Antibacterial protective film for high-frequency contact surface and preparation method thereof

By using a thorn-shaped core-shell structure fiber membrane of metal peroxide nanoparticles and quaternized chitosan on high-frequency contact surfaces, the problem that high-frequency contact surfaces cannot block the spread of bacteria in a short time is solved, and real-time sterilization and Effective in preventing the spread of bacteria.

CN118743773AActive Publication Date: 2024-10-08XIAN UNIV OF TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410810341.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-08
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing high-touch surfaces cannot block the spread of bacteria in a short time. Traditional disinfection methods have volatile odors that are irritating and harmful to the body. Antibacterial agents that rely on ultraviolet irradiation have limited effectiveness on contact surfaces in public places.

Method used

Metal peroxide nanoparticles and quaternized chitosan are used as shell materials, and polyvinyl alcohol is used as core material. An antibacterial protective film with a thorn-like core-shell structure is constructed through coaxial electrospinning, using electrostatic attraction and reactive oxygen species. Release to achieve rapid sterilization.

Benefits of technology

Effectively captures and inactivates bacteria in a short time, blocks the spread of bacteria, and does not rely on liquid environment or ultraviolet irradiation, providing real-time sterilization effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743773A_ABST
    Figure CN118743773A_ABST
Patent Text Reader

Abstract

The invention discloses an antibacterial protective film for a high-frequency contact surface and a preparation method thereof, and the preparation method specifically comprises the following steps: taking metal peroxide nanoparticles and quaternized chitosan as shell materials, taking polyvinyl alcohol as a core material, carrying out coaxial electrostatic spinning and crosslinking, and finally drying to obtain the antibacterial protective film for the high-frequency contact surface. The antibacterial protective film for the high-frequency contact surface with a core-shell structure and thorn-shaped fiber morphology is constructed, quaternized chitosan half-coated metal peroxide particles are used as a shell spine material, quaternized chitosan and the metal peroxide particles are synergistically antibacterial, polyvinyl alcohol is used as a flexible core material, and the antibacterial protective film for the high-frequency contact surface with the core-shell structure and thorn-shaped fiber morphology is prepared. Effective antibacterial components are concentrated on the fiber surface, and the problem that an existing high-frequency contact surface cannot block bacterial propagation in a short time is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fiber membrane preparation, and in particular relates to a method for preparing an antibacterial protective membrane for a high-frequency contact surface, and also relates to the antibacterial protective membrane for a high-frequency contact surface. Background Art

[0002] Daily disinfection of public places mostly adopts the method of spraying disinfectant regularly. The effective bactericidal ingredients in the disinfectant, such as sodium hypochlorite, will evaporate into the air along with the alcohol, and the smell is irritating and harmful to the body. The traditional method of spraying disinfectant regularly will wet the surface of objects, emit irritating odors, and is limited by the spraying frequency. It cannot achieve real-time sterilization to block the spread of bacteria. The most effective way to deal with the above practical problems is to cover the high-frequency contact surface with an antibacterial protective film that can sterilize in real time. On the basis of protecting the surface of objects and not volatile harmful gases, it can achieve the goal of real-time rapid adsorption of bacteria to block the spread of bacteria and inactivate them.

[0003] Chinese patent "A template-free chitosan@inorganic SiO 2 Nanofiber aerogel and its preparation method and application" (Application No.: 202310603535.7, Publication No.: CN116651406A, Publication Date: 2023-08-29) discloses a template-free chitosan@inorganic SiO 2Nanofiber aerogel and its preparation method and application have three antibacterial effects of adsorption / complexation / contact, but the antibacterial component is single, which limits its sterilization rate in a short time and cannot achieve real-time sterilization. The Chinese patent "An antibacterial and oil-proof high-barrier self-assembled film and its preparation method and application" (application number: 202311116298.8, publication number: CN117050363A, publication date: 2023.11.14) discloses an antibacterial and oil-proof high-barrier self-assembled film and its preparation method and application, which can effectively improve the waterproof, oil-proof, barrier and other properties, and introduce composite antibacterial agents to improve the antibacterial properties, but nano titanium dioxide is a photocatalyst, and its antibacterial properties depend on ultraviolet irradiation. It is difficult to ensure that high-frequency contact surfaces in public places such as elevator buttons, door handles, counters, etc. receive sufficient ultraviolet light, and the antibacterial effect is inhibited. The Chinese patent "An antibacterial fiber membrane with in-situ patterned release of peroxide and its preparation method" (application number: 202311041833.8, publication number: CN117071180A, publication date: 2023-11-17) discloses an antibacterial fiber membrane with in-situ patterned release of peroxide and its preparation method. When the antibacterial fiber membrane comes into contact with the wound surface, the soluble polymer contained in the fiber shell dissolves, and a nano-groove structure is formed in situ patterned on the fiber surface, which is conducive to cell adhesion and proliferation along the fiber direction. At the same time, the metal peroxide nanoparticles in the fiber shell are quickly released, and the bactericidal and angiogenesis-promoting effects are simultaneously achieved. However, it still needs to rely on a large amount of liquid environment to release metal peroxides to achieve antibacterial effects. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing an antibacterial protective film for high-frequency contact surfaces, so as to solve the problem that the existing high-frequency contact surfaces cannot block the spread of bacteria in a short time.

[0005] Another object of the present invention is to provide an antibacterial protective film for the above-mentioned high-frequency contact surface.

[0006] The technical solution adopted by the present invention is a method for preparing an antibacterial protective film for high-frequency contact surfaces, using metal peroxide nanoparticles and quaternized chitosan as shell materials, polyvinyl alcohol as core material, coaxial electrospinning, cross-linking, and finally drying to obtain the antibacterial protective film for high-frequency contact surfaces.

[0007] The present invention is also characterized in that:

[0008] Follow the steps below to implement it:

[0009] Step 1, preparing a shell precursor of an antibacterial protective film for high-frequency contact surfaces; specifically:

[0010] Step 1.1, dissolving quaternized chitosan and polyvinyl alcohol in deionized water, heating in a water bath with stirring, and cooling to room temperature to obtain a quaternized chitosan solution;

[0011] Step 1.2, dissolve the metal salt and polyvinyl pyrrolidone in deionized water, add NaOH aqueous solution under stirring in an ice-water bath at 0-2°C, and then add H 2 O 2 The solution is stirred in an ice-water bath for 20-40 minutes, and then washed by centrifugation with ethanol for multiple times, and then added to the quaternary ammonium chitosan solution and stirred for 4-6 hours to obtain quaternary ammonium chitosan-coated metal peroxide nanoparticles, which are the shell precursors of the antibacterial protective film for high-frequency contact surfaces;

[0012] Step 2, dissolving polyvinyl alcohol in deionized water, heating and stirring in a water bath, to obtain a core precursor of an antibacterial protective film for high-frequency contact surfaces;

[0013] Step 3, constructing an antibacterial protective film for high-frequency contact surfaces with a thorn-shaped core-shell structure;

[0014] Step 3.1, placing the precursor of the shell layer of the high-frequency contact surface antibacterial protective film prepared in step 1 in the shell layer extrusion device of the electrospinning device, placing the core precursor of the high-frequency contact surface antibacterial protective film prepared in step 2 in the core layer extrusion device of the electrospinning device, and performing coaxial electrospinning to obtain a composite nanofiber membrane;

[0015] Step 3.2, dissolving the glutaraldehyde solution in anhydrous ethanol to obtain a glutaraldehyde cross-linking solution with a volume concentration of 4-6%, placing the dried composite nanofiber membrane in the glutaraldehyde cross-linking solution, heating in a water bath for cross-linking, and drying the cross-linked composite nanofiber membrane for 10-20 minutes to obtain a high-frequency contact surface antibacterial protective film with a thorn-like core-shell structure.

[0016] In step 1.1, the heating and stirring temperature is 70-90° C., and the heating and stirring time is 2-3 h; the mass ratio of quaternized chitosan, polyvinyl alcohol and deionized water is 0.1-0.15:0.4-0.6:10-15.

[0017] In step 1.2, the metal salt is at least one of cupric chloride dihydrate and silver nitrate; the mass ratio of the metal salt, polyvinyl pyrrolidone and deionized water is 0.15-0.2:1-1.5:50-70.

[0018] In step 2, the heating and stirring temperature is 70-90° C., and the heating and stirring time is 2-3 h.

[0019] In step 3.1, during electrospinning: the voltage was set to 18 kV, the injection speed was set to 0.0003 mm / s-0.0006 mm / s, the distance between the spinneret and the collecting plate was 20 cm, and the spinning time was 4.5 h.

[0020] In step 3.2, the heating temperature is 50-60°C and the heating time is 35-45 min.

[0021] Another technical solution adopted by the present invention is that the antibacterial protective film for high-frequency contact surface is prepared by the above method.

[0022] The beneficial effects of the present invention are:

[0023] 1. The present invention exposes metal peroxide nanoparticles on the fiber surface to form a thorn-like fiber morphology, and achieves uniform distribution of metal peroxide nanoparticles and quaternized chitosan on the fiber surface. When the skin surface (such as the finger pulp) contacts the antibacterial protective film, on the one hand, a large number of positively charged amino groups on the quaternized chitosan molecules and negatively charged bacteria generate electrostatic attraction to capture bacteria, which can effectively prevent bacteria from falling off and spreading, while also having bactericidal ability; on the other hand, secretions such as sweat on the skin surface are weakly acidic, which can induce metal peroxide nanoparticles to react with water molecules in a humid environment, releasing metal ions and a large number of reactive oxygen species (ROS) such as hydrogen peroxide and hydroxyl free radicals. The oxidative stress caused by excessive ROS can destroy biological molecules, such as proteins, lipids, RNA and DNA, thereby inactivating bacteria on high-frequency contact surfaces in a short time. The two work together to inactivate bacteria in a short time, thereby blocking the transmission path of bacteria on high-frequency contact surfaces.

[0024] 2. The present invention constructs an antibacterial fiber membrane for high-frequency contact surfaces with a thorn-like core-shell structure, wherein the shell layer is a functional part that has adsorption and antibacterial effects, and quaternary ammonium chitosan semi-coated metal peroxide particles are used as the shell layer spike material of the antibacterial fiber membrane for high-frequency contact surfaces. The quaternary ammonium chitosan and the metal peroxide particles form a semi-coated structure. The cationic properties of the quaternary ammonium chitosan can both adsorb bacteria and have antibacterial ability, and work synergistically with the metal peroxide to achieve adsorption and rapid inactivation of bacteria, effectively blocking the spread of bacteria on high-frequency contact surfaces; the core portion mainly functions to improve mechanical properties, and polyvinyl alcohol is used as the flexible core material of the antibacterial fiber membrane for high-frequency contact surfaces, which not only supports the shell layer, but also improves the spinning performance and flexibility of the fiber membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a schematic diagram of the structure of the antibacterial protective film for high-frequency contact surfaces of Example 1;

[0026] Figure 2is the antibacterial activity of the antibacterial protective film of each embodiment when it is in contact with bacteria for 1 hour;

[0027] Figure 3 This is a detection diagram of hydrogen peroxide produced by the antibacterial protective film of Example 1. DETAILED DESCRIPTION

[0028] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0029] The method for preparing the antibacterial protective film for high-frequency contact surfaces of the present invention uses metal peroxide nanoparticles and quaternized chitosan as shell materials, polyvinyl alcohol as core material, performs coaxial electrostatic spinning, performs cross-linking, and finally obtains the antibacterial protective film for high-frequency contact surfaces through drying.

[0030] Follow the steps below to implement it:

[0031] Step 1, preparing a shell precursor of an antibacterial protective film for high-frequency contact surfaces;

[0032] Step 1.1, dissolving quaternized chitosan and polyvinyl alcohol in deionized water, heating in a water bath with stirring, and cooling to room temperature to obtain a quaternized chitosan solution;

[0033] The heating and stirring temperature is 70-90°C, and the heating and stirring time is 2-3h;

[0034] The mass ratio of quaternized chitosan, polyvinyl alcohol and deionized water is 0.1-0.15:0.4-0.6:10-15;

[0035] Step 1.2, dissolve the metal salt and polyvinyl pyrrolidone in deionized water, add 0.15 mol / L NaOH aqueous solution under the condition of 0-2℃ ice water bath, and then add H 2 O 2 The solution is stirred in an ice-water bath for 20-40 minutes, and then washed by centrifugation with ethanol for multiple times, and then added to the quaternary ammonium chitosan solution and stirred for 4-6 hours to obtain quaternary ammonium chitosan-coated metal peroxide nanoparticles, which are the shell precursors of the antibacterial protective film for high-frequency contact surfaces;

[0036] The metal salt is at least one of cupric chloride dihydrate and silver nitrate;

[0037] The mass ratio of metal salt, polyvinyl pyrrolidone and deionized water is 0.15-0.2:1-1.5:50-70;

[0038] The concentration of NaOH aqueous solution is 0.15 mol / L; H 2 O 2 The volume concentration of the solution was 3%. To ensure sufficient reaction, excess NaOH aqueous solution and H2 O 2 The volume of NaOH aqueous solution is 15-25 mL, calculated based on 2.5-3 times the amount of metal salt; the volume of H 2 O 2 The solution volume is 95-115mL.

[0039] Step 2, preparing a core precursor of an antibacterial protective film for high-frequency contact surfaces;

[0040] Dissolving polyvinyl alcohol in deionized water, heating and stirring in a water bath, and preparing a core precursor of an antibacterial protective film for high-frequency contact surfaces;

[0041] The heating and stirring temperature is 70-90°C, and the heating and stirring time is 2-3h;

[0042] The mass fraction of polyvinyl alcohol is 8%-10%;

[0043] Step 3, constructing an antibacterial protective film for high-frequency contact surfaces with a thorn-shaped core-shell structure;

[0044] Step 3.1, placing the precursor of the shell layer of the high-frequency contact surface antibacterial protective film prepared in step 1 in the shell layer extrusion device of the electrospinning device, placing the core precursor of the high-frequency contact surface antibacterial protective film prepared in step 2 in the core layer extrusion device of the electrospinning device, and performing coaxial electrospinning to obtain a composite nanofiber membrane;

[0045] During electrospinning: the voltage was set to 18 kV, the injection speed was set to 0.0003 mm / s-0.0006 mm / s, the distance between the spinneret and the collecting plate was 20 cm, and the spinning time was 4.5 h;

[0046] Step 3.2, dissolving the glutaraldehyde solution in anhydrous ethanol to obtain a glutaraldehyde cross-linking solution with a volume concentration of 4-6%, placing the dried composite nanofiber membrane in the glutaraldehyde cross-linking solution, heating in a water bath for cross-linking, and drying the cross-linked composite nanofiber membrane for 10-20 minutes to obtain a high-frequency contact surface antibacterial protective film with a thorn-like core-shell structure;

[0047] The heating temperature is 50-60°C and the heating time is 35-45 minutes.

[0048] The volume concentration of glutaraldehyde solution is 50%;

[0049] The present invention constructs an antibacterial protective film for high-frequency contact surfaces with a core-shell structure and a thorn-like fiber morphology, uses quaternary ammonium chitosan to semi-coat metal peroxide particles as shell spike materials, and quaternary ammonium chitosan and metal peroxide particles synergistically have antibacterial effects. Polyvinyl alcohol is used as a flexible core material, so that effective antibacterial components are concentrated on the fiber surface, thereby solving the problem that existing high-frequency contact surfaces cannot block the spread of bacteria in a short time.

[0050] Example 1

[0051] Weigh 0.15g of quaternized chitosan and 0.5g of polyvinyl alcohol and dissolve them in 15mL of deionized water. Heat in a water bath at 70℃ and stir for 3h. Cool to room temperature. Weigh 0.2g of cupric chloride dihydrate and 1.5g of polyvinyl pyrrolidone and dissolve them in 70mL of deionized water. Heat in an ice water bath at 0-2℃ and stir. Add 25mL of 0.15mol / L NaOH aqueous solution. Add 3% H 2 O 2 The solution was 115 mL and stirred in an ice-water bath for 40 minutes. After multiple centrifugal washings with ethanol, it was added to the cooled quaternized chitosan solution and stirred for 6 hours to obtain the metal peroxide nanoparticles coated with quaternized chitosan as the shell precursor of the antibacterial protective film for high-frequency contact surfaces, and then placed in the shell extrusion device of the electrospinning device. Then 1 g of polyvinyl alcohol was weighed and dissolved in 10 mL of deionized water, heated in a water bath at 70 ° C and stirred for 3 hours to obtain the flexible core precursor of the antibacterial protective film for high-frequency contact surfaces, and then placed in the core extrusion device of the electrospinning device. The voltage was set to 18 kV, the injection speed was set to 0.0003 mm / s, the distance between the spinneret and the collecting plate was 20 cm, and coaxial electrospinning was performed for 4.5 hours. Finally, in a fume hood, glutaraldehyde crosslinking liquid was prepared, 5 mL of 50% glutaraldehyde solution was dissolved in 45 mL of anhydrous ethanol to obtain a 5% glutaraldehyde crosslinking liquid, the fiber membrane obtained by spinning was dried and placed in 50 mL of the crosslinking liquid, and heated in a water bath at 55°C for 40 minutes. The crosslinked composite nanofiber membrane was dried at room temperature for 20 minutes to obtain an antibacterial protective film for high-frequency contact surfaces.

[0052] Example 2

[0053] Weigh 0.12g of quaternized chitosan and 0.5g of polyvinyl alcohol and dissolve them in 13mL of deionized water. Heat in a water bath at 85℃ and stir for 2.5h. Cool to room temperature. Weigh 0.19g of silver nitrate and 1.4g of polyvinyl pyrrolidone and dissolve them in 66mL of deionized water. Heat in an ice water bath at 0-2℃ and stir. Add 23mL of 0.15mol / L NaOH aqueous solution. Add 3% H 2 O 2The solution was 111 mL and stirred in an ice-water bath for 30 minutes. After multiple centrifugal washings with ethanol, it was added to the cooled quaternized chitosan solution and stirred for 5.5 hours to obtain the metal peroxide nanoparticles coated with quaternized chitosan as the shell precursor of the antibacterial protective film for high-frequency contact surfaces, and then placed in the shell extrusion device of the electrospinning equipment. Then 1g of polyvinyl alcohol was weighed and dissolved in 10mL of deionized water, heated to 85°C in a water bath and stirred for 2.5 hours to obtain the flexible core precursor of the antibacterial protective film for high-frequency contact surfaces, and then placed in the core extrusion device of the electrospinning equipment. The voltage was set to 18kV, the injection speed was set to 0.0003mm / s, the distance between the spinneret and the collecting plate was 20cm, and coaxial electrospinning was performed for 4.5 hours. Finally, in a fume hood, glutaraldehyde crosslinking liquid was prepared, 5 mL of 50% glutaraldehyde solution was dissolved in 45 mL of anhydrous ethanol to prepare a 5% glutaraldehyde crosslinking liquid, the fiber membrane obtained by spinning was dried and placed in 50 mL of the crosslinking liquid, and heated in a water bath at 50°C for 45 minutes. The crosslinked composite nanofiber membrane was dried at room temperature for 15 minutes to obtain an antibacterial protective film for high-frequency contact surfaces.

[0054] Example 3

[0055] Weigh 0.13g of quaternized chitosan and 0.4g of polyvinyl alcohol and dissolve them in 11mL of deionized water. Heat in a water bath at 80℃ and stir for 2.5h. Cool to room temperature. Weigh 0.17g of cupric chloride dihydrate and 1.25g of polyvinyl pyrrolidone and dissolve them in 60mL of deionized water. Heat in an ice water bath at 0-2℃ and stir. Add 20mL of 0.15mol / L NaOH aqueous solution. Add 3% H 2 O 2The solution was 105 mL and stirred in an ice-water bath for 30 minutes. After centrifugation and washing with ethanol several times, it was added to the cooled quaternized chitosan solution and stirred for 5 hours to obtain the quaternized chitosan-coated metal peroxide nanoparticles as the shell precursor of the antibacterial protective film for high-frequency contact surfaces, and then placed in the shell extrusion device of the electrospinning equipment. Then 0.9 g of polyvinyl alcohol was weighed and dissolved in 10 mL of deionized water, heated to 80 ° C in a water bath and stirred for 2.5 hours to obtain the flexible core precursor of the antibacterial protective film for high-frequency contact surfaces, and then placed in the core extrusion device of the electrospinning equipment. The voltage was set to 18 kV, the injection speed was set to 0.0004 mm / s, the distance between the spinneret and the collecting plate was 20 cm, and coaxial electrospinning was performed for 4.5 hours. Finally, in a fume hood, prepare glutaraldehyde crosslinking liquid, take 8 mL of 50% glutaraldehyde solution and dissolve it in 42 mL of anhydrous ethanol to obtain 6% glutaraldehyde crosslinking liquid, place the composite nanofiber membrane dried in step 4 in 50 mL of crosslinking liquid, heat it in a water bath at 60°C for 35 minutes. Dry the crosslinked composite nanofiber membrane at room temperature for 20 minutes to obtain an antibacterial protective film for high-frequency contact surfaces.

[0056] Example 4

[0057] Weigh 0.10g of quaternized chitosan and 0.6g of polyvinyl alcohol and dissolve them in 10mL of deionized water. Heat in a water bath at 75℃ and stir for 2h. Cool to room temperature. Weigh 0.16g of cupric chloride dihydrate and 1.1g of polyvinyl pyrrolidone and dissolve them in 55mL of deionized water. Heat in an ice water bath at 0-2℃ and stir. Add 18mL of 0.15mol / L NaOH aqueous solution. Add 3% H 2 O 2The solution was stirred in an ice-water bath for 25 minutes, then washed by centrifugation with ethanol several times, and then added to the cooled quaternized chitosan solution and stirred for 4.5 hours to obtain the metal peroxide nanoparticles coated with quaternized chitosan as the shell precursor of the antibacterial protective film for high-frequency contact surfaces, and then placed in the shell extrusion device of the electrospinning equipment. Then 0.8g of polyvinyl alcohol was weighed and dissolved in 10mL of deionized water, heated in a water bath at 75°C and stirred for 3 hours to obtain the flexible core precursor of the antibacterial protective film for high-frequency contact surfaces, and then placed in the core extrusion device of the electrospinning equipment. The voltage was set to 18kV, the injection speed was set to 0.0005mm / s, the distance between the spinneret and the collecting plate was 20cm, and coaxial electrospinning was performed for 4.5 hours. Finally, in a fume hood, prepare glutaraldehyde crosslinking liquid, take 5 mL of 50% glutaraldehyde solution and dissolve it in 45 mL of anhydrous ethanol to prepare 5% glutaraldehyde crosslinking liquid, place the composite nanofiber membrane dried in step 4 in 50 mL of crosslinking liquid, heat it in a water bath at 55°C for 40 minutes. Dry the crosslinked composite nanofiber membrane at room temperature for 15 minutes to obtain an antibacterial protective film for high-frequency contact surfaces.

[0058] Example 5

[0059] Weigh 0.11g of quaternized chitosan and 0.6g of polyvinyl alcohol and dissolve them in 10mL of deionized water. Heat in a water bath at 90℃ and stir for 2h. Cool to room temperature. Weigh 0.15g of cupric chloride dihydrate and 1g of polyvinyl pyrrolidone and dissolve them in 50mL of deionized water. Place in an ice water bath at 0-2℃ and stir. Add 15mL of 0.15mol / L NaOH aqueous solution. Add 3% H 2 O 295mL of solution was stirred in an ice-water bath for 20min, and then centrifuged and washed with ethanol several times, and then added to the cooled quaternized chitosan solution and stirred for 4h to obtain quaternized chitosan-coated metal peroxide nanoparticles as the shell precursor of the antibacterial protective film for high-frequency contact surfaces, and then placed in the shell extrusion device of the electrospinning equipment. Then weigh 0.8g of polyvinyl alcohol and dissolve it in 10mL of deionized water, heat it in a water bath at 90℃ and stir it for 2h to obtain the flexible core precursor of the antibacterial protective film for high-frequency contact surfaces, and then place it in the core extrusion device of the electrospinning equipment. The voltage was set to 18kV, the injection speed was set to 0.0006mm / s, the distance between the spinneret and the collecting plate was 20cm, and coaxial electrospinning was performed for 4.5h. Finally, in a fume hood, prepare glutaraldehyde crosslinking liquid, take 4 mL of 50% glutaraldehyde solution and dissolve it in 46 mL of anhydrous ethanol to obtain 4% glutaraldehyde crosslinking liquid, place the composite nanofiber membrane dried in step 4 in 50 mL of crosslinking liquid, heat it in a water bath at 60°C for 35 minutes. Dry the crosslinked composite nanofiber membrane at room temperature for 10 minutes to obtain an antibacterial protective film for high-frequency contact surfaces.

[0060] The present invention mixes metal peroxide nanoparticles with high molecular polymers for spinning, and utilizes the fact that when the skin surface (such as the fingertips) contacts the metal peroxide nanoparticles, secretions such as sweat on the skin surface are weakly acidic, which can induce the metal peroxide nanoparticles to react with water molecules in a humid environment, releasing metal ions and a large amount of reactive oxygen species (ROS) such as hydrogen peroxide and hydroxyl free radicals. The oxidative stress caused by the excessive ROS can inactivate bacteria on the high-frequency contact surface in a short time.

[0061] Figure 1 The schematic diagram of the structure of the antibacterial protective film for high-frequency contact surfaces of Example 1, wherein the antibacterial protective film has a core-shell structure, wherein the core is polyvinyl alcohol, and the shell is composed of quaternized chitosan and CuO 2 Nanoparticle composite composition, CuO 2 The nanoparticles were half-coated with quaternized chitosan; Figure 2 is the antibacterial activity of the antibacterial protective film of each embodiment when it is in contact with bacteria for 1 hour. 2 The antibacterial protective film was taken out after being fully in contact with a certain amount of bacteria for 1 hour, and then the antibacterial rate was calculated after continuing to be cultured for 24 hours. After the antibacterial protective film of each embodiment was in contact with bacteria for only 1 hour, the antibacterial rate was >90%, which had a significant bactericidal effect and could achieve rapid and efficient antibacterial in a short time. With the increase of peroxide content, the antibacterial effect was significantly improved. Taking the composite nanofiber membrane prepared in Example 1 as an example, Figure 3 This is a detection diagram of hydrogen peroxide produced by the composite nanofiber membrane of Example 1. 2The antibacterial protective film was immersed in a phosphate buffer containing tetramethylbenzidine (40 μg / mL). After incubation for different time periods, the phosphate buffer after incubation was mixed with a titanium sulfate solution (1 mg / mL) at a volume ratio of 1:1. The absorbance of the culture solution at 412 nm was detected by a photometer to characterize the hydrogen peroxide generation ability of the antibacterial fiber membrane. At 1 h, the exposed CuO 2 The nanoparticles react with the environment to produce a large amount of hydrogen peroxide. After 1 hour, the CuO 2 Nanoparticles are consumed, and the antibacterial protective film is coated on the CuO inside the chitosan 2 Nanoparticles react with the environment to produce a large amount of hydrogen peroxide again. The production of a large amount of hydrogen peroxide and reactive oxygen species (ROS) such as hydroxyl radicals can cause oxidative stress and inactivate bacteria on high-frequency contact surfaces in a short period of time.

Claims

1. A method for preparing an antibacterial protective film for high-frequency contact surfaces, characterized in that: The metal peroxide nanoparticles and quaternized chitosan are used as shell materials, polyvinyl alcohol is used as core material, coaxial electrospinning is performed, cross-linking is performed, and finally an antibacterial protective film for high-frequency contact surfaces is obtained through drying.

2. The method for preparing an antibacterial protective film for high-frequency contact surfaces according to claim 1, characterized in that: Follow the steps below to implement it: Step 1, preparing a shell precursor of an antibacterial protective film for high-frequency contact surfaces; specifically: Step 1.1, dissolving quaternized chitosan and polyvinyl alcohol in deionized water, heating in a water bath with stirring, and cooling to room temperature to obtain a quaternized chitosan solution; Step 1.2, dissolving the metal salt and polyvinyl pyrrolidone in deionized water, adding the NaOH aqueous solution under stirring in an ice water bath at 0-2°C, then adding the H2O2 solution dropwise, and continuing to stir in the ice water bath for 20-40 minutes, then washing by centrifugation with ethanol for multiple times, adding to the quaternized chitosan solution, stirring for 4-6 hours, to obtain quaternized chitosan-coated metal peroxide nanoparticles, which are the shell precursors of the antibacterial protective film for high-frequency contact surfaces; Step 2, dissolving polyvinyl alcohol in deionized water, heating and stirring in a water bath, to obtain a core precursor of an antibacterial protective film for high-frequency contact surfaces; Step 3, constructing an antibacterial protective film for high-frequency contact surfaces with a thorn-shaped core-shell structure; Step 3.1, placing the precursor of the shell layer of the high-frequency contact surface antibacterial protective film prepared in step 1 in the shell layer extrusion device of the electrospinning device, placing the core precursor of the high-frequency contact surface antibacterial protective film prepared in step 2 in the core layer extrusion device of the electrospinning device, and performing coaxial electrospinning to obtain a composite nanofiber membrane; Step 3.2, dissolving the glutaraldehyde solution in anhydrous ethanol to obtain a glutaraldehyde cross-linking solution with a volume concentration of 4-6%, placing the dried composite nanofiber membrane in the glutaraldehyde cross-linking solution, heating in a water bath for cross-linking, and drying the cross-linked composite nanofiber membrane for 10-20 minutes to obtain a high-frequency contact surface antibacterial protective film with a thorn-like core-shell structure.

3. The method for preparing an antibacterial protective film for high-frequency contact surfaces according to claim 2, characterized in that: In the step 1.1, the heating and stirring temperature is 70-90° C., and the heating and stirring time is 2-3 hours; the mass ratio of quaternized chitosan, polyvinyl alcohol and deionized water is 0.1-0.15:0.4-0.6:10-15.

4. The method for preparing an antibacterial protective film for high-frequency contact surfaces according to claim 2, characterized in that: In the step 1.2, the metal salt is at least one of cupric chloride dihydrate and silver nitrate; the mass ratio of the metal salt, polyvinyl pyrrolidone and deionized water is 0.15-0.2:1-1.5:50-70.

5. The method for preparing an antibacterial protective film for high-frequency contact surfaces according to claim 2, characterized in that: In the step 2, the heating and stirring temperature is 70-90° C., and the heating and stirring time is 2-3 h.

6. The method for preparing an antibacterial protective film for high-frequency contact surfaces according to claim 2, characterized in that: In the step 3.1, during electrospinning: the voltage is set to 18 kV, the injection speed is set to 0.0003 mm / s-0.0006 mm / s, the distance between the spinneret and the collecting plate is 20 cm, and the spinning time is 4.5 h.

7. The method for preparing an antibacterial protective film for high-frequency contact surfaces according to claim 2, characterized in that: In the step 3.2, the heating temperature is 50-60° C. and the heating time is 35-45 min. 8.Antibacterial protective film for high-frequency contact surfaces, characterized in that: The method is prepared by any one of claims 1 to 7.

Citation Information

Patent Citations

  • Antibacterial type blended electro spinning nanometer fiber membrane biological dressing and the preparing method thereof

    CN101062426A

  • Preparation of multifunctional electrostatic spinning fiber membrane for grafting

    CN107881648A

  • Liquid-absorbing antibacterial 3D nanofiber composite medical dressing and preparation method thereof

    CN114073786A

  • Biomass antibacterial composite membrane material and preparation method thereof

    CN115625945A

  • Quaternary ammonium salt chitosan antibacterial composite nanofiber membrane and preparation method thereof

    CN117005113A