Commercial wheel edge half axle production method based on controlled forging and controlled cooling process

Through the controlled forging and controlled cooling process, the problem of insufficient fatigue performance of traditional commercial wheel side axles has been solved, and a high-strength, high-toughness and low-cost production method has been achieved, ensuring that the performance indicators of commercial wheel side axles meet the requirements.

CN118744314APending Publication Date: 2024-10-08UNIV OF SCI & TECH BEIJING
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410771337.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Traditional commercial wheel side axles have insufficient fatigue performance during the quenching and tempering heat treatment process, resulting in insufficient static torsional strength, which limits their lightweight design and application. Moreover, the traditional manufacturing process consumes high energy and costs.

Method used

High-strength and high-toughness medium-carbon microalloy ferrite-pearlitic non-quenched and tempered steel is produced through a controlled forging and controlled cooling process. The specific process includes medium-frequency induction heating, die forging, online controlled cooling, machining, surface induction quenching and Staged cooling ensures microstructure matching and avoids the generation of bainite or martensite structures.

Benefits of technology

It achieves both high strength and toughness of the commercial wheel side axle. The tensile strength, yield strength and room temperature impact energy reach 890~950MPa, 600~650MPa and 40~50J. The Vickers hardness is between 280~300HV. Production costs and energy consumption are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744314A_ABST
    Figure CN118744314A_ABST
Patent Text Reader

Abstract

The invention discloses a commercial wheel edge half axle production method based on a controlled forging and controlled cooling process. The commercial wheel edge half axle production method comprises the following steps that a bar is blanked; the two ends of the bar are heated to 950-1050 DEG C through a medium-frequency induction furnace, and heat preservation is conducted for 1-2 min to enable the bar to be completely austenitized; after die forging is conducted on the two ends of a half axle, the final forging temperature is controlled to be 890-920 DEG C; and then carrying out controlled cooling, cutting, gear rolling, medium-frequency surface induction quenching, beating, straightening and finish turning, shot blasting cleaning, flaw detection, strong shot blasting and inspection and warehousing in a mode of firstly carrying out rapid cooling and then carrying out air cooling. According to the method, only the two ends of the bar are subjected to die forging to form the spline blank, and then controlled cooling is conducted. The rod part is still of the original pearlite and ferrite structure of the bar, and in order to achieve structure performance matching of the spline end and the rod part, the controlled forging and controlled cooling process is the key content of the invention. According to the microstructure obtained through the controlled forging and controlled cooling process, the proportion of pearlite and ferrite is 93-96%, the tensile strength Rm is 890-950 MPa, the yield strength Rp0.2 is 600-650 MPa, the percentage elongation after fracture is 12-18%, the room temperature impact energy AKU is 40-50 J, and the Vickers hardness is 280-300 HV.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal materials and is a high-strength and high-toughness medium-carbon microalloy ferrite-pearlite non-quenched and tempered steel for commercial vehicle wheel half shafts, and in particular relates to a production method for commercial vehicle wheel half shafts based on a controlled forging and controlled cooling process. Background Art

[0002] The commercial wheel-side reduction drive axle is a bridge structure that is connected to the frame through the suspension and has wheels installed at both ends. The drive axle is mainly composed of the main reducer, differential, half shaft and drive axle housing. The wheel-side half shaft is a solid shaft that transmits the torque transmitted by the differential to the wheels, drives the wheels and propels the vehicle to travel. It is a key structural component in the wheel-side reduction drive axle. The wheel-side half shaft needs to withstand torsional loads and complex and sudden impact loads during service, so the strength and toughness of the wheel-side half shaft material must have a relatively good matching relationship. At present, most half shaft products are manufactured and produced using medium-carbon alloy steels such as 40Cr and 42CrMo. The mechanical properties are stable, but a large amount of consumption will be generated during the quenching and tempering heat treatment process, which increases the production process and cost. At the same time, under the double "sandwich" of long-distance railway transportation and short-distance transportation advantages of new energy commercial vehicles, commercial vehicles traditionally used for road transportation urgently need to develop lightweight to meet the challenges. The static torsional strength margin of commercial wheel axles produced under the current traditional manufacturing process is large, but the traditional heat treatment and quenching and straightening process leads to insufficient fatigue performance of the wheel axles, which limits its lightweight design and application. In the present invention, the wheel axles are made of ferrite-pearlite non-quenched and tempered steel, the middle rod of the wheel axles is made of original bars, and the splines at both ends are hot-formed by die forging. In order to ensure the fatigue performance of the wheel axles, the microstructure and properties of the two ends after hot forming need to match the original bars of the rod, so the heating temperature, final forging temperature, cooling rate and other process parameters must be strictly controlled.

[0003] Non-quenched and tempered steel is called green steel. Its main characteristics are micro-alloying and obtaining the ideal mechanical properties required by the product through controlled forging and controlled cooling technology. On the basis of being able to obtain ideal mechanical properties, the quenching + tempering process is eliminated. The advantages of non-quenched and tempered steel are mainly reflected in the following aspects: ① During rough machining of the blank, the structure is ferrite-pearlite, and the hardness is low, which improves the machining performance and reduces tool consumption; ② The quenching and tempering process is omitted. Compared with 42CrMo quenched and tempered steel, non-quenched and tempered steel has comparable mechanical properties and fatigue properties under the premise of comparable raw material costs. This can save manufacturing companies from the long tempering process, reduce energy consumption, and improve production efficiency. The use of non-quenched and tempered steel to produce wheel rim axles can effectively solve problems such as insufficient fatigue performance and energy consumption caused by quenching deformation.

[0004] Domestic enterprises are actively carrying out relevant research on using non-quenched and tempered steel to replace traditional quenched and tempered steel to produce half shafts. Chinese patent CN114107817A involves a non-quenched and tempered steel that replaces normalized heat-treated 45 steel and its application. The non-quenched and tempered steel is mainly adjusted by adjusting the chemical composition so that the strength and plasticity index of the non-quenched and tempered steel reaches the normalized performance index of 45 steel. However, the current research on the precise control of material structure and performance, especially the control technology of the secondary forming process, is still scarce, so non-quenched and tempered half shafts have not been widely used. In the secondary forging process of ferrite-pearlite non-quenched and tempered steel, improper cooling rate control will cause the forging to produce bainite or martensite structure during cooling phase transformation. The characteristics of bainite and martensite structure are quite different from those of ferrite and pearlite structure. When the half shaft is subjected to sudden loads such as torsional impact, cracks are easily generated at different structures with large performance differences, which has a significant adverse effect on the strength and toughness of ferrite-pearlite non-quenched and tempered steel, and seriously limits the application of ferrite-pearlite non-quenched and tempered steel in high-strength and toughness automotive parts. Therefore, while ensuring that the high-strength and high-toughness medium-carbon ferrite-pearlite non-quenched and tempered steel for the wheel half shaft has high strength and toughness, the matching of the microstructure should be regulated to avoid the generation of martensite or bainite with strip-shaped distribution as much as possible. The proportion matching relationship of pearlite, ferrite, bainite and martensite in the high-strength and high-toughness medium-carbon ferrite-pearlite non-quenched and tempered steel for the wheel half shaft is regulated by means of segmented controlled cooling after forging, so that it has good strength and toughness. Summary of the invention

[0005] The purpose of the present invention is to provide a production method of a commercial vehicle wheel half shaft based on a controlled forging and controlled cooling process, wherein the controlled forging and controlled cooling process is the key. After being processed by the process, the microstructure of the splines at both ends of the commercial vehicle wheel half shaft is a ferrite + pearlite structure, and a small amount of bainite structure distributed in a strip shape, wherein the proportion of pearlite + ferrite structure accounts for 93-96%, the tensile strength Rm is 890-950MPa, the yield strength Rp0.2 is 600-650MPa, the elongation after fracture is between 12% and 15%, the room temperature impact energy AKU is 40-50J, and the Vickers hardness is controlled between 280-300HV.

[0006] The specific technical solutions of the present invention are as follows:

[0007] The invention discloses a non-quenched and tempered steel for a commercial wheel half shaft, wherein the chemical composition by mass percentage is as follows: 0.40%-0.48% C, 0.30%-0.60% Si, 1.1%-1.65% Mn, 0.10%-0.40% Cr, 0.03%-0.18% V, 0.01%-0.03% Ti, 0.01%-0.035% Nb, 0.02%-0.07% Mo, S≤0.01%, P≤0.015%, 0.010%-0.015% N, and the balance is Fe and unavoidable impurities.

[0008] Furthermore, the non-quenched and tempered steel for the commercial vehicle wheel half shaft comprises the following chemical components in percentage by mass: 0.40% to 0.48% C, 0.40% to 0.60% Si, 1.3% to 1.65% Mn, 0.20% to 0.40% Cr, 0.08% to 0.12% V, 0.02% to 0.03% Ti, 0.01% to 0.020% Nb, 0.04% to 0.07% Mo, S≤0.01%, P≤0.015%, 0.010% to 0.015% N, and the balance is Fe and unavoidable impurities;

[0009] The present invention provides a controlled forging and controlled cooling process for producing a wheel side axle by using the non-quenched and tempered steel for the commercial vehicle wheel side axle. The main process flow is as follows: ① bar material cutting → ② medium frequency induction furnace heating and heat preservation of the ends of the axle → ③ die forging of the ends → ④ online controlled cooling → ⑤ machining and gear rolling → ⑥ medium frequency surface induction quenching → ⑦ beating, straightening, and fine turning → ⑧ shot blasting → ⑨ flaw detection → ⑩ strong shot peening → Inspection and storage.

[0010] In step ④, a segmented cooling method of first rapid cooling and then air cooling is used for cooling control.

[0011] Furthermore, the controlled forging and controlled cooling process for producing the wheel side axle of the commercial vehicle wheel side axle with non-quenched and tempered steel is specifically as follows:

[0012] (1) Medium frequency induction heating process: The ferrite-pearlite non-quenched and tempered steel bar is heated by medium frequency induction until it is completely austenitized. The austenitization heating temperature is 950-1020°C, and the holding time is 1-2 minutes, followed by die forging;

[0013] (2) Controlled forging and controlled cooling process: The non-quenched and tempered steel bars are forged after austenitization, and the final forging temperature is 890-940℃. After forging, the bars are controlled to cool online, and the cooling is carried out in a segmented cooling method of first rapid cooling and then air cooling. After forging, the bars are rapidly cooled to 450-500℃, and then air cooled to room temperature. The cooling rate of rapid cooling is 0.5-0.8℃ / s.

[0014] In the above technical solution, the induction heating temperature is 950-1020°C. If the heating temperature is too low, the forgeability of the forging will be deteriorated and the austenitization of the steel will be uneven; while if the heating temperature is too high, it will easily cause overheating, overburning and coarse grains of the forging, which is not conducive to obtaining the target structure and performance, resulting in a decrease in the product yield.

[0015] In the above technical solution, the holding time is 1 to 2 minutes. If the heating time is too short, the austenitization will be incomplete and uneven, while if it is too long, the austenite grains will be coarsened, which is also not conducive to obtaining the target structure and performance and reduces production efficiency.

[0016] In the above technical solution, the final forging temperature is 890-940° C. If the forging temperature is too high, the microstructure will be coarse and the toughness will be reduced; if the forging temperature is too low, it is easy to forge cracks, and the equipment cannot forge, and the equipment capacity does not allow it.

[0017] In the above technical scheme, the controlled cooling process is a segmented cooling method of slow cooling followed by air cooling, first fast cooling to 450-500°C, then air cooling, and the rapid cooling (0.5-0.8°C / s) is to allow the steel to fully undergo phase transformation in the pearlite transformation zone, maximize the pearlite + ferrite structure, and reduce the proportion of bainite or martensite structure.

[0018] The present invention provides a commercial vehicle non-quenched and tempered steel wheel half shaft, which is obtained by adopting the above-mentioned controlled forging and controlled cooling process and production method.

[0019] The spline structure of the two ends of the commercial wheel half shaft is mainly ferrite + pearlite, accounting for 93% to 96%; the tensile strength R m 890~950MPa, yield strength R p0.2 The hardness of the steel is 600-650 MPa, the elongation after fracture is between 12% and 15%, the impact energy AKU at room temperature is 40-50 J, and the Vickers hardness is controlled between 280-300 HV. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is the technical roadmap of controlled forging and controlled cooling process;

[0021] Figure 2 , Figure 3 The microstructure morphology of the non-quenched and tempered steel in Example 1 under different viewing fields;

[0022] Figure 4 , Figure 5 The microstructure morphology of the non-quenched and tempered steel in Example 2 under different viewing fields;

[0023] Figure 6 , Figure 7 The microstructure morphology of the non-quenched and tempered steel in Example 3 under different viewing fields;

[0024] Figure 8 , Fig. 9 The microstructure morphology of the non-quenched and tempered steel in Comparative Example 4 under different viewing fields;

[0025] Fig.10 , Fig.11 These are the organizational morphologies of the non-quenched and tempered steel in Comparative Example 5 under different viewing fields. DETAILED DESCRIPTION

[0026] A high-strength and high-toughness medium-carbon ferrite-pearlite non-quenched and tempered steel for a wheel rim half shaft has the following chemical composition in mass percentage: 0.46% C, 0.46% Si, 1.36% Mn, 0.013% P, 0.002% S, 0.25% Cr, 0.05% Mo, 0.082% V, 0.02% Ti, 0.017Nb, 0.0126% N, and the balance is Fe.

[0027] The controlled forging and controlled cooling process parameters used in Examples 1 to 5 are shown in Table 1, and the microstructure photos are shown in Figures 2 to 11 As shown, the proportion of microstructures and mechanical properties are shown in Table 2. It can be seen that after controlled cooling by a segmented cooling method of first rapid cooling and then air cooling, the microstructures of Example 1, Example 2, and Example 3 are basically composed of ferrite + pearlite, and there are also a small amount of bainite or martensite structures distributed in strips. After controlled forging and controlled cooling, Example 1 has a pearlite + ferrite structure content of 96.9%, an original austenite grain size of 24.88μm, a tensile strength of 930MPa, a yield strength of 638MPa, an impact energy AKU of 48J at room temperature, and a Vickers hardness of 292HV; After controlled forging and controlled cooling, Example 2 has a pearlite + ferrite structure content of 95.7%, an original austenite grain size of 17.01μm, a tensile strength of 950MPa, a yield strength of 649MPa, an impact energy AKU of 44J at room temperature, and a Vickers hardness of 298HV; After controlled forging and controlled cooling, the pearlite + ferrite structure content of Example 3 is 93.0%, the original austenite grain size is 26.19μm, the tensile strength is 890MPa, the yield strength is 605MPa, the room temperature impact energy AKU is 46J, and the Vickers hardness is 283HV; After controlled forging and controlled cooling, the pearlite + ferrite structure content of Comparative Example 4 and Comparative Example 5 is only 64.8% and 63.2%, respectively, and the bainite + martensite structure accounts for more than 35%, which exceeds the technical agreement value by a lot, and therefore the mechanical properties are not tested.

[0028] It can be seen that after the controlled forging and controlled cooling process of the present invention, the microstructure of the spline end of the wheel side half shaft is mainly ferrite + pearlite, the proportion of pearlite + ferrite structure is 93-96%, the tensile strength Rm is 890-950 MPa, the yield strength Rp0.2 is 600-650 MPa, the elongation after fracture is between 12% and 18%, the room temperature impact energy AKU is 40-50 J, and it has a suitable Vickers hardness, and the hardness is controlled between 280 and 300 HV.

[0029] Table 1 Controlled forging and controlled cooling process parameters used in the embodiment

[0030] serial number Heating temperature / ℃ Final forging temperature / ℃ Cooling speed℃ / s Example 1 950 890 0.5→air cooling Example 2 1000 920 0.5→air cooling Example 3 1000 950 0.75→air cooling Comparative Example 4 950 920 1→air cooling Comparative Example 5 1000 890 1→air cooling

[0031] Table 2 Main tissue content and mechanical properties after treatment in Example

[0032]

Claims

1. A method for producing a commercial vehicle wheel half-axle based on a controlled forging and controlled cooling process, characterized in that: The method comprises the following steps: ① bar blanking → ② the ends of the bar are heated to 950-1050°C in a medium frequency induction furnace and kept warm for 1-2 minutes → ③ the ends are die forged with a deformation of 7%-20%, and the final forging temperature is controlled at 890-920°C → ④ a segmented cooling method of first fast cooling and then slow cooling is adopted, with a fast cooling rate of 0.5-0.8°C / s, and air cooling is performed after cooling to 450-500°C → ⑤ machining, and 3-7 passes of tooth rolling are performed on both ends to form splines → ⑥ medium frequency surface induction quenching → ⑦ beating, straightening, and precision turning → ⑧ shot blasting to remove burrs → ⑨ flaw detection, checking internal and external defects of the material → ⑩ strong shot peening, introducing surface residual compressive stress → Inspection and storage.

2. The method for producing a commercial vehicle wheel half-axle based on controlled forging and controlled cooling process according to claim 1, characterized in that: In the step ①, the rod material is ferrite-pearlite non-quenched and tempered steel.

3. The method for producing a commercial vehicle wheel half-axle based on controlled forging and controlled cooling process according to claim 1, characterized in that: In the step ②, the heating temperature of the two ends of the rod is 950-1050° C., and the holding time is 1-2 minutes to make it completely austenitized.

4. The method for producing a commercial vehicle wheel half-axle based on controlled forging and controlled cooling process according to claim 1, characterized in that: In the step ③, only the ends of the half shaft are die forged to form a spline blank, and the final forging temperature is controlled at 890-920°C.

5. The method for producing a commercial vehicle wheel half-axle based on controlled forging and controlled cooling process according to claim 1, characterized in that: In step ④, after die forging, a staged cooling method of first rapid cooling and then air cooling is adopted, and the rapid cooling adopts fan blast cooling, and the cooling rate is 0.5-0.8°C / s. After rapid cooling to 450-500°C, an air cooling process is adopted.

6. A commercial vehicle wheel half shaft based on controlled forging and controlled cooling process, characterized in that: The product is produced by the manufacturing process described in any one of claims 1 to 5.

7. The commercial vehicle wheel half shaft based on controlled forging and controlled cooling process according to claim 6 is characterized in that: The microstructure of the splines at both ends of the commercial vehicle wheel half-axle is 93% to 96% pearlite + ferrite, and 4% to 7% bainite and martensite distributed in a band shape.

8. The commercial vehicle wheel half shaft based on controlled forging and controlled cooling process according to claim 7, characterized in that: The tensile strength Rm of the splines at both ends of the commercial wheel half-axle is 890-950MPa, the yield strength Rp0.2 is 600-650MPa, the elongation after fracture is between 12-15%, the room temperature impact energy AKU is 40-50J, and the Vickers hardness is controlled between 280-300HV.

Citation Information

Patent Citations

  • Ferrite and pearlite type bainite control method for non-quenched and tempered steel crankshaft forged piece

    CN106555114A

  • Manufacturing process of vehicle hollow half shaft

    CN107283122A

  • Non-quenched-tempered half axle and manufacturing method thereof

    CN107470852A

  • Non-quenched-tempered brake camshaft and manufacturing method thereof

    CN107470853A

  • Electric driving shaft non-quenched and tempered steel material and production process

    CN111390512A