Manganese slag-based catalyst as well as preparation method and application thereof

By adding iron substances or cobalt in the preparation of manganese slag-based catalysts and adopting electrolytic manganese slag/H2O2 heterogeneous Fenton-like system, the problem of insufficient degradation ability of manganese slag catalysts in the existing technology for various organic pollutants is solved. , achieving efficient and low-cost organic wastewater treatment, suitable for industrial applications, and alleviating environmental pressure.

CN118743995APending Publication Date: 2024-10-08TONGREN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410948354.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing preparation method of manganese slag-based catalysts has a high degradation rate for carbamazepine, but its ability to degrade other organic pollutants is limited, and it relies on the assistance of ultraviolet radiation, which is costly and difficult to achieve industrial application.

Method used

During the preparation process of the manganese slag-based catalyst, ironic substances or cobalt are added, and the catalyst is prepared by the equal volume impregnation method to promote the catalytic generation of •OH, improve the degradation effect of organic pollutants, and adopt the electrolytic manganese slag/H2O2 heterogeneous type Fenton system for organic wastewater degradation.

Benefits of technology

It significantly improves the degradation efficiency of organic pollutants, has strong degradation ability, low cost, is suitable for industrial applications, and can effectively alleviate the environmental pressure caused by the accumulation of electrolytic manganese slag, and the treated slag can be utilized as resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743995A_ABST
    Figure CN118743995A_ABST
Patent Text Reader

Abstract

The invention provides a manganese slag-based catalyst and a preparation method and application thereof, the preparation method of the manganese slag-based catalyst comprises the following steps: soaking manganese slag with deionized water, drying, adding nitrate to dissolve the manganese slag to form a solution, and controlling the mass ratio of the manganese slag to the nitrate to be (3-4): 1; and then dropwise adding the solution into manganese slag, standing, drying, grinding into powder after drying, calcining to 500-700 DEG C, preserving heat for more than 2 hours, and finally naturally cooling. According to the manganese slag-based catalyst, an iron substance or cobalt is added in the preparation process, a synergistic effect is achieved on catalytic generation and utilization of OH, removal of organic pollutants is better facilitated, and the degradation effect of the organic pollutants is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0002] The invention relates to the field of organic wastewater treatment, and in particular to a manganese slag-based catalyst and a preparation method and application thereof. Background Art

[0004] The common preparation method of manganese slag-based catalysts in the prior art is to grind, wash and dry the resulting photocatalyst, and then put it into organic wastewater to treat the wastewater. Ultraviolet light is usually used during the treatment process to degrade pollutants in the organic wastewater.

[0005] Although the preparation method of the catalyst in the prior art is simple, the manganese catalyst prepared has a high degradation rate only for carbamazepine, and the type of organic pollutants degraded is single. Moreover, the technology needs to rely on ultraviolet radiation for auxiliary degradation, which is not only costly but also difficult to achieve industrial application.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0008] The first purpose of the present invention is to provide a method for preparing a manganese slag-based catalyst. The manganese slag-based catalyst adds ferrous substances or cobalt during the preparation process, which has a synergistic effect on the catalytic generation and utilization of •OH, is more conducive to the removal of organic pollutants, and improves the degradation effect of organic pollutants.

[0009] The second purpose of the present invention is to provide a manganese slag-based catalyst prepared by the above-mentioned preparation method, which has a wide range of subsequent application value, can improve the degradation effect, and has a strong degradation efficiency.

[0010] The third purpose of the present invention is to provide a further application of the above-mentioned manganese slag-based catalyst, using an electrolytic manganese slag catalyst / H2O2 heterogeneous Fenton-like system to degrade organic wastewater, thereby treating waste with waste. Not only does it have a wide degradation concentration range, strong degradation ability, and mild reaction conditions, but it also effectively alleviates the environmental pressure caused by excessive stacking of electrolytic manganese slag. At the same time, the treated slag after large-scale treatment can be further utilized as a resource.

[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: The present invention provides a method for preparing a manganese slag-based catalyst, comprising the following steps: First, the manganese slag is soaked in deionized water and dried, and nitrate is added to dissolve it to form a solution. The mass ratio of manganese slag to nitrate is controlled at (3-4): 1; Then the solution is added dropwise to the manganese slag, allowed to stand, and then dried. After drying, the mixture is ground into powder, calcined to 500-700° C., kept at this temperature for more than 2 hours, and finally cooled naturally; Preferably, water is added to the cobalt nitrate hexahydrate and / or the iron nitrate nonahydrate to dissolve them to form a solution; Preferably, as a further feasible solution, cobalt nitrate hexahydrate and ferric nitrate nonahydrate are used simultaneously; Preferably, as a further implementable solution, the mass ratio between cobalt nitrate hexahydrate and ferric nitrate nonahydrate is 1:1.

[0012] In the scheme of the present invention, the catalyst is prepared by the equal volume impregnation method. The mechanism of the catalytic effect of the manganese catalyst is: the reaction surface adsorbs an atom or molecule from the substrate, and then catalyzes the reaction by oxidizing protons or separating hydrogen atoms or separating carbon-carbon double bonds. Nitrates are creatively added in the process of preparing the catalyst, and preferably cobalt nitrate hexahydrate and / or ferric nitrate nonahydrate are selected, so as to enhance the synergistic effect, promote the catalytic generation of •OH, and further improve the adsorption effect. The •OH free radical has strong oxidizing properties and can oxidize various toxic and difficult-to-degrade organic compounds to achieve the purpose of removing pollutants.

[0013] A better solution is to use cobalt nitrate hexahydrate and / or ferric nitrate nonahydrate in combination, and the mass ratio of the two is best controlled at 1:1, because it has been found through practice that after the two are used together, their catalytic effect can be significantly improved, and their adsorption capacity is enhanced, which is more conducive to the removal of pollutants in the subsequent degradation treatment of organic wastewater.

[0014] Preferably, as a further feasible solution, the manganese slag is soaked in deionized water for 3-5 hours, preferably 4 hours.

[0015] Preferably, as a further feasible solution, the drying temperature after soaking is 100-120° C., and the drying time is 10-14 hours.

[0016] Preferably, as a further feasible solution, after the solution is dripped into the manganese slag, the standing time is more than 4 hours, more preferably 5 hours, 6 hours.

[0017] Preferably, as a further feasible solution, the drying temperature after standing is 100-130° C., and the drying time is 7-9 hours.

[0018] The reason why the equal volume impregnation method is used in the preparation of the catalyst is that the equal volume impregnation method can control the loading amount of the active component more conveniently, and the loading amount is easy to calculate. This is particularly important for the preparation of catalysts that require precise control of the content of the active component.

[0019] Although the preparation method of isovolumetric impregnation method is simple, the parameters involved in the preparation method need to be more carefully constrained in order to further improve the catalytic performance of the prepared catalyst. The standing process is to allow the metal ions or active components to be fully adsorbed on the surface and pores of the carrier, but if the standing time is too long, the effect will not be further improved, so the standing process is best controlled within an appropriate time range.

[0020] During the preparation process, the drying temperature and time should be adjusted according to the specific system to avoid carrier cracking or loss of active components. After drying, calcination treatment is required to further solidify the active components and improve the thermal stability of the catalyst. The calcination temperature and time are optimized according to specific experimental conditions.

[0021] The present invention also provides a manganese slag-based catalyst prepared by the above-mentioned preparation method. The prepared manganese slag-based catalyst has good application in organic matter degradation.

[0022] Preferably, as a further feasible solution, the concentration of the manganese slag-based catalyst added to the organic wastewater is controlled at 0.5-2 g / L, and hydrogen peroxide is added for degradation.

[0023] Preferably, as a further feasible solution, the temperature of the degradation reaction is 20-30° C., and the time of the degradation reaction is between 200-400 min.

[0024] Compared with the prior art, the present invention has the following beneficial effects: (1) The method for degrading wastewater of the present invention is easy to operate. It uses an electrolytic manganese slag catalyst / H2O2 heterogeneous Fenton-like system to degrade organic wastewater. Most organic pollutants can be degraded once to meet the direct discharge standard. Wastewater that does not meet the discharge standard can be treated with cyclic degradation to achieve a high pollutant removal rate. The cost is low, there is no secondary pollution, and it is easy to realize industrialization.

[0025] (2) The electrolytic manganese slag catalyst / H2O2 heterogeneous Fenton-like system is used to degrade organic wastewater, treating waste with waste. It not only has a wide degradation concentration range, strong degradation ability, and mild reaction conditions, but also effectively alleviates the environmental pressure caused by excessive storage of electrolytic manganese slag. At the same time, the treated slag after large-scale treatment can be further utilized as a resource.

[0026] (3) By adding nitrate to the preparation system, a synergistic effect is exerted on the catalytic generation and utilization of •OH, which is more conducive to the removal of organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] By reading the detailed description of the preferred embodiment below, various other advantages and benefits will become clear to those of ordinary skill in the art. The accompanying drawings are only used for the purpose of illustrating the preferred embodiment and are not considered to be limitations of the present invention. In addition, the same reference symbols are used to represent the same components throughout the accompanying drawings.

[0029] Figure 1 This is a graph showing the experimental results of degrading organic wastewater provided in Experimental Example 1 of the present invention. DETAILED DESCRIPTION

[0031] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0032] Example 1 (1) Preparation of catalyst: First, soak the manganese slag in deionized water for 4 hours, clean the manganese slag, dry it at 110℃ for 12 hours, and then use the equal volume impregnation method to prepare the catalyst; first take 10g of the dried manganese slag, then weigh 2.463g of cobalt nitrate hexahydrate [Co(NO3).6H2O] in a beaker, add 6ml of water to dissolve it, then use a rubber-tipped dropper to drip the solution into the manganese slag, let it stand for 4 hours, and then dry it at 110℃ for 8 hours. After that, grind it into powder, put it in a muffle furnace and calcine it to 600℃, keep it warm for 2 hours, take it out and let it cool naturally. At this point, the manganese slag-based catalyst is ready.

[0033] (2) Degradation of organic matter (paracetamol): The pH value of organic wastewater was 7.31; the concentration of manganese slag-based catalyst added to organic wastewater was 1 g / L; the amount of H2O2 added was 5 g (the concentration of hydrogen peroxide was 30%), and the concentration of paracetamol in organic wastewater was 20 mg / L; during the degradation reaction, the temperature of the degradation reaction was 25 °C, the degradation reaction time was 300 min, and the degradation effect of paracetamol was measured by liquid chromatography. At 300 min, the degradation rate of paracetamol was 58%.

[0034] Example 2 (1) Preparation of catalyst: First, soak the manganese slag in deionized water for 4 hours, clean the manganese slag, dry it at 110℃ for 12 hours, and then use the equal volume impregnation method to prepare the catalyst; first take 10g of the dried manganese slag, then weigh 3.608g of iron nitrate [Fe(NO3).9H2O] in a beaker, add 6ml of water to dissolve it, and then use a rubber-tipped dropper to drip the solution into the manganese slag, let it stand for 4 hours, and then dry it at 110℃ for 8 hours, then grind it into powder, and then put it into a muffle furnace to calcine it to 500℃, keep it warm for 2 hours, take it out, and let it cool naturally. At this point, the manganese slag-based catalyst is ready.

[0035] (2) Degradation of organic matter (paracetamol): The pH value of the organic wastewater is 7.31; the manganese slag-based catalyst prepared in step (1) is added to the organic wastewater at a concentration of 1 g / L; the amount of H2O2 added is 5 g, and the acetaminophen concentration in the organic wastewater is 20 mg / L; during the degradation reaction, the degradation reaction temperature is 25°C, the degradation reaction time is 300 min, and the degradation effect of acetaminophen is measured by liquid chromatography. At 300 min, the degradation rate of acetaminophen is 60%.

[0036] Example 3 (1) Preparation of catalyst: First, soak the manganese slag in deionized water for 4 hours, clean the manganese slag, dry it at 110℃ for 12 hours, and then use the equal volume impregnation method to make the catalyst; first take 10g of the dried manganese slag, then weigh 2.289g of manganese nitrate [Mn(NO3)] in a beaker, add 6ml of water to dissolve it, and then use a rubber-tipped dropper to drip the solution into the manganese slag, let it stand for 4 hours, and then dry it at 110℃ for 8 hours. After that, grind it into powder, put it in a muffle furnace and calcine it to 400℃, keep it warm for 2 hours, take it out, and let it cool naturally. At this point, the manganese slag-based catalyst is ready.

[0037] (2) Degradation of organic matter (paracetamol): The pH value of the organic wastewater was 7.31; the manganese slag-based catalyst prepared in step (1) was added to the organic wastewater at a concentration of 1 g / L; the amount of H2O2 added was 5 g, and the acetaminophen concentration in the organic wastewater was 20 mg / L; during the degradation reaction, the degradation reaction temperature was 25°C, the degradation reaction time was 300 min, and the degradation effect of acetaminophen was measured by liquid chromatography. At 300 min, the degradation rate of acetaminophen was 59%.

[0038] Example 4 (1) Preparation of catalyst: First, soak the manganese slag in deionized water for 4 hours, clean the manganese slag, dry it at 110℃ for 12 hours, and then use the equal volume impregnation method to prepare the catalyst; first take 10g of the dried manganese slag, then weigh 1.544g of cerium nitrate hexahydrate [Ce(NO3).6H2O] in a beaker, add 6ml of water to dissolve it, and then use a rubber-tipped dropper to drip the solution into the manganese slag, let it stand for 4 hours, and then dry it at 110℃ for 8 hours. After that, grind it into powder, put it in a muffle furnace and calcine it to 500℃, keep it warm for 2 hours, take it out, and let it cool naturally. At this point, the manganese slag-based catalyst is ready.

[0039] (2) Degradation of organic matter (paracetamol): The pH value of the organic wastewater is 7.31; the manganese slag-based catalyst prepared in step (1) is added to the organic wastewater at a concentration of 1 g / L; the amount of H2O2 added is 5 g, and the acetaminophen concentration in the organic wastewater is 20 mg / L; during the degradation reaction, the degradation reaction temperature is 25°C, the degradation reaction time is 300 min, and the degradation effect of acetaminophen is measured by liquid chromatography. At 300 min, the degradation rate of acetaminophen is 60%.

[0040] Example 5 (1) Preparation of catalyst: First, soak the manganese slag in deionized water for 4 hours, clean the manganese slag, dry it at 110℃ for 12 hours, and then use the equal volume impregnation method to make the catalyst; first take 10g of the dried manganese slag, then weigh 2.289g of zinc nitrate [Zn(NO3).6H2O] in a beaker, add 6ml of water to dissolve it, then use a rubber-tipped dropper to drip the solution into the manganese slag, let it stand for 4 hours, and then dry it at 110℃ for 8 hours. After that, grind it into powder, put it in a muffle furnace and calcine it to 400℃, keep it warm for 2 hours, take it out and let it cool naturally. At this point, the manganese slag-based catalyst is ready.

[0041] (2) Degradation of organic matter (paracetamol): The pH value of the organic wastewater was 7.31; the manganese slag-based catalyst prepared in step (1) was added to the organic wastewater at a concentration of 1 g / L; the amount of H2O2 added was 5 g, and the acetaminophen concentration in the organic wastewater was 20 mg / L; during the degradation reaction, the degradation reaction temperature was 25°C, the degradation reaction time was 300 min, and the degradation effect of acetaminophen was measured by liquid chromatography. At 300 min, the degradation rate of acetaminophen was 57%.

[0042] Example 6 (1) Preparation of catalyst: First, soak the manganese slag in deionized water for 3 hours, clean the manganese slag, and then dry it at 100℃ for 14 hours, and then use the equal volume impregnation method to make the catalyst; first take 10g of the dried manganese slag, then weigh 3.608g of iron nitrate [Fe(NO3).9H2O] in a beaker, add 6ml of water to dissolve it, and then use a rubber-tipped dropper to drip the solution into the manganese slag, let it stand for 5 hours, and then dry it at 130℃ for 7 hours. After that, grind it into powder, put it in a muffle furnace and calcine it to 500℃, keep it warm for 3 hours, take it out, and let it cool naturally. At this point, the manganese slag-based catalyst is ready.

[0043] (2) Degradation of organic matter (paracetamol): The pH value of the organic wastewater is 7.31; the manganese slag-based catalyst prepared in step (1) is added to the organic wastewater at a concentration of 0.5 g / L; the amount of H2O2 added is 5 g, and the acetaminophen concentration in the organic wastewater is 20 mg / L; during the degradation reaction, the degradation reaction temperature is 20°C, the degradation reaction time is 400 min, and the degradation effect of acetaminophen is measured by liquid chromatography. At 400 min, the degradation rate of acetaminophen is 56%.

[0044] Example 7 (1) Preparation of catalyst: First, soak the manganese slag in deionized water for 5 hours, clean the manganese slag, dry it at 120℃ for 10 hours, and then use the equal volume impregnation method to make the catalyst; first take 10g of the dried manganese slag, then weigh 3.608g of iron nitrate [Fe(NO3).9H2O] in a beaker, add 6ml of water to dissolve it, then use a rubber-tipped dropper to drip the solution into the manganese slag, let it stand for 6 hours, and then dry it at 100℃ for 9 hours. After that, grind it into powder, put it in a muffle furnace and calcine it to 700℃, keep it warm for 4 hours, take it out and let it cool naturally. At this point, the manganese slag-based catalyst is ready.

[0045] (2) Degradation of organic matter (paracetamol): The pH value of the organic wastewater was 7.31; the manganese slag-based catalyst prepared in step (1) was added to the organic wastewater at a concentration of 2 g / L; the amount of H2O2 added was 5 g, and the acetaminophen concentration in the organic wastewater was 20 mg / L; during the degradation reaction, the degradation reaction temperature was 30°C, the degradation reaction time was 200 min, and the degradation effect of acetaminophen was measured by liquid chromatography. At 200 min, the degradation rate of acetaminophen was 54%.

[0046] Comparative Example 1 Degradation of organic matter (paracetamol): The pH value of organic wastewater is 7.31; manganese slag is directly added to the organic wastewater at a concentration of 1g / L; the amount of H2O2 added is 5g (the concentration of hydrogen peroxide is 30%), and the concentration of paracetamol in the organic wastewater is 20mg / L; during the degradation reaction, the temperature of the degradation reaction is 25℃, the degradation reaction time is 300min, and the degradation effect of paracetamol is measured by liquid chromatography. At 300min, the degradation rate of paracetamol is as follows: Figure 1 shown.

[0047] Example 8 The other operation steps were the same as those in Example 1, except that 2.463 g of cobalt nitrate hexahydrate [Co(NO3).6H2O] and ferric nitrate nonahydrate [Fe(NO3).9H2O] were weighed in a beaker, and the mass ratio between the two was 1:1. The degradation effect of acetaminophen was measured by liquid chromatography. At 300 min, the degradation rate of acetaminophen was 65%.

[0048] Experimental Example 1 Attached Figure 1 In the figure, the graph of manganese slag loaded with Co oxidation corresponds to the scheme of Example 1, the graph of manganese slag loaded with Co adsorption corresponds to the scheme of Example 1 without H2O2, the graph of original manganese slag oxidation corresponds to the scheme of Comparative Example 1, the graph of original manganese slag adsorption corresponds to the scheme of Comparative Example 1 without H2O2, and the graph of hydrogen peroxide oxidation corresponds to the scheme of Comparative Example 1 without manganese slag. For specific degradation rates, see Figure 1 The vertical coordinate of .

[0049] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications within the scope of the present invention in the appended claims.

Claims

1. A method for preparing a manganese slag-based catalyst, characterized in that: The steps include: First, the manganese slag is soaked in deionized water and dried, and nitrate is added to dissolve it to form a solution. The mass ratio of manganese slag to nitrate is controlled at (3-4): 1; Then the solution is added dropwise to the manganese slag, allowed to stand, and then dried. After drying, the mixture is ground into powder, calcined to 500-700° C., kept at this temperature for more than 2 hours, and finally cooled naturally; Preferably, water is added to the cobalt nitrate hexahydrate and / or the iron nitrate nonahydrate to dissolve them to form a solution; Preferably, cobalt nitrate hexahydrate and ferric nitrate nonahydrate are used simultaneously; Preferably, the mass ratio between cobalt nitrate hexahydrate and ferric nitrate nonahydrate is 1:

1.

2. The preparation method according to claim 1, characterized in that: The manganese slag is soaked in deionized water for 3-5 hours, preferably 4 hours.

3. The preparation method according to claim 1, characterized in that: After soaking, the drying temperature is 100-120°C and the drying time is 10-14h.

4. The preparation method according to claim 1, characterized in that: After the solution is added dropwise to the manganese slag, the solution is allowed to stand for more than 4 hours.

5. The preparation method according to claim 1, characterized in that: After standing, the drying temperature is 100-130°C and the drying time is 7-9h.

6. The manganese slag-based catalyst prepared by the preparation method according to any one of claims 1 to 5.

7. Use of the manganese slag-based catalyst prepared by the preparation method according to any one of claims 1 to 5 in the degradation of organic matter.

8. The use according to claim 7, characterized in that: The concentration of manganese slag-based catalyst added to organic wastewater is controlled at 0.5-2 g / L, and hydrogen peroxide is added for degradation.

9. The use according to claim 8, characterized in that: The temperature of the degradation reaction is 20-30°C, and the time of the degradation reaction is between 200-400 minutes.