Preparation method of nanofiber composite membrane for photocatalysis
Highly crystalline g-C3N4 powder was prepared through high-temperature calcination of urea and ionothermal method, and combined with polyacrylonitrile, and electrospinning technology was used to prepare protonated g-C3N4/PAN nanofiber membrane, which solved the problem of low crystallinity and agglomeration of photocatalysts. , achieving efficient dye wastewater treatment and cycle stability.
Patent Information
- Application Number
- CN202410468132.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-08
AI Technical Summary
The low crystallinity of existing photocatalysts such as g-C3N4 leads to a reduction in the separation rate of photogenerated carriers, and the nanoscale photocatalysts are easy to agglomerate and difficult to recycle, which limits their application in dye wastewater treatment.
g-C3N4 powder is prepared by high-temperature calcination of urea, combined with ionothermal method and protonation treatment to form highly crystalline molten salt g-C3N4 powder, and combined with polyacrylonitrile (PAN), using electrospinning technology to prepare protonated g-C3N4 /PAN nanofiber membrane.
It improves the crystallinity and photocatalytic effect of g-C3N4, solves the agglomeration problem, enhances the photocatalytic efficiency and cycle stability of the nanofiber membrane, and achieves the ability to efficiently degrade dye wastewater.
Smart Images

Figure CN118744006A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a photocatalytic film in the technical field of photocatalysis, and in particular to a method for preparing a photocatalyst-loaded nanofiber film. Background Art
[0002] In recent years, the rapid development of industrialized cities has aroused people's concern about water pollution. At present, dye wastewater has become one of the important issues of global natural environment. Dye wastewater not only seriously damages the ecosystem, but also induces various diseases, seriously affecting human health. Removing dye molecules from dye wastewater is one of the solutions to alleviate water pollution problems. There are many treatment methods for removing dye molecules, such as adsorption, microbial method, chemical flocculation method, photocatalysis, ozone oxidation method, etc. Among them, the photocatalytic method uses clean and pollution-free solar energy as the energy driving force, and combines it with a semiconductor photocatalyst with light response to carry out catalytic reaction. Due to its low cost, simple preparation, can completely degrade dye molecules and will not produce secondary pollution, it has broad prospects in treating dye wastewater. In the field of dye wastewater treatment, the ideal photocatalyst should have the following characteristics: strong hydrophilicity, high degradation efficiency and excellent recyclability.
[0003] At present, a variety of photocatalysts have been developed for use in the field of photocatalysis, such as metal oxides, metal sulfides, bismuth-based materials, carbon-based materials, metal organic frameworks, etc. Traditional metal oxides such as TiO2 (3.2eV) and ZnO (3.37eV) have a wide band gap and can only be excited by ultraviolet light, which limits their utilization of sunlight. The non-metallic semiconductor g-C3N4 (2.7eV) has a narrow band gap, is non-toxic, and has stable chemical properties. It is a very promising photocatalyst. However, in practical applications, g-C3N4 prepared by polycondensation reaction of nitrogen-containing organic precursors has a low crystallinity due to insufficient deamination, resulting in a reduced separation rate of photogenerated carriers. In order to solve this problem, patent CN202111542092.2 discloses a method for preparing highly crystalline g-C3N4, which is mainly prepared by calcination and molten salt-assisted method. After two-step calcination, the crystallinity of g-C3N4 is improved, and its photocatalytic effect is also improved.
[0004] In addition, nanoscale photocatalysts are easy to agglomerate and difficult to recycle in practical applications, and will cause secondary pollution to the environment, thus limiting their application in dye wastewater. In order to solve this problem, many researchers have proposed that photocatalysts can be loaded onto membrane-based materials for easy recycling. Among them, electrospun polyacrylonitrile (PAN) nanofiber membrane is an ideal photocatalyst loading material. However, since the g-C3N4 powder prepared by high-temperature calcination in the spinning solution is very easy to agglomerate, a large number of nodules and beads appear after combining with the prepared PAN electrospun nanofiber membrane, which is not conducive to the photocatalytic reaction. Summary of the invention
[0005] In view of the problems of low separation rate of photogenerated carriers of g-C3N4 and high recycling cost, the present invention aims to provide a method for preparing a protonated g-C3N4 nanofiber membrane. The photocatalytic composite membrane prepared by the present invention is used to treat dye wastewater and has the characteristics of high degradation efficiency and high reuse rate.
[0006] To this end, the present invention provides the following technical solutions:
[0007] A method for preparing a nanofiber membrane for photocatalysis, characterized in that it comprises the following steps:
[0008] (1) a certain amount of urea is calcined at high temperature in an inert gas atmosphere to prepare a light yellow powder g-C3N4, i.e., the original g-C3N4 powder;
[0009] (2) mixing the obtained g-C3N4 powder with a certain proportion of a mixture of potassium salt and lithium salt by an ion thermal method, grinding it fully into a fine powder, and performing secondary calcination to obtain a highly crystalline molten salt g-C3N4 powder;
[0010] (3) protonating the obtained high-crystalline molten salt g-C3N4 powder to obtain protonated g-C3N4 powder;
[0011] (4) polyacrylonitrile (PAN), protonated g-C3N4 powder, and N,N-dimethylformamide (DMF) are prepared in a certain proportion and stirred evenly;
[0012] (5) Protonated g-C3N4 / PAN nanofiber membrane was prepared using electrospinning technology.
[0013] Wherein, the protonation treatment in step (3) adopts an acid with a pH of 1-4, and the acid can be selected from hydrochloric acid, sulfuric acid, formic acid, etc.
[0014] Preferably, in step (1), high-temperature calcination is carried out in a tubular furnace in a nitrogen atmosphere to prepare g-C3N4 powder; in step (2), secondary calcination is carried out in a tubular furnace.
[0015] Preferably, in step (3), the molten salt g-C3N4 powder is placed in a hydrochloric acid solution of a certain concentration for protonation treatment to obtain protonated g-C3N4 powder.
[0016] Preferably, the ratio of g-C3N4 powder to the sum of the masses of lithium chloride and potassium chloride is 1:10; the mass ratio of lithium chloride to potassium chloride is 5:15, 9:11, 13:7, 17:3.
[0017] Preferably, the concentration of protonated g-C3N4 powder is 3-7%.
[0018] A preferred implementation is:
[0019] Step (1) and step (2) are specifically as follows:
[0020] Preparation of molten salt g-C3N4 powder: 10g urea was placed in a crucible and the upper end was sealed with tin foil. The crucible was placed in a tube furnace and heated to 500-600℃ in a nitrogen atmosphere for calcination for 3 hours to obtain a light yellow powder g-C3N4. 44 , i.e. original g-C3N4 powder; mixing the obtained original g-C3N4 powder with lithium chloride and potassium chloride, grinding them fully into fine powder, and then placing them in a tube furnace for secondary calcination at 500-600°C to obtain molten salt g-C3N4 powder, wherein the mass ratio of g-C3N4 to lithium chloride and potassium chloride is 2:9:11;
[0021] Step (3) is specifically as follows:
[0022] Preparation of protonated g-C3N4 powder: placing the obtained molten salt g-C3N4 powder into a hydrochloric acid solution and ultrasonically treating the solution, wherein the pH of the hydrochloric acid solution is 1-4 and the ultrasonic treatment time is 1-3 hours;
[0023] Step (4) is specifically as follows:
[0024] Preparation of protonated g-C3N4 / PAN nanofiber membrane: protonated g-C3N4 powder is added to N,N-dimethylformamide solution and ultrasonically treated to make the mixture evenly mixed, then PAN powder is added, and then stirred at 60°C to completely dissolve the PAN powder to obtain a spinning solution, and the spinning solution is spun by electrospinning technology to obtain a protonated g-C3N4 / PAN nanofiber membrane, wherein the spinning solution contains protonated g-C3N4, PAN and N,N-dimethylformamide, wherein the mass percentage of protonated g-C3N4 in the total solution is 3-7%, and the concentration of PAN solution is 14%.
[0025] As can be seen from the above technical scheme, the present invention adopts ion thermal method, protonation treatment and electrostatic spinning technology to prepare protonated g-C3N4 / PAN nanofiber membrane. The molten salt g-C3N4 treated with hydrochloric acid will change the charge of g-C3N4, so that its surface potential changes from negative to positive, improve the spinning stability, and can also increase the crystallinity of g-C3N4, thereby enhancing its photocatalytic effect. Combining protonated g-C3N4 powder with PAN nanofiber membrane not only solves the problem of agglomeration of g-C3N4 powder in spinning solution, but also makes g-C3N4 powder uniformly dispersed in nanofibers, while protonation treatment improves the crystallinity of g-C3N4 powder and thus improves the separation rate of photogenerated carriers, thereby effectively improving the photocatalytic efficiency of nanofiber composite membrane.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1) The crystallinity of the molten salt g-C3N4 powder treated with hydrochloric acid is improved and its photocatalytic effect is enhanced.
[0028] 2) The nanofiber membrane is prepared by electrospinning technology, which has a stable fiber structure and good chemical stability, and can improve its cyclic stability.
[0029] 3) The molten salt g-C3N4 powder treated with hydrochloric acid transforms the negatively charged g-C3N4 into a positively charged one, thereby strengthening the bonding with the nanofibers, making the photocatalyst and the base film complement each other and improving the application effect in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a physical comparison picture of the g-C3N4 powder of Example 1 and the protonated g-C3N4 powder of Example 3, wherein the left one is g-C3N4 powder and the right one is protonated g-C3N4 powder, both weighing 1.5 g.
[0031] Figure 2 Schematic diagram of the actual XRD ray diffraction of the g-C3N4 powder of Example 1 and the protonated g-C3N4 powder of Example 3.
[0032] Figure 3 Zeta potential diagram of g-C3N4 powder in Example 1 and protonated g-C3N4 powder in Example 3.
[0033] Figure 4 This is a scanning electron microscope schematic diagram of Example 1g-C3N4 nanofiber membrane.
[0034] Figure 5 This is a scanning electron microscope schematic diagram of the protonated g-C3N4 nanofiber membrane of Example 3.
[0035] Figure 6 Schematic diagram of the degradation of Rhodamine B (RhB) by g-C3N4 nanofiber membrane in Example 1 and protonated g-C3N4 nanofiber membrane in Implementation Example 3.
[0036] Figure 7 Schematic diagram of the cyclic degradation of RhB by protonated g-C3N4 nanofiber membrane in Example 3. DETAILED DESCRIPTION
[0037] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. The embodiments of the present invention are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0038] Example 1
[0039] (1) Preparation of g-C3N4 powder: 10 g of urea was placed in a crucible and the upper end was sealed with tin foil. The crucible was placed in a tube furnace and heated to 550°C for calcination for 3 hours under a nitrogen atmosphere to obtain light yellow powder g-C3N4, i.e., the original g-C3N4 powder.
[0040] (2) Preparation of g-C3N4 / PAN nanofiber membrane: The original g-C3N4 powder was added to N,N-dimethylformamide solution for ultrasonic treatment, and then PAN powder was added after mixing evenly, and then stirred at 60°C to completely dissolve the PAN powder to obtain a spinning solution. The above solution was spun using electrospinning technology to obtain a g-C3N4 / PAN nanofiber membrane, wherein the spinning solution contained original g-C3N4, PAN and N,N-dimethylformamide, wherein the mass percentage of the original g-C3N4 in the whole solution was 3%, and the concentration of the PAN solution was 14%. The g-C3N4 / PAN nanofiber membrane was used to degrade RhB dye with a concentration of 10 mg / L. After treatment for 1 hour under dark conditions, the concentration of RhB remained basically unchanged, indicating that the catalyst had no catalytic effect in the absence of light. A 300W xenon lamp was used to simulate sunlight. After irradiation for 4 hours, the degradation rate of RhB could reach 54.68%.
[0041] Example 2
[0042] (1) Preparation of g-C3N4 powder: 10 g of urea was placed in a crucible and the upper end was sealed with tin foil. The crucible was placed in a tube furnace and heated to 550°C for calcination for 3 hours under a nitrogen atmosphere to obtain light yellow powder g-C3N4, i.e., the original g-C3N4 powder.
[0043] (2) Preparation of molten salt g-C3N4 powder: The obtained original g-C3N4 is mixed with lithium chloride and potassium chloride, and fully ground into fine powder, and then placed in a tubular furnace for secondary calcination to obtain molten salt g-C3N4 powder. The mass ratio of g-C3N4 to lithium chloride and potassium chloride is 2:9:11.
[0044] (3) Preparation of protonated g-C3N4 powder: The obtained molten salt g-C3N4 powder was placed in a hydrochloric acid solution and ultrasonically treated. The pH of the hydrochloric acid solution was 1 and the ultrasonic treatment time was 2 hours.
[0045] (4) Preparation of protonated g-C3N4 / PAN nanofiber membrane: g-C3N4 powder treated with hydrochloric acid was added to N,N-dimethylformamide solution for ultrasonic treatment, and then PAN powder was added after mixing evenly, and then stirred at 60°C to completely dissolve the PAN powder to obtain a spinning solution. The above solution was spun using electrospinning technology to obtain a protonated g-C3N4 / PAN nanofiber membrane, wherein the spinning solution contained protonated g-C3N4, PAN and N,N-dimethylformamide, wherein the mass percentage of protonated g-C3N4 powder in the whole solution was 3%, and the concentration of PAN solution was 14%. The protonated g-C3N4 / PAN nanofiber membrane was used to degrade RhB dye with a concentration of 10 mg / L. After treatment for 1 hour under dark conditions, the concentration of RhB remained basically unchanged, indicating that the catalyst had no catalytic effect in the absence of light. A 300W xenon lamp was used to simulate sunlight. After irradiation for 4 hours, the degradation rate of RhB could reach 89.25%.
[0046] Example 3
[0047] (1) Preparation of g-C3N4 powder: 10 g of urea was placed in a crucible and the upper end was sealed with tin foil. The crucible was placed in a tube furnace and heated to 550°C for calcination for 3 hours under a nitrogen atmosphere to obtain light yellow powder g-C3N4, i.e., the original g-C3N4 powder.
[0048] (2) Preparation of molten salt g-C3N4 powder: The obtained original g-C3N4 powder is mixed with lithium chloride and potassium chloride, and fully ground into fine powder, and then placed in a tubular furnace for secondary calcination to obtain molten salt g-C3N4 powder. The mass ratio of g-C3N4 to lithium chloride and potassium chloride is 2:9:11.
[0049] (3) Preparation of protonated g-C3N4 powder: The obtained molten salt g-C3N4 powder was placed in a hydrochloric acid solution and ultrasonically treated. The pH of the hydrochloric acid solution was 1 and the ultrasonic treatment time was 2 hours.
[0050] (4) Preparation of protonated g-C3N4 / PAN nanofiber membrane: g-C3N4 powder treated with hydrochloric acid was added to N,N-dimethylformamide solution for ultrasonic treatment, and then PAN powder was added after mixing evenly, and then stirred at 60°C to completely dissolve the PAN powder to obtain a spinning solution. The above solution was spun using electrospinning technology to obtain a protonated g-C3N4 / PAN nanofiber membrane, wherein the spinning solution contained protonated g-C3N4, PAN and N,N-dimethylformamide, wherein the mass percentage of protonated g-C3N4 powder in the whole solution was 5%, and the concentration of PAN solution was 14%. The protonated g-C3N4 / PAN nanofiber membrane was used to degrade RhB dye with a concentration of 10 mg / L. After treatment for 1 hour under dark conditions, the concentration of RhB remained basically unchanged, indicating that the catalyst had no catalytic effect in the absence of light. A 300W xenon lamp was used to simulate sunlight. After irradiation for 4 hours, the degradation rate of RhB could reach 99.80%.
[0051] Example 4
[0052] (1) Preparation of g-C3N4 powder: 10 g of urea was placed in a crucible and the upper end was sealed with tin foil. The crucible was placed in a tube furnace and heated to 550°C for calcination for 3 hours under a nitrogen atmosphere to obtain light yellow powder g-C3N4, i.e., the original g-C3N4 powder.
[0053] (2) Preparation of molten salt g-C3N4 powder: The obtained original g-C3N4 powder is mixed with lithium chloride and potassium chloride, and fully ground into fine powder, and then placed in a tubular furnace for secondary calcination to obtain molten salt g-C3N4 powder. The mass ratio of g-C3N4 to lithium chloride and potassium chloride is 2:9:11.
[0054] (3) Preparation of protonated g-C3N4 powder: The obtained molten salt g-C3N4 powder was placed in a hydrochloric acid solution and ultrasonically treated. The pH of the hydrochloric acid solution was 1 and the ultrasonic treatment time was 2 hours.
[0055] (4) Preparation of protonated g-C3N4 / PAN nanofiber membrane: g-C3N4 powder treated with hydrochloric acid was added to N,N-dimethylformamide solution for ultrasonic treatment, and then PAN powder was added after mixing evenly, and then stirred at 60°C to completely dissolve the PAN powder to obtain a spinning solution. The above solution was spun using electrospinning technology to obtain a protonated g-C3N4 / PAN nanofiber membrane, wherein the spinning solution contained protonated g-C3N4, PAN and N,N-dimethylformamide, wherein the mass percentage of protonated g-C3N4 powder in the whole solution was 7%, and the concentration of PAN solution was 14%. The protonated g-C3N4 / PAN nanofiber membrane was used to degrade RhB dye with a concentration of 10 mg / L. After treatment for 1 hour under dark conditions, the concentration of RhB remained basically unchanged, indicating that the catalyst had no catalytic effect in the absence of light. A 300W xenon lamp was used to simulate sunlight. After irradiation for 4 hours, the degradation rate of RhB could reach 95.62%.
[0056] The nanofiber membranes obtained in the above four examples were subjected to photocatalytic tests, and the results are shown in Table 1:
[0057] Table 1 Photocatalytic film performance test results
[0058]
[0059]
[0060] From the results in Table 1, it can be seen that the photocatalytic nanofiber membrane prepared in the present invention is used to degrade dyes, and compared with Example 1, it shows higher degradation efficiency and better cycle stability, which is conducive to long-term stable operation in degrading dyes.
Claims
1. A method for preparing a nanofiber membrane for photocatalysis, characterized in that: The following steps are involved: (1) calcining urea at high temperature under an inert gas atmosphere to prepare light yellow powder g-C3N4, i.e., original g-C3N4 powder; (2) mixing the obtained original g-C3N4 powder with a mixture of potassium salt and lithium salt by an ion thermal method, grinding it fully into a fine powder, and performing secondary calcination to obtain a highly crystalline molten salt g-C3N4 powder; (3) protonating the obtained high-crystalline molten salt g-C3N4 powder to obtain protonated g-C3N4 powder; (4) polyacrylonitrile (PAN), protonated g-C3N4 powder, and N,N-dimethylformamide (DMF) are mixed in proportion and stirred evenly; (5) Protonated g-C3N4 / PAN nanofiber membrane was prepared using electrospinning technology.
2. The method for preparing a nanofiber membrane for photocatalysis according to claim 1, characterized in that: In step (1), g-C3N4 powder is prepared by high-temperature calcination in a tubular furnace and in a nitrogen atmosphere; in step (2), secondary calcination is carried out in a tubular furnace.
3. The method for preparing a nanofiber membrane for photocatalysis according to claim 1, characterized in that: In step (3), the molten salt g-C3N4 powder is placed in a hydrochloric acid solution for protonation treatment to obtain protonated g-C3N4 powder.
4. The method for preparing a nanofiber membrane for photocatalysis according to claim 1, characterized in that: Step (1) and step (2) are specifically as follows: Preparation of molten salt g-C3N4 powder: put 10g of urea into a crucible and seal the upper end with tin foil; put the crucible into a tube furnace and heat it to 500-600℃ in a nitrogen atmosphere for calcination for 3 hours to obtain light yellow powder g-C3N4, i.e. original g-C3N4 powder; mix the obtained original g-C3N4 powder with lithium chloride and potassium chloride, grind them into fine powder, and then put them into a tube furnace for secondary calcination to obtain molten salt g-C3N4 powder, wherein the mass ratio of g-C3N4 to lithium chloride and potassium chloride is 2:9:11; Step (3) is specifically as follows: Preparation of protonated g-C3N4 powder: placing the obtained molten salt g-C3N4 powder into a hydrochloric acid solution and ultrasonically treating the solution, wherein the pH of the hydrochloric acid solution is 1-4 and the ultrasonic treatment time is 1-3 hours; Step (4) is specifically as follows: Preparation of protonated g-C3N4 / PAN nanofiber membrane: protonated g-C3N4 powder is added to N,N-dimethylformamide solution and ultrasonically treated to make the mixture evenly mixed, then PAN powder is added, and then stirred at 60°C to completely dissolve the PAN powder to obtain a spinning solution, and the spinning solution is spun by electrospinning technology to obtain a protonated g-C3N4 / PAN nanofiber membrane, wherein the spinning solution contains protonated g-C3N4, PAN and N,N-dimethylformamide, wherein the mass percentage of protonated g-C3N4 in the whole solution is 3-7%, and the concentration of PAN solution is 10-20%.
Citation Information
Patent Citations
Method for degrading organic pollutants in wastewater by catalyzing percarbonate
CN107188294A
Preparation method and application of g-C3N4 composite nanometer fibrous membrane based on electrostatic spinning process
CN110694661A
Preparation method and application of ultrathin high-crystallinity carbon nitride photocatalyst
CN113318765A
Protonated graphite phase carbon nitride nanosheet and preparation method and application thereof
CN113501507A
Simple preparation method and application of high-crystallinity graphite carbon nitride
CN114377711A
Cited By
Recycled carbon nanofiber composite light-dark continuous catalytic material and preparation method thereof
CN121669296A