumption of electrolyte by the pores of the electrode sheet, and thus improving the volume energy density of the battery.
[0168] In some embodiments, the positive electrode active material layer may further include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0169] In some embodiments, the positive electrode active material layer may further include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0170] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is provided on either or both of the two facing surfaces of the positive electrode current collector.
[0171] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0172] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the ternary positive electrode material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0173] The secondary battery, battery module, battery pack, and electric device of the present application are described below with reference to the accompanying drawings as appropriate.
[0174] A fourth aspect of the present application provides a secondary battery.
[0175] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During the battery's charge and discharge processes, active ions are inserted and removed between the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.
[0176] In some embodiments, the filling coefficient of the secondary battery is 2.1g / Ah to 2.2g / Ah. The filling coefficient is a fixed constant determined when designing the battery, which refers to the ratio of the filling mass of the electrolyte in the battery to the designed discharge capacity of the battery. In a specific example, the filling coefficient of the secondary battery is 2.1g / Ah, 2.11g / Ah, 2.12g / Ah, 2.13g / Ah, 2.14g / Ah, 2.15g / Ah, 2.16g / Ah, 2.17g / Ah, 2.18g / Ah, 2.19g / Ah, 2.2g / Ah or a range consisting of any two of these values. Under the above filling coefficient, the capacity and cycle retention rate of the secondary battery are still high, but the amount of electrolyte used is reduced, which is beneficial to improve the energy density of the battery.
[0177] Positive electrode
[0178] The positive electrode plate is the positive electrode plate provided in the third aspect of this application and will not be described in detail here.
[0179] Negative electrode
[0180] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0181] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0182] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0183] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0184] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0185] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0186] In some embodiments, the negative electrode film layer may optionally further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0187] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0188] electrolytes
[0189] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0190] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0191] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0192] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0193] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0194] Isolation film
[0195] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0196] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0197] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0198] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0199] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0200] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG2 shows a secondary battery 5 having a square structure as an example.
[0201] In some embodiments, referring to Figure 3, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0202] A fifth aspect of the present application provides a battery module. The battery module includes the secondary battery of the fourth aspect of the present application. In one example, the battery module is assembled from secondary batteries.
[0203] In some embodiments, the number of secondary batteries contained in the battery module may be one or more, and those skilled in the art may select the specific number based on the application and capacity of the battery module.
[0204] Figure 4 shows an example battery module 4. Referring to Figure 4 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.
[0205] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0206] A sixth aspect of the present application provides a battery pack comprising the battery module of the fifth aspect of the present application. In one example, the battery pack is assembled from the battery modules. In some embodiments, the battery pack may include one or more battery modules, the specific number of which can be selected by those skilled in the art based on the application and capacity of the battery pack.
[0207] Figures 5 and 6 illustrate an example battery pack 1. Referring to Figures 5 and 6 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0208] The seventh aspect of the present application further provides an electrical device, which includes at least one selected from the secondary battery provided in the fourth aspect of the present application, the battery module provided in the fifth aspect of the present application, and the battery pack provided in the sixth aspect of the present application. The secondary battery, battery module or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto. Among them, the mobile device may be, for example, a mobile phone, a laptop computer, etc.; the electric vehicle may be, for example, a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., but is not limited thereto.
[0209] As an electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.
[0210] FIG7 shows an example of an electric device 6. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the electric device's requirements for high power and high energy density of secondary batteries, a battery pack or battery module may be used.
[0211] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0212] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0213] Example 1
[0214] Preparation of positive electrode active materials:
[0215] (1) Benzylamine and lithium iron phosphate with a Dv50 of 300 nm were mixed in a mass ratio of 0.01:100, added to a mixed solution of ethanol and water, and ball-milled for 10 h. In the mixed solution, the concentration of benzylamine monomer was 0.5 M. 0.5 M hydrochloric acid was added as a doping acid and 1 M ammonium persulfate was added as an initiator to oxidize the benzylamine monomer. The reaction system was then placed in an ice-water bath at 4 ° C and stirred for 14 h. After the reaction, the mixture was washed with anhydrous ethanol and deionized water, respectively, and dried in a vacuum at 60 ° C for 12 h to obtain a polybenzylamine-coated lithium iron phosphate precursor. The polybenzylamine-coated lithium iron phosphate precursor was heated to 700 ° C at a heating rate of 5 ° C / min in a nitrogen atmosphere and calcined for 3 h to obtain N-doped carbon-coated lithium iron phosphate.
[0216] (2) The N-doped carbon-coated lithium iron phosphate obtained in (1) is further mixed with benzylamine, with the mass ratio of benzylamine to the mass of benzylamine added in (1) being 2:1, and then added to a mixed solution of ethanol and water for ball milling for 2 hours. In the mixed solution, the concentration of benzylamine monomer is 0.5M, and 0.5M hydrochloric acid is added as a doping acid and 1M ammonium persulfate is added as an initiator to oxidize the benzylamine monomer. The reaction system is then placed in an ice-water bath at 4°C and stirred for 14 hours. After the reaction is completed, the reaction is vacuum dried at 60°C for 12 hours to obtain polybenzylamine-coated carbon-coated lithium iron phosphate. The reaction is then calcined in a nitrogen atmosphere at a heating rate of 5°C / min, a calcination temperature of 700°C, and a calcination time of 3 hours. A second carbon coating layer with a serrated edge is coated on the outside of the N-doped carbon-coated lithium iron phosphate, and lattice defects are formed at the interface between the N-doped carbon layer and the second carbon coating layer. Finally, the obtained coating was ground to obtain the lithium iron phosphate positive electrode active material of Example 1.
[0217] Preparation of positive electrode:
[0218] The prepared lithium iron phosphate cathode active material (Dv50 = 300 nm), nickel cobalt manganese (NCM) ternary cathode material (Dv50 = 6 μm), conductive carbon black, binder polyvinylidene fluoride (PVDF), and N-methylpyrrolidone (NMP) were mixed uniformly in a weight ratio of 2.88:92.96:1.47:1.55:1.14 to obtain a cathode slurry. The cathode slurry was evenly coated on the cathode current collector, and the cathode sheets were obtained after drying, cold pressing, and slitting.
[0219] Preparation of negative electrode sheet:
[0220] The active material (artificial graphite), silicon oxide, conductive agent (carbon black), binder (styrene-butadiene rubber (SBR), and thickener (sodium carboxymethyl cellulose (CMC)) were dissolved in deionized water at a weight ratio of 72.3:24.9:0.8:0.8:1.2, mixed evenly, and prepared into a negative electrode slurry. The negative electrode slurry was then coated onto the negative electrode current collector copper foil and cold pressed to obtain a negative electrode sheet.
[0221] Preparation of electrolyte:
[0222] In an argon atmosphere glove box, organic solvents ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / diethyl carbonate (DEC) were mixed uniformly in a volume ratio of 36:29:35, 1M LiPF6 lithium salt was added and dissolved in the organic solvent, and stirred uniformly to obtain an electrolyte.
[0223] Isolation film:
[0224] Polypropylene film is used as the isolation film.
[0225] Preparation of lithium-ion batteries:
[0226] The positive electrode sheet, separator, and negative electrode sheet of Example 1 were stacked in order, with the separator positioned between the positive and negative electrode sheets to provide isolation. The sheets were then wound to obtain a bare cell. The tabs were welded to the bare cell and placed in an aluminum shell. The shell was then baked at 100°C to remove moisture. The electrolyte was then injected and sealed to obtain an uncharged battery. The uncharged battery then underwent a series of steps, including resting, hot and cold pressing, formation, shaping, and capacity testing, to obtain the lithium-ion battery of Example 1.
[0227] Example 2 to Example 7
[0228] The difference between Examples 2 to 7 and Example 1 is that the mass ratio of benzylamine added in the preparation step (1) of the positive electrode active material to the benzylamine added in the step (2) is different and is adjusted to: 3:1, 4:1, 1:1, 1:2, 1:3, 1:4, respectively. The other steps are the same as in Example 1.
[0229] Example 8 to Example 9
[0230] The difference between Examples 8 and 9 and Example 1 is that in the preparation step (1) of the positive electrode active material, the mass ratio of lithium iron phosphate to benzylamine is different, adjusted to 100:0.005 and 100:0.02 respectively. The other steps are the same as Example 1.
[0231] Example 10 to Example 14
[0232] The difference between Examples 10 to 14 and Example 1 is that in the preparation steps (1) and (2) of the positive electrode active material, the calcination temperatures are different and are adjusted to 300° C., 500° C., 600° C., 800° C., and 900° C., respectively. The other steps are the same as in Example 1.
[0233] Example 15 to Example 19
[0234] The difference between Examples 15 to 19 and Example 1 is that in the preparation steps (1) and (2) of the positive electrode active material, the calcination time is different and is adjusted to 1 h, 2 h, 4 h and 5 h respectively. The other steps are the same as in Example 1.
[0235] Example 20
[0236] The difference between Example 20 and Example 1 is that the preparation process of the positive electrode active material is different, and the other steps are the same as Example 1. Specifically, the preparation process of the positive electrode active material is as follows:
[0237] (1) Polybenzylamine and lithium iron phosphate with a Dv50 of 300 nm were mixed in a mass ratio of 0.01:100, added to a mixed solution of ethanol and water, and ball-milled for 10 h to uniformly mix the polybenzylamine and lithium iron phosphate. The mixture was then washed with anhydrous ethanol and deionized water and vacuum-dried at 60°C for 12 h to obtain a polybenzylamine-coated lithium iron phosphate precursor. The polybenzylamine-coated lithium iron phosphate precursor was heated to 700°C at a heating rate of 5°C / min under a nitrogen atmosphere and calcined for 3 h to obtain N-doped carbon-coated lithium iron phosphate.
[0238] (2) The nitrogen-doped carbon-coated lithium iron phosphate obtained in (1) is further mixed with polyaniline, with the mass ratio of polybenzylamine to the mass of polybenzylamine added in (1) being 2:1, and then added to a mixed solution of ethanol and water for ball milling for 2 hours, and then washed with anhydrous ethanol and deionized water, and then vacuum-dried at 60°C and calcined in nitrogen, wherein the heating rate is 5°C / min, the calcination temperature is 700°C, and the calcination time is 3 hours. A second carbon coating layer with a serrated edge is coated on the outside of the carbon-coated lithium iron phosphate, and lattice defects are formed at the interface between the N-doped carbon layer and the second carbon coating layer. Finally, the obtained coating is ground to obtain the lithium iron phosphate positive electrode active material of Example 20.
[0239] Example 21 to Example 22
[0240] The difference between Examples 21 and 22 and Example 1 is that the monomers in steps (1) and (2) of the preparation process of the positive electrode active material are different, being adjusted to aniline and ethylenediamine respectively. The other steps are the same as in Example 1.
[0241] Example 23
[0242] The difference between Example 23 and Example 1 is that in step (1) of the preparation process of the positive electrode active material, the first monomer is different, and pyrrole is used to replace the benzylamine in Example 1. The other steps are the same as in Example 1.
[0243] Example 24
[0244] The difference between Example 24 and Example 1 is that the matrix of the positive electrode active material is different, and the lithium iron phosphate matrix in Example 1 is replaced by a lithium manganese phosphate matrix. The other steps are the same as those in Example 1.
[0245] Example 25-Example 26
[0246] Examples 25 and 26 differ from Example 1 in that, during the preparation of the positive electrode active material, the volume average particle size Dv50 of the lithium iron phosphate matrix is adjusted to 200 nm and 400 nm, respectively. Accordingly, during the preparation of the positive electrode sheet, the volume average particle size Dv50 of the positive electrode active material is adjusted to 200 nm and 400 nm, respectively. All other steps are the same as in Example 1.
[0247] Example 27 to Example 31
[0248] The difference between Examples 27 to 31 and Example 1 is that during the preparation of the positive electrode sheets, the mass ratios of the lithium iron phosphate positive electrode active material to the ternary positive electrode material are different and are adjusted to 0.005:1, 0.02:1, 0.05:1, 0.1:1, and 0.2:1, respectively. The other steps are the same as in Example 1.
[0249] Example 32 to Example 34
[0250] The difference between Examples 32 to 34 and Example 1 is that during the preparation of the lithium-ion battery, the electrolyte injection coefficient is adjusted from 2.2 g / Ah to 2.15 g / Ah, 2.10 g / Ah, and 2.05 g / Ah, respectively. The other steps are the same as in Example 1.
[0251] Comparative Example 1
[0252] The difference between Comparative Example 1 and Example 1 is that the positive electrode active material is different, and accordingly, the preparation process of the positive electrode sheet is different. The other steps are the same as those in Example 1. The preparation process of the positive electrode sheet is as follows:
[0253] Uncoated lithium iron phosphate was used as the positive electrode active material. Lithium iron phosphate (Dv50 = 300 nm), NCM (nickel cobalt manganese) ternary positive electrode material (Dv50 = 6 μm), carbon black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a solvent were thoroughly stirred and mixed in a weight ratio of 2.88:92.96:1.47:1.55:1.14 to produce a positive electrode slurry. The positive electrode slurry was then evenly coated on the positive electrode current collector, followed by drying, cold pressing, and slitting to produce the positive electrode sheet of Comparative Example 1.
[0254] Comparative Example 2
[0255] The difference between Comparative Example 2 and Example 1 is that the preparation process of the lithium iron phosphate positive electrode active material is different, and the remaining steps are the same as those in Example 1. Specifically, the preparation process of the lithium iron phosphate positive electrode active material in Comparative Example 2 is as follows:
[0256] Benzylamine and lithium iron phosphate (LFP) with a Dv50 of 300 nm were mixed in a mass ratio of 0.02:100 and added to a mixed solution of ethanol and water for 10 hours. The benzylamine monomer concentration in the mixed solution was 0.5M. 0.5M hydrochloric acid was added as a doping acid and 1M ammonium persulfate was added as an initiator to oxidize the benzylamine monomer. The reaction system was then placed in an ice-water bath at 4°C and stirred for 14 hours. After the reaction, the mixture was washed with anhydrous ethanol and deionized water, respectively, and dried under vacuum at 60°C for 12 hours to obtain a polybenzylamine-coated LFP precursor. The polybenzylamine-coated LFP precursor was then heated to 700°C under a nitrogen atmosphere at a heating rate of 5°C / min and calcined for 3 hours to obtain N-doped carbon-coated LFP.
[0257] Comparative Example 3
[0258] The difference between Comparative Example 3 and Example 1 is that the preparation process of the lithium iron phosphate positive electrode active material is different, and the remaining steps are the same as those in Example 1. Specifically, the preparation process of the lithium iron phosphate positive electrode active material in Comparative Example 3 is as follows:
[0259] (1) Sucrose and lithium iron phosphate with a Dv50 of 300 nm were mixed in a mass ratio of 0.01:100, added to a mixed solution of ethanol and water, and ball-milled for 10 h to uniformly mix the sucrose and lithium iron phosphate. The mixture was then washed with anhydrous ethanol and deionized water and vacuum-dried at 60°C for 12 h to obtain a sucrose-coated lithium iron phosphate precursor. The sucrose-coated lithium iron phosphate precursor was heated to 700°C at a heating rate of 5°C / min under a nitrogen atmosphere and calcined for 3 h to obtain carbon-coated lithium iron phosphate.
[0260] (2) The carbon-coated lithium iron phosphate obtained in (1) was further mixed with sucrose, with the mass ratio of sucrose to the mass of sucrose added in (1) being 2:1, and then added to a mixed solution of ethanol and water for ball milling for 2 hours, and then washed with anhydrous ethanol and deionized water, and then vacuum-dried at 60°C and calcined in nitrogen, wherein the heating rate was 5°C / min, the calcination temperature was 700°C, and the calcination time was 3 hours, and a second carbon coating layer was coated on the outside of the carbon-coated lithium iron phosphate. Finally, the obtained coating was ground to obtain the lithium iron phosphate positive electrode active material of Comparative Example 3.
[0261] Comparative Example 4
[0262] The difference between Comparative Example 4 and Example 1 is that the preparation process of the lithium iron phosphate positive electrode active material is different, and the remaining steps are the same as those in Example 1. Specifically, the preparation process of the lithium iron phosphate positive electrode active material in Comparative Example 4 is as follows:
[0263] (1) Benzylamine and lithium iron phosphate with a Dv50 of 300 nm were mixed in a mass ratio of 0.01:100, added to a mixed solution of ethanol and water, and ball-milled for 10 h. In the mixed solution, the concentration of benzylamine monomer was 0.5 M. 0.5 M hydrochloric acid was added as a doping acid and 1 M ammonium persulfate was added as an initiator to oxidize the benzylamine monomer. The reaction system was then placed in an ice-water bath at 4 ° C and stirred for 14 h. After the reaction, the mixture was washed with anhydrous ethanol and deionized water, respectively, and dried in a vacuum at 60 ° C for 12 h to obtain a polybenzylamine-coated lithium iron phosphate precursor. The polybenzylamine-coated lithium iron phosphate precursor was heated to 700 ° C at a heating rate of 5 ° C / min in a nitrogen atmosphere and calcined for 3 h to obtain N-doped carbon-coated lithium iron phosphate.
[0264] (2) The N-doped carbon-coated lithium iron phosphate obtained in (1) was further added to a mixed solution of ethanol and water for ball milling for 2 h, and then vacuum dried at 60°C for 12 h, and then calcined under a nitrogen atmosphere at a heating rate of 5°C / min, a calcination temperature of 700°C, and a calcination time of 3 h. Finally, the calcined product was ground to obtain the lithium iron phosphate positive electrode active material of Comparative Example 4.
[0265] Comparative Example 5
[0266] The difference between Comparative Example 5 and Example 1 is that step (1) in the preparation process of the lithium iron phosphate positive electrode active material is different, and the remaining steps are the same as those in Example 1. Specifically, step (1) in the preparation process of the lithium iron phosphate positive electrode active material in Comparative Example 5 is as follows:
[0267] (1) Starch and lithium iron phosphate with a Dv50 of 300 nm were mixed in a mass ratio of 0.01:100, added to a mixed solution of ethanol and water, and ball-milled for 10 h to uniformly mix the starch and lithium iron phosphate. The mixture was then washed with anhydrous ethanol and deionized water and vacuum-dried at 60°C for 12 h to obtain a starch-coated lithium iron phosphate precursor. The starch-coated lithium iron phosphate precursor was heated to 700°C at a heating rate of 5°C / min under a nitrogen atmosphere and calcined for 3 h to obtain carbon-coated lithium iron phosphate.
[0268] Comparative Example 6
[0269] The difference between Comparative Example 6 and Example 1 is that step (2) in the preparation process of the lithium iron phosphate positive electrode active material is different, and the remaining steps are the same as those in Example 1. Specifically, step (2) in the preparation process of the lithium iron phosphate positive electrode active material in Comparative Example 6 is as follows:
[0270] (2) The nitrogen-doped carbon-coated lithium iron phosphate obtained in (1) is further mixed with starch, with the mass ratio of starch to the mass of benzylamine added in (1) being 2:1, and then added to a mixed solution of ethanol and water for ball milling for 2 hours, and then washed with anhydrous ethanol and deionized water, and then vacuum-dried at 60°C and calcined in nitrogen, wherein the heating rate is 5°C / min, the calcination temperature is 700°C, and the calcination time is 3 hours, and a second carbon coating layer is coated on the outside of the carbon-coated lithium iron phosphate. Finally, the obtained coating is ground to obtain the lithium iron phosphate positive electrode active material of Comparative Example 6.
[0271] Comparative Example 7
[0272] The difference between Comparative Example 7 and Example 24 is that the positive electrode active material is different, and accordingly, the preparation process of the positive electrode sheet is different. The other steps are the same as Example 24. The preparation process of the positive electrode sheet is as follows:
[0273] Uncoated lithium manganese phosphate was used as the positive electrode active material. Lithium manganese phosphate (Dv50 = 300 nm), NCM (nickel cobalt manganese) ternary positive electrode material (Dv50 = 6 μm), carbon black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a solvent were thoroughly stirred and mixed in a weight ratio of 2.88:92.96:1.47:1.55:1.14 to produce a positive electrode slurry. The slurry was then evenly coated on the positive electrode current collector, followed by drying, cold pressing, and slitting to produce the positive electrode sheet of Comparative Example 7.
[0274] Test part:
[0275] (1) The relevant parameters of the positive electrode active material and the positive electrode sheet are tested as follows:
[0276] 1. Morphology test
[0277] The positive electrode active material was tested using a ZEISS Sigma 300 scanning electron microscope and then tested according to the standard JY / T010-1996 to observe the sample morphology. FIG8 is a SEM image of the positive electrode active material prepared in Example 1.
[0278] 2. Total thickness test of the first carbon coating layer and the second carbon coating layer
[0279] The pre-cold-pressed electrode was cut into 6 cm x 6 cm samples using scissors and polished using an IB-19500CP ion cross-section polisher to obtain polished samples with cut surfaces. The samples were then tested using a ZEISS Sigma 300 in accordance with standard JY / T010-1996. Ten locations were randomly selected from the test sample for testing, and the average values were used to determine the thickness of the first and second carbon coating layers, as well as the total thickness.
[0280] 3. Lattice defect test
[0281] Taking Example 1 as an example, 2 mg of the positive electrode active material prepared in Example 1 was added to 10 mL of ethylene glycol solution for ultrasonic dispersion. The dispersed solution was dropped onto a copper mesh. After drying, the positive electrode active material was observed using a high-resolution transmission electron microscope (HRTEM, JEM-2010). Figure 9 is an HRTEM image of the positive electrode active material prepared in Example 1. It can be seen from the figure that the lattice arrangement at the interface between the first carbon coating layer and the second carbon coating layer is irregular, which proves the presence of lattice defects.
[0282] 4. Tap density test
[0283] Refer to the standard GB / T 5162-2006, use a powder tap density tester (such as Dandong Better BT-300), and use a 25mL graduated cylinder for testing.
[0284] 5. Conductivity test
[0285] The impedance of the powder (pressed into a disc) was measured using an electrochemical workstation. The conductivity of the sample was calculated according to the following formula:
[0286] σ=l / (S×R) (1)
[0287] Where, R is the impedance, Ω; l is the thickness of the disc, cm; S is the cross-sectional area of the disc, cm 2 ;σ-conductivity, S / cm. Before the test, Ag paste was symmetrically scraped on both sides of the sample as a point electrode with an area of 0.5 cm 2 During the test, the AC bias amplitude is 20mV and the frequency range is 10-10 6 Hz.
[0288] 6. Test of lithium ion diffusion coefficient
[0289] Taking the GITT method as an example, the steps for testing the lithium ion diffusion coefficient of the positive electrode active material are as follows:
[0290] The positive electrode active material was ground into a powder microelectrode. This powder microelectrode was connected to an electrochemical workstation and coulometric titration was performed. A 20μA pulse current was used for a 1-hour titration, followed by a 4-hour rest period. (Note: To compare the effects of pulse current and duration, a parallel experiment with 10μA and 10 minutes was performed.) After obtaining the GITT curve, the lithium ion diffusion coefficient was calculated using the following formula:
[0291] Where D is the lithium ion diffusion coefficient; i is the applied current 20 μA; Vm is the molar volume of the positive electrode active material; F is the Faraday constant; A is the electrode surface area, dE / dδ is the slope of the coulomb titration curve, that is, the slope of the open circuit potential at a certain concentration on the Li concentration curve in the electrode; (dE) / (dt 1 / 2 ) is the polarization voltage versus t 1 / 2 The slope of the curve.
[0292] 7. Porosity test
[0293] Taking Example 1 as an example, the process of testing the porosity of the positive electrode sheet is as follows:
[0294] Test Environment: Pre-treatment in a conventional laboratory: Use tweezers to select >20 discs with good appearance and no powder falling from the edges and place them into the sample cup. Record the number of discs and calculate the apparent volume. Test: Place the sample cup containing the sample in the true density tester. Close the test system and introduce helium according to the program. Measure the gas pressure in the sample chamber and expansion chamber. Then calculate the true volume according to Bohr's law (PV = nRT) to obtain the porosity of the sample to be tested. Sample cup volume: 3.5cm 3 .Analytical gas: Helium.
[0295] 8. Element Mapping Test
[0296] Sample preparation: Cut the positive electrode into 5mm×5mm size with scissors and stick it on the sample table with conductive glue;
[0297] Parameter settings: Mode: In-lens, Voltage: 20kv, Aperture: 60μm, Working distance: 8.5mm
[0298] Test process: Select 3 positions for point scanning, refer to the standard GB / T 17359-2012, and use a Hitachi scanning electron microscope HITACHI electron microscope SU390.
[0299] FIG10 is a mapping diagram of the positive electrode sheet prepared in Example 1. As can be seen from FIG10 , lithium iron phosphate is evenly dispersed on the positive electrode sheet.
[0300] (2) Performance test of lithium-ion batteries
[0301] 1. Capacity test
[0302] Taking Example 1 as an example, the battery capacity test process is as follows: At 25°C, the corresponding battery of Example 1 is charged at a constant current of 1 / 3C to 4.25V, then charged at a constant voltage of 4.25V to a current of 0.05C, left for 5 minutes, and then discharged at a constant current of 1 / 3C to 2.8V. The resulting capacity is recorded as the initial capacity C0. The capacity ratio is the ratio of the capacity values obtained in different Examples or Comparative Examples to the capacity value of Example 1.
[0303] 2. Battery capacity retention test
[0304] Taking Example 1 as an example, the battery capacity retention rate test process is as follows: At 25°C, the battery corresponding to Example 1 is charged at a constant current of 1 / 3C to 4.25V, then charged at a constant voltage of 4.25V to a current of 0.05C, left for 5 minutes, and then discharged at 1 / 3C to 2.8V. The resulting capacity is recorded as the initial capacity C0. The above steps are repeated for the same battery, and the discharge capacity Cn of the battery after the nth cycle is recorded at the same time. The battery capacity retention rate after each cycle is Pn = Cn / C0 × 100%. The 190 points P1, P2...P190 are used as the vertical coordinates and the corresponding number of cycles is used as the horizontal coordinates to obtain the curve of the capacity retention rate of the lithium-ion battery of Example 1 and the number of cycles as shown in Figure 11.
[0305] During this test, the first cycle corresponds to n=1, the second cycle corresponds to n=2, and so on and so forth. The battery capacity retention data for Example 1 in Table 1 is the data measured after 190 cycles under the aforementioned test conditions, i.e., the P190 value. The testing procedures for the comparative example and other examples are the same as above.
[0306] 3. DCR DC impedance test
[0307] Taking Example 1 as an example, the DCR DC impedance test process is as follows: at 25°C, the battery corresponding to Example 1 is charged to 4.25V at a constant current of 1 / 3C, the SOC is adjusted to 50% at a rate of 1 / 3C, and then pulse-discharged at a constant current of 4C for 30s, and left for 5 minutes. The ratio of the voltage difference before and after the pulse discharge to the current difference is the DCR DC impedance value.
[0308] 4. Energy density test
[0309] At room temperature, charge to 4.2V at 0.33C standard, charge to 0.05C at 4.2V constant voltage, let it stand for 10 minutes, and then discharge to 2.8V at 0.33C. Record the discharge energy and then calculate the energy density during discharge.
[0310] Energy density (Wh / L) = discharge energy (Wh) / lithium-ion secondary battery volume (L)
[0311] The process parameters and test data in the preparation process of the above examples and comparative examples are shown in Tables 1 and 2 below:
[0312] Table 1
[0313]
[0314]
[0315] As can be seen from Table 1, the thickness ratios of the first carbon coating layer and the second carbon coating layer in Examples 1 to 7 are different. By adjusting the thickness ratio of the first carbon coating layer and the second carbon coating layer, the tap density, electrical conductivity and lithium ion diffusion coefficient of the lithium iron phosphate positive electrode material can be further improved.
[0316] The total thickness of the first carbon coating layer and the second carbon coating layer in Examples 8 to 9 is different from that in Example 1. The total thickness will affect the conductive properties, and further affect electron transfer and ion diffusion.
[0317] The calcination temperatures of Examples 10 to 14 were different from those of Example 1, and the calcination times of Examples 15 to 19 were different from those of Example 1. As can be seen from Table 1, the calcination temperature and calcination time affect the ion diffusivity and electrical conductivity of the positive electrode active material. Appropriate calcination temperature and calcination time can make the lattice defects at the interface between the first carbon coating layer and the second carbon coating layer more uniform, thereby improving the electrical properties of the coated positive electrode active material.
[0318] In Comparative Example 1, the lithium iron phosphate was not coated, the positive electrode active material of Comparative Example 2 was only coated with one layer, and Comparative Example 3 adopted conventional double-layer coating. The tap density, electrical conductivity and ion diffusion coefficient of the positive electrode active materials of Comparative Example 1, Comparative Example 2 and Comparative Example 3 were significantly lower than those of the embodiment.
[0319] Table 2
[0320]
[0321] As can be seen from Table 2, Example 20 differs from Example 1 in that Example 20 is directly coated with polybenzylamine without starting from polymerization. The carbon layer directly coated with polybenzylamine may not be as dense as the carbon layer obtained by monomer polymerization, resulting in a larger DCR value, thereby affecting the capacity value. However, the performance is still better than that of the comparative example.
[0322] The materials used in the coating layers of Examples 21 to 23 are different from those of Example 1, and their electrical performance is better than that of Comparative Example 1, indicating that using other substances with a serrated spatial structure as carbon sources to coat the surface of the positive electrode active material matrix can also improve battery performance.
[0323] The positive electrode active material matrix used in Example 24 is different from that in Example 1, and the electrical performance is better than that of Comparative Example 7, indicating that the use of other positive electrode active material matrices can also improve battery performance.
[0324] The Dv50 of the positive electrode active material matrix used in Examples 25 to 26 is different from that in Example 1, and the electrical performance is better than that of Comparative Example 1, indicating that the use of positive electrode active material matrices of different sizes can also improve battery performance.
[0325] Compared with Example 1, in Examples 27 to 31, different proportions of LFP particles are added when making the positive electrode sheets. The mass ratio of LFP to NCM will affect the capacity of the battery cell to a certain extent. Therefore, it is necessary to select an appropriate amount of LFP and ternary particles.
[0326] Examples 32 to 34 have different injection coefficients from Example 1. As the injection coefficient decreases, the capacity and cycle retention rate of the battery cell will also decrease. When the injection coefficient is 2.15 g / Ah, the capacity and cycle retention rate are basically the same as those in Example 1, but the amount of electrolyte used is reduced, and the energy density increases from 201Wh / L to 203Wh / L, which is beneficial to improving the energy density of the battery cell.
[0327] The positive electrode active material of Comparative Example 1 is not carbon-coated, the positive electrode active material of Comparative Example 2 is only coated with one layer, and the positive electrode active material of Comparative Example 3 is coated with a traditional carbon coating layer. The capacity retention rate, DCR value and energy density of Comparative Examples 1, 2 and 3 are significantly lower than those of the embodiment.
[0328] The positive electrode active material of Comparative Example 4 was coated once with polybenzylamine having a zigzag spatial structure as a carbon source, but after two calcinations, the capacity retention rate of the prepared battery was significantly lower. This is because when there is only one carbon coating layer, even after two calcinations, lattice defects cannot be formed, and the lithium ion diffusion rate and electron conductivity are lower.
[0329] The molecules of the first carbon source in Comparative Example 5 do not have a serrated spatial structure, and the molecules of the second carbon source in Comparative Example 6 do not have a serrated spatial structure. The capacity retention rates of the positive electrode active materials of Comparative Examples 5 and 6 are significantly lower. This is because when one of the molecules of the first carbon source and the molecules of the second carbon source does not have a serrated spatial structure, no lattice defects are formed at the interface between the first carbon coating layer and the second carbon coating layer, and the lithium ion diffusion rate and the electron conductivity are lower.
[0330] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0331] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, and such modifications and improvements are all within the scope of protection of the present application. Therefore, the scope of protection of the present application shall be determined by the appended claims.
Claims
1. A positive electrode active material comprising: A positive electrode active material matrix, a first carbon coating layer, and a second carbon coating layer. The first carbon coating layer covers the surface of the positive electrode active material matrix, and the second carbon coating layer covers the surface of the first carbon coating layer; There are lattice defects at the interface between the first carbon coating layer and the second carbon coating layer, and the second carbon coating layer has a serrated surface.
2. The positive electrode active material according to claim 1, characterized in that The lattice defects include line defects.
3. The positive electrode active material according to any one of claims 1 to 2, characterized in that The second carbon coating layer has an atomic-level serrated surface.
4. The positive electrode active material according to any one of claims 1 to 3, characterized in that At least one of the first carbon coating layer and the second carbon coating layer is a nitrogen-doped carbon layer.
5. The positive electrode active material according to any one of claims 1 to 4, characterized in that The total thickness of the first carbon coating layer and the second carbon coating layer is 10 nm to 30 nm.
6. The positive electrode active material according to any one of claims 1 to 5, characterized in that The thickness ratio of the first carbon coating layer to the second carbon coating layer is (1 to 10):(1 to 5).
7. The positive electrode active material according to any one of claims 1 to 6, characterized in that The positive electrode active material matrix includes at least one of lithium iron phosphate, lithium manganese phosphate, and lithium manganese iron phosphate.
8. The positive electrode active material according to any one of claims 1 to 7, characterized in that The volume average particle size Dv50 of the positive electrode active material matrix is 100 nm to 500 nm.
9. A preparation method of a positive electrode active material, comprising the following steps: Coat a first carbon source on the surface of the positive electrode active material matrix, and perform a first calcination to obtain a carbon-coated matrix; Coat a second carbon source on the surface of the carbon-coated matrix, and perform a second calcination; The molecules of the first carbon source and the second carbon source both have a serrated spatial structure.
10. The method for preparing a positive electrode active material according to claim 9, characterized in that: Both the first carbon source and the second carbon source include components with a conjugated molecular structure.
11. The method for preparing a positive electrode active material according to any one of claims 9 to 10, characterized in that: Both the first carbon source and the second carbon source include materials with the following structure: -(A-B-A) n -, Where n is an integer, A includes at least one of an aromatic group and an alkenyl group, B includes an N atom, and 90° < bond angle of A - B - A < 180°.
12. The method for preparing a positive electrode active material according to any one of claims 9 to 11, characterized in that: The first carbon source and the second carbon source each independently include at least one of polybenzylamine, polyaniline, polypyrrole, and polyethylene diamine.
13. The method for preparing a positive electrode active material according to any one of claims 9 to 12, characterized in that: The mass ratio of the first carbon source to the positive electrode active material matrix is (0.001 to 0.5):100; Optionally, the mass ratio of the first carbon source to the positive electrode active material matrix is (0.003 to 0.2):100; Optionally, the mass ratio of the first carbon source to the positive electrode active material matrix is (0.01 to 0.2):
100.
14. The method for preparing a positive electrode active material according to any one of claims 9 to 13, characterized in that: The mass ratio of the first carbon source to the second carbon source is (1 to 10):(1 to 5).
15. The method for preparing a positive electrode active material according to any one of claims 9 to 14, characterized in that: The temperatures of the first calcination and the second calcination are each independently 200°C to 1000°C; Optionally, the temperatures of the first calcination and the second calcination are each independently 600°C to 800°C.
16. The method for preparing a positive electrode active material according to any one of claims 9 to 15, characterized in that: The times of the first calcination and the second calcination are each independently 17. The method for preparing a positive electrode active material according to any one of claims 9 to 16, characterized in that: The monomers are mixed with the core material and ball-milled, and then a doping acid and an initiator are added to polymerize the monomers to form a carbon source coating the core material on the surface of the core material. The core material is the positive electrode active material matrix or the carbon-coated matrix, and the carbon source is the first carbon source or the second carbon source.
18. The method for preparing a positive electrode active material according to claim 17, characterized in that: The doping acid includes at least one of hydrochloric acid, sulfuric acid and nitric acid.
19. The method for preparing a positive electrode active material according to any one of claims 17 to 18, characterized in that: The initiator includes at least one of ammonium persulfate, potassium persulfate and sodium persulfate.
20. The method for preparing a positive electrode active material according to any one of claims 17 to 19, characterized in that: The molar ratio of the doping acid, the initiator and the monomer is (1-3):(0.5-2.5):(1-5).
21. The method for preparing a positive electrode active material according to any one of claims 17 to 20, characterized in that: In the process of coating the first carbon source on the surface of the positive electrode active material matrix and coating the second carbon source on the surface of the carbon-coated matrix, the steps of polymerizing the monomers independently include: The monomer, the core material, the doping acid and the initiator are reacted at 4° C. to 10° C. for 14 to 18 hours, and then washed and vacuum dried at 60° C. to 80° C. for 12 to 18 hours.
22. The method for preparing a positive electrode active material according to any one of claims 9 to 16, characterized in that: The coating of the first carbon source on the surface of the positive electrode active material matrix and the coating of the second carbon source on the surface of the carbon-coated matrix each independently include: The carbon source and the core material are mixed and ball-milled for 10 to 16 hours, then washed, and vacuum-dried at 60 to 80 degrees Celsius for 12 to 18 hours, wherein the carbon source is the first carbon source or the second carbon source, and the core material is the positive electrode active material matrix or the carbon-coated matrix.
23. The method for preparing a positive electrode active material according to any one of claims 9 to 22, characterized in that: The positive electrode active material matrix includes at least one of lithium iron phosphate, lithium manganese phosphate and lithium manganese iron phosphate.
24. The method for preparing a positive electrode active material according to any one of claims 9 to 23, characterized in that: The volume average particle size Dv50 of the positive electrode active material matrix is 100 nm to 500 nm.
25. A positive electrode plate, comprising: positive electrode current collector; as well as A positive electrode active material layer, the positive electrode active material layer is located on at least one surface of the positive electrode current collector, the positive electrode active material layer comprises the positive electrode active material according to any one of claims 1 to 8 or the positive electrode active material prepared by the method for preparing the positive electrode active material according to any one of claims 9 to 24.
26. The positive electrode sheet according to claim 25, characterized in that: The positive electrode active material matrix includes at least one of lithium iron phosphate, lithium manganese phosphate and lithium manganese iron phosphate, and the positive electrode active material layer also includes a ternary positive electrode material, the molecular formula of the ternary positive electrode material is LiNi x Co y Mn 1-x-y O2, x>0, y>0, or LiNi 0.8+a+b Co 0.15-a Al 0.05-b O2, 0≤a<0.15, 0≤b<0.
05.
27. The positive electrode sheet according to claim 26, characterized in that: The mass ratio of the positive electrode active material to the ternary positive electrode material is (0.1-20):100; Optionally, the mass ratio of the positive electrode active material to the ternary positive electrode material is (0.1-10):
100.
28. The positive electrode sheet according to any one of claims 26 to 27, characterized in that: The ratio of the volume average particle size Dv50 of the positive electrode active material to the volume average particle size Dv50 of the ternary positive electrode material is (0.1-20):100; Optionally, the ratio of the volume average particle size Dv50 of the positive electrode active material to the volume average particle size Dv50 of the ternary positive electrode material is (0.1-12):
100.
29. The positive electrode sheet according to any one of claims 25 to 28, characterized in that: The porosity of the positive electrode sheet is 20% to 25%.
30. A secondary battery comprising the positive electrode sheet according to any one of claims 25 to 29.
31. The secondary battery according to claim 30, characterized in that The secondary battery has a liquid filling coefficient of 2.1 g / Ah to 2.2 g / Ah.
32. A battery module comprising the secondary battery according to any one of claims 30 to 31.
33. A battery pack comprising the battery module according to claim 32.
34. An electrical device comprising at least one selected from the group consisting of the secondary battery according to any one of claims 30 to 31, the battery module according to claim 32, and the battery pack according to claim 33.
Citation Information
Patent Citations
Cathode material having double-layer carbon coating and preparation method therefor
CN103347813A
Composite cathode material, preparation method thereof, lithium ion secondary battery negative plate and lithium ion secondary battery
CN105098185A
Preparation method of N-doped mesoporous carbon-coated ternary cathode material of lithium ion battery
CN107732220A
Double-layer carbon-coated lithium iron phosphate composite material and preparation method thereof
CN110265647A
Nonaqueous electrolyte secondary battery
US20200403221A1