Preparation method of metal monatomic doped graphene wave-absorbing material
By introducing metal single atom doping and N coordination atoms into graphene, electric dipoles and structural distortions are formed, which solves the problem of graphene's insufficient absorption performance at low filling amounts and achieves efficient electromagnetic wave absorption.
Patent Information
- Application Number
- CN202410729410.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-08
AI Technical Summary
At low filling amounts, graphene has poor dielectric loss strength, narrow absorption frequency band, and weak absorption performance, resulting in its poor performance in the field of electromagnetic wave absorption.
Using the preparation method of metal single atom doped graphene, single atom Fe-N4 is embedded into reduced graphene oxide through the N coordination atom-assisted strategy, and the conductivity, dielectric parameters and wave absorption properties are adjusted to form an electric dipole and introduced Structural distortion and interface polarization, enhanced conductivity loss and polarization loss.
The electrical properties of graphene are effectively controlled at low filling amounts to achieve lightweight, broadband and efficient wave absorption performance. The maximum absorption intensity reaches -74.05dB and the maximum effective bandwidth is 4.34GHz. It is suitable for electromagnetic wave absorption materials.
Smart Images

Figure CN118744983A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of electromagnetic wave absorbing materials, and in particular to a method for preparing a metal single atom doped graphene absorbing material. Background Art
[0002] With the rapid development of modern science and technology, electromagnetic radiation pollution has become increasingly serious due to the widespread use of electronic equipment. Electromagnetic radiation not only interferes with the normal operation of equipment, but also harms the environment and human health. The design and preparation of high-performance electromagnetic wave absorbing materials has become a research hotspot for protecting electronic equipment and the human body from electromagnetic interference and radiation. Carbon-based materials such as graphite, carbon black, carbon nanotubes, graphene, etc. have become a new type of electromagnetic wave absorbing material with great application potential due to their advantages such as low density, large specific surface area, high conductivity, large dielectric loss, and stable physical and chemical properties.
[0003] Graphene is a two-dimensional carbon-based material composed of a single layer of carbon atoms. It has unique electronic properties and excellent electron transport capabilities, and has broad application prospects in the field of wave absorption. However, due to the contradiction between graphene's filler loading, impedance matching and loss intensity, the wave absorption performance obtained directly from graphene is not ideal. Studies have shown that pure graphene absorbers can only achieve ideal wave absorption performance when the filling amount is greater than 5wt%. Therefore, how to regulate the electrical properties of graphene at a low filling amount and achieve the coordinated optimization of impedance matching and high attenuation has become an important challenge in the field of wave absorption.
[0004] So far, researchers have tried many strategies to adjust the conductivity of graphene, such as vacancies, chemical doping, network structure, surface adsorption, and external electric field. Considering the structural stability, process complexity, and repeatability, heterogeneous atom doping is undoubtedly an effective means to regulate the electrical and dielectric properties of graphene to obtain good wave absorption performance. Summary of the invention
[0005] The present invention is to solve the technical problems of poor dielectric loss strength, narrow absorption band and weak absorption performance of graphene under low filling amount, and proposes a preparation method of metal single atom doped graphene absorbing material.
[0006] A method for preparing a metal single atom doped graphene absorbing material is specifically carried out according to the following steps:
[0007] Step 1: placing graphene oxide powder in deionized water and ultrasonically stirring to obtain a graphene oxide suspension;
[0008] Step 2: adding urea powder into the graphene oxide suspension obtained in step 1, and stirring with magnetic force to obtain a graphene oxide mixed solution;
[0009] Step 3, placing ferric chloride hexahydrate into deionized water and stirring it magnetically until it is completely dissolved to obtain a ferric chloride solution;
[0010] Step 4: adding the ferric chloride solution obtained in step 3 to the graphene oxide mixed solution obtained in step 2, and magnetically stirring to obtain a uniformly dispersed metal salt graphene oxide mixed solution containing a nitrogen source;
[0011] Step 5: Freeze the metal salt graphene oxide mixed solution containing a nitrogen source obtained in step 4 into a solid, and then place it in a freeze dryer for freeze drying; then place it in a tubular furnace for thermal reduction under an inert protective atmosphere to obtain a black solid powder, which is the metal single atom doped graphene absorbing material, and the preparation is completed.
[0012] The present invention adopts the N-coordinated atom-assisted strategy to embed single-atom Fe-N4 into reduced graphene oxide, and establishes the relationship between conductivity, dielectric parameters and wave absorption performance at the atomic scale. The 3d-2p orbital hybridization in Fe-N induces the formation of electric dipoles, resulting in dipole polarization. The resulting electron migration leads to enhanced conductivity loss, effectively adjusting the impedance matching characteristics of graphene. In addition, the introduction of heterogeneous atoms causes the graphene sheet structure to be distorted, increasing defect-induced polarization and interface polarization, thereby synergistically promoting electromagnetic wave energy loss.
[0013] The beneficial effects of the present invention are:
[0014] The present invention adjusts the graphene band gap and electrical properties by introducing heterogeneous atoms at a low filling content, thereby effectively regulating the graphene conductivity loss and polarization loss mechanism to achieve lightweight, broadband and high-efficiency wave absorbing performance.
[0015] (1) The single-atom-doped graphene absorbing material of the present invention has a simple preparation process, low cost, and can be produced on a large scale.
[0016] (2) Since the graphene network structure has a strong CC covalent bond and a high energy barrier, the present invention uses N atoms as a "bridge" to effectively solve the problem of directly doping transition metal atoms in graphene.
[0017] (3) In the single-atom doped graphene absorber prepared by the method of the present invention, Fe-N can act as a polarization center to increase dipole polarization, and the introduction of heterogeneous atoms produces structural distortion to cause defect-induced polarization. In addition, the electron migration inside Fe further leads to conductivity loss, thereby synergistically promoting energy attenuation.
[0018] (4) The single-atom doped graphene absorbing material prepared by the method of the present invention has high-efficiency absorbing performance. When the filling amount is 1wt%, the maximum absorption intensity is -74.05dB, the maximum effective bandwidth is 4.34GHz, and the matching thickness is 2.0mm. The present invention provides a new and important reference for achieving "light, thin, wide, and strong" electromagnetic wave absorption performance.
[0019] The single-atom doped graphene absorbing material prepared by the method of the present invention is applied in the field of electromagnetic wave absorbing materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 XRD spectra of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1 and the comparative samples of RGO, Fe / RGO and N-RGO;
[0021] Figure 2 TEM image of RGO comparison sample;
[0022] Figure 3 Microscopic images of Fe / RGO comparative samples, where (a) is a TEM image, (b) is a HRTEM image, and (c) is a SAED image;
[0023] Figure 4 TEM image of N-RGO comparison sample;
[0024] Figure 5 The microscopic images of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1, wherein (a) is a TEM image, (b) is a HRTEM image, and (c) is a SAED image;
[0025] Figure 6 This is a HAADF-STEM image of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1, wherein Figure (b) is a partial enlarged view of Figure (a);
[0026] Figure 7 The Fe2p and N1s fine spectra of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1;
[0027] Figure 8 The synchrotron radiation absorption spectrum of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1, wherein (a) is the Fe K-edge XANES spectrum, (b) is the FT-EXAFS curve, (c) is the k-space fitting curve, and (d) is the R-space fitting curve and the atomic structure model diagram;
[0028] Fig. 9KPFM, EFM, and C-AFM images of the metal single atom-doped graphene material (Fe-N-RGO) obtained in step five of Example 1 and the comparative samples RGO and N-RGO, wherein (a1) is the KPFM image of the comparative sample RGO, (a2) is the EFM image of the comparative sample RGO, (a3) is the C-AFM image of the comparative sample RGO, (b1) is the KPFM image of the comparative sample N-RGO, (b2) is the EFM image of the comparative sample N-RGO, (b3) is the C-AFM image of the comparative sample N-RGO, (c1) is the KPFM image of Fe-N-RGO, (c2) is the EFM image of Fe-N-RGO, and (c3) is the C-AFM image of Fe-N-RGO;
[0029] Fig.10 This is the electromagnetic parameter curve of the RGO comparison sample; from the electromagnetic parameters, its dielectric dispersion characteristics are not obvious, the real and imaginary parts of the dielectric constant are low. The real and imaginary parts of the magnetic permeability are 1 and 0 respectively, proving that there is no magnetic loss.
[0030] Fig.11 is a curve diagram of the wave absorption performance of the RGO comparison sample, curve 1 represents 1.0mm thickness, curve 2 represents 1.5mm thickness, curve 3 represents 2.0mm thickness, curve 4 represents 2.5mm thickness, curve 5 represents 3.0mm thickness, curve 6 represents 3.5mm thickness, curve 7 represents 4.0mm thickness, curve 8 represents 4.5mm thickness, curve 9 represents 5.0mm thickness, and curve 10 represents 5.5mm thickness;
[0031] Fig.12 It is the electromagnetic parameter curve of Fe / RGO comparison sample;
[0032] Fig.13 is a curve diagram of the wave absorption performance of the Fe / RGO comparison sample, curve 1 represents 1.0 mm thickness, curve 2 represents 1.5 mm thickness, curve 3 represents 2.0 mm thickness, curve 4 represents 2.5 mm thickness, curve 5 represents 3.0 mm thickness, curve 6 represents 3.5 mm thickness, curve 7 represents 4.0 mm thickness, curve 8 represents 4.5 mm thickness, curve 9 represents 5.0 mm thickness, and curve 10 represents 5.5 mm thickness;
[0033] Fig.14 It is the electromagnetic parameter curve of N-RGO comparison sample;
[0034] Fig.15is a curve diagram of the wave absorption performance of the N-RGO comparison sample, curve 1 represents 1.0 mm thickness, curve 2 represents 1.5 mm thickness, curve 3 represents 2.0 mm thickness, curve 4 represents 2.5 mm thickness, curve 5 represents 3.0 mm thickness, curve 6 represents 3.5 mm thickness, curve 7 represents 4.0 mm thickness, curve 8 represents 4.5 mm thickness, curve 9 represents 5.0 mm thickness, and curve 10 represents 5.5 mm thickness;
[0035] Fig.16 This is a graph of electromagnetic parameters of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1;
[0036] Fig.17 This is a graph of the wave absorption performance of the metal single atom doped graphene material (Fe-N-RGO) obtained in step five of Example 1, where curve 1 represents a thickness of 1.0 mm, curve 2 represents a thickness of 1.5 mm, curve 3 represents a thickness of 2.0 mm, curve 4 represents a thickness of 2.5 mm, curve 5 represents a thickness of 3.0 mm, curve 6 represents a thickness of 3.5 mm, curve 7 represents a thickness of 4.0 mm, curve 8 represents a thickness of 4.5 mm, curve 9 represents a thickness of 5.0 mm, and curve 10 represents a thickness of 5.5 mm. DETAILED DESCRIPTION
[0037] Specific implementation method 1: This implementation method is a method for preparing a metal single atom doped graphene absorbing material, which is specifically carried out in the following steps:
[0038] Step 1: placing graphene oxide powder in deionized water and ultrasonically stirring to obtain a graphene oxide suspension;
[0039] Step 2: adding urea powder into the graphene oxide suspension obtained in step 1, and stirring with magnetic force to obtain a graphene oxide mixed solution;
[0040] Step 3, placing ferric chloride hexahydrate into deionized water and stirring it magnetically until it is completely dissolved to obtain a ferric chloride solution;
[0041] Step 4: adding the ferric chloride solution obtained in step 3 to the graphene oxide mixed solution obtained in step 2, and magnetically stirring to obtain a uniformly dispersed metal salt graphene oxide mixed solution containing a nitrogen source;
[0042] Step 5: Freeze the metal salt graphene oxide mixed solution containing a nitrogen source obtained in step 4 into a solid, and then place it in a freeze dryer for freeze drying; then place it in a tubular furnace for thermal reduction under an inert protective atmosphere to obtain a black solid powder, which is the metal single atom doped graphene absorbing material, and the preparation is completed.
[0043] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the concentration of the graphene oxide suspension in step 1 is 4-10 mg / mL. Other aspects are the same as those in specific embodiment 1.
[0044] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that: in the ultrasonic stirring process described in step one, the ultrasonic time is controlled to be 1 to 3 hours, the power is 500 to 100 W, the magnetic stirring is 1 to 4 hours, and the stirring speed is 300 to 500 r / min.
[0045] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the mass ratio of the urea powder in step 2 to the graphene oxide in the graphene oxide suspension is (1 to 3): 1. The rest is the same as specific embodiments 1 to 3.
[0046] Specific implementation mode 5: This implementation mode is different from specific implementation modes 1 to 4 in that the magnetic stirring time in step 2 is 1 to 4 hours, and the stirring speed is 300 to 500 r / min. The rest is the same as specific implementation modes 1 to 4.
[0047] Specific implementation method 6: This implementation method is different from the specific implementation methods 1 to 5 in that the concentration of ferric chloride hexahydrate added in step 3 is 2 to 10 mg / mL. The rest is the same as the specific implementation methods 1 to 5.
[0048] Specific implementation method 7: This implementation method is different from specific implementation methods 1 to 6 in that: in the stirring process described in step 3, the magnetic stirring time is controlled to be 0.5 to 1 h, and the stirring speed is 300 to 500 r / min. Other aspects are the same as specific implementation methods 1 to 6.
[0049] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that the mass ratio of ferric chloride hexahydrate in the ferric chloride solution and graphene oxide in the graphene oxide mixed solution in step 4 is 0.06:1. Others are the same as specific embodiments 1 to 7.
[0050] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the magnetic stirring time in step 4 is 3 to 6 hours and the magnetic stirring speed is 300 to 500 r / min. The rest is the same as specific embodiments 1 to 8.
[0051] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: the freeze-drying time in step 5 is 24 to 48 hours, the temperature is -60°C, and the pressure is 0.1 Pa; during the thermal reduction process, the inert protective atmosphere is a nitrogen atmosphere or an argon atmosphere, the heating rate is controlled to be 5 to 10°C / min, the temperature is 600 to 900°C, and the insulation time is 1 to 3 hours. Others are the same as specific embodiments 1 to 9.
[0052] The content of the present invention is not limited to the content of the above-mentioned embodiments. The combination of one or several specific embodiments can also achieve the purpose of the invention.
[0053] Embodiment 1:
[0054] The present embodiment provides a method for preparing a metal single atom doped graphene absorbing material (Fe-N-RGO), which is specifically carried out in the following steps:
[0055] Step 1: Place 1 g of graphene oxide powder in 200 mL of deionized water and ultrasonicate for 2 h at a power of 800 W, a magnetic stirring time of 3 h, and a stirring speed of 400 r / min to obtain a uniformly dispersed graphene oxide suspension with a concentration of 5 mg / mL;
[0056] Step 2: Add 2.4 g of urea powder into the graphene oxide suspension obtained in step 1, and stir magnetically for 2 h at a stirring speed of 400 r / min to obtain a graphene oxide mixed solution;
[0057] Step 3: Place 60 mg of ferric chloride hexahydrate into 10 mL of deionized water and stir magnetically until completely dissolved. The stirring time is controlled to be 2 h and the stirring speed is 400 r / min to obtain a ferric chloride solution.
[0058] Step 4: adding the ferric chloride solution obtained in step 3 to the graphene oxide mixed solution obtained in step 2, and magnetically stirring for 4 hours at a stirring speed of 400 r / min to obtain a uniformly dispersed metal salt graphene oxide mixed solution containing a nitrogen source;
[0059] Step 5. The metal salt graphene oxide mixed solution containing a nitrogen source obtained in step 4 is sealed and placed in a refrigerator, frozen into a solid for 14 hours, and then placed in a freeze dryer, the temperature is controlled to be -60°C, the pressure is 0.1Pa, and freeze-dried for 36 hours; then placed in a tubular furnace for thermal reduction under an inert protective atmosphere, the inert protective atmosphere is an argon atmosphere, the heating rate is controlled to be 5°C / min, the temperature is 800°C, and the insulation time is 1 hour to obtain a black solid powder, which is the metal single atom doped graphene absorbing material (Fe-N-RGO), and the preparation is completed.
[0060] Preparation of test samples:
[0061] The metal single atom doped graphene absorbing material (Fe-N-RGO) prepared in Example 1 was placed in paraffin at a mass ratio of 1%, heated to 80°C, and kept warm for 0.5h. The sample was placed in a mold to finally obtain a coaxial ring with an outer diameter of 7mm, an inner diameter of 3.04mm, and a height of 2mm.
[0062] RGO comparison sample:
[0063] The 200 mL graphene oxide suspension obtained in step 1 of Example 1 was sealed and placed in a refrigerator to freeze into a solid for 14 h, and then placed in a freeze dryer for freeze drying for 36 h at a temperature of -60 ° C and a pressure of 0.1 Pa; finally, it was placed in a tubular furnace for thermal reduction under an inert protective atmosphere, the inert protective atmosphere was an argon atmosphere, the heating rate was controlled to be 5 ° C / min, the temperature was 800 ° C, and the insulation time was 1 h to obtain a black solid powder, and an RGO comparison sample was obtained.
[0064] Fe / RGO comparison sample:
[0065] The ferric chloride solution of step three of Example 1 is slowly added to the graphene oxide suspension of step one, and a uniformly dispersed mixed solution is obtained by magnetic stirring, the magnetic stirring time is 4 hours, and the stirring speed is 400r / min; after sealing, it is placed in a refrigerator and frozen into a solid, the refrigeration time is 14 hours, and then placed in a freeze dryer for freeze drying for 36 hours, the temperature is -60°C, and the pressure is 0.1Pa; finally, it is placed in a tubular furnace for thermal reduction under an inert protective atmosphere, the inert protective atmosphere is an argon atmosphere, the heating rate is controlled to be 5°C / min, the temperature is 800°C, and the insulation time is 1 hour to obtain a black solid powder, and an Fe / RGO comparison sample is obtained.
[0066] N-RGO comparison sample:
[0067] The mixed solution of urea and graphene oxide in step 2 of Example 1 was sealed and placed in a refrigerator to freeze into a solid for 14 hours, and then placed in a freeze dryer for 36 hours at a temperature of -60°C and a pressure of 0.1 Pa. Finally, it was placed in a tubular furnace for thermal reduction under an inert protective atmosphere, the inert protective atmosphere was an argon atmosphere, the heating rate was controlled to be 5°C / min, the temperature was 800°C, and the insulation time was 1 hour to obtain a black solid powder, and a Fe / RGO comparison sample was obtained.
[0068] The RGO, Fe / RGO and N-RGO comparison samples were prepared as test samples in the same manner as in Example 1.
[0069] The metal single atom doped graphene absorbing material (Fe-N-RGO) prepared in Example 1 was tested together with RGO, Fe / RGO, and N-RGO comparative samples.
[0070] Figure 1 This is the XRD spectrum of the metal single atom doped graphene material (Fe-N-RGO) obtained in step five of Example 1 and the comparison samples of RGO, Fe / RGO, and N-RGO. It can be seen from the figure that the sample is mainly composed of the "mantou peak" of RGO, the crystallinity of carbon is poor, and it exists in the form of amorphous carbon.
[0071] Figure 2 This is the TEM image of the RGO comparison sample. Figure 3 The microscopic images of the Fe / RGO comparison sample, where (a) is the TEM image, (b) is the HRTEM image and (c) is the SAED image. It can be seen from the figures that in the absence of N atoms, Fe is uniformly dispersed on RGO in the form of particles of ~10 nm. Figure 4 This is the TEM image of the N-RGO comparison sample, and its morphology is consistent with that of RGO.
[0072] Figure 5 The microscopic images of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1, wherein (a) is a TEM image, (b) is a HRTEM image, and (c) is a SAED image. It can be seen from the figure that its morphology is consistent with that of RGO and is amorphous carbon. This indicates that Fe and N mainly exist in RGO in atomic form.
[0073] Figure 6 This is a HAADF-STEM image of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1, where Figure (b) is a partial enlarged view of Figure (a); the isolated bright spots marked with circles in the figure represent partially dispersed Fe atoms, because the atomic number is much larger than that of C. It can be observed that the iron atoms are uniformly dispersed in Fe-N-RGO.
[0074] Figure 7 The Fe2p and N1s fine spectra of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1. The Fe 2p spectrum curve fitting found that there were two typical peaks at 710.1 and 723.7 eV, which are Fe2p 3 / 2 and Fe 2p 1 / 2 . Specifically, it can be divided into: Fe 2+ 2p 3 / 2 (709.6eV), Fe 3+ 2p 3 / 2 (711.7eV), Fe 2+ 2p 1 / 2 (723.6eV) and Fe 3+ 2p 1 / 2 (725.5eV), proving the presence of Fe in the sample 2+ and Fe 3+The N1s spectrum can be decomposed into pyridinic N (398.2 eV), Fe-Nx (398.8 eV), pyridinic N (399.7 eV) and graphitic N (401.4 eV). Fe-N is formed by the interaction between pyridinic N and isolated metallic Fe atoms in RGO, indicating that the introduction of N atoms can effectively promote the formation of Fe-N configuration.
[0075] Figure 8 This is the synchrotron radiation absorption spectrum of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1. It can be seen from the figure that no additional peak is observed at 7110.5 eV, indicating that it is a planar structure. From the Fourier transform EXAFS analysis of the bonding characteristics of Fe, it can be seen that Fe-N-RGO does not show obvious Fe-Fe interaction This indicates that Fe is atomically dispersed, which is consistent with the results of HAADF-STEM. There is an obvious peak at the Fe-N bond with a coordination number of 3.9. This indicates that the four N atoms form a planar structure centered on the Fe atom.
[0076] Fig. 9 KPFM, EFM, C-AFM images of metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of embodiment 1 and comparison samples RGO and N-RGO. It can be seen from the figure that the surface potential, phase and current distribution image of RGO are all at a lower value (dark area). The electrical signal intensity of N-RGO and Fe-N-RGO gradually increases, and the color distribution is uniform (bright area). It is mainly attributed to the following aspects: First, the surface potential difference proves that the Fermi level of graphene has changed due to the doping of Fe atoms. Secondly, the doping of Fe and N atoms forms a strong electric dipole (NC and Fe-NC), which enhances the internal potential and charge accumulation, resulting in a higher surface charge distribution. Third, due to the electron migration of dopants to graphene, the conductivity of graphene is enhanced, and the surface current distribution image shows an increasing trend.
[0077] Fig.10 This is the electromagnetic parameter curve of the RGO comparison sample; from the electromagnetic parameters, its dielectric dispersion characteristics are not obvious, the real and imaginary parts of the dielectric constant are low. The real and imaginary parts of the magnetic permeability are 1 and 0 respectively, proving that there is no magnetic loss.
[0078] Fig.11The curve diagram of the wave absorption performance of the RGO comparison sample shows that curve 1 represents 1.0mm thickness, curve 2 represents 1.5mm thickness, curve 3 represents 2.0mm thickness, curve 4 represents 2.5mm thickness, curve 5 represents 3.0mm thickness, curve 6 represents 3.5mm thickness, curve 7 represents 4.0mm thickness, curve 8 represents 4.5mm thickness, curve 9 represents 5.0mm thickness, and curve 10 represents 5.5mm thickness. The wave absorption performance is not shown at the thickness of 1 to 5.5mm, and the reflection loss values are all greater than -10dB.
[0079] Fig.12 This is the electromagnetic parameter curve of the Fe / RGO comparison sample. Compared with the pure RGO comparison sample, its dielectric parameters are relatively improved, showing a dielectric dispersion trend.
[0080] Fig.13 The wave absorption performance curve of the Fe / RGO comparison sample, curve 1 represents 1.0mm thickness, curve 2 represents 1.5mm thickness, curve 3 represents 2.0mm thickness, curve 4 represents 2.5mm thickness, curve 5 represents 3.0mm thickness, curve 6 represents 3.5mm thickness, curve 7 represents 4.0mm thickness, curve 8 represents 4.5mm thickness, curve 9 represents 5.0mm thickness, and curve 10 represents 5.5mm thickness. It can be seen from the figure that compared with the RGO comparison sample, the wave absorption performance is slightly improved. When the matching thickness is 5.5mm, the filling amount is 1wt%, and the frequency is 18GHz, the maximum reflection loss is -13.56dB.
[0081] Fig.14 This is the electromagnetic parameter curve of the N-RGO comparison sample. Compared with the RGO and Fe / RGO comparison samples, its dielectric parameters are enhanced, showing an obvious dielectric dispersion trend.
[0082] Fig.15 The wave absorption performance curve of the N-RGO comparison sample, curve 1 represents 1.0mm thickness, curve 2 represents 1.5mm thickness, curve 3 represents 2.0mm thickness, curve 4 represents 2.5mm thickness, curve 5 represents 3.0mm thickness, curve 6 represents 3.5mm thickness, curve 7 represents 4.0mm thickness, curve 8 represents 4.5mm thickness, curve 9 represents 5.0mm thickness, and curve 10 represents 5.5mm thickness. Compared with the RGO and Fe / RGO comparison samples, the wave absorption performance is significant. When the matching thickness is 3.5mm, the filling amount is 1wt%, and the frequency is 7.97GHz, the maximum reflection loss is -45.27dB.
[0083] Fig.16This is a graph of electromagnetic parameters of the metal single atom doped graphene material (Fe-N-RGO) obtained in step five of Example 1. It can be seen that its dielectric parameter phase exhibits obvious dielectric dispersion characteristics and exhibits obvious polarization peaks due to the enhancement of dipole polarization.
[0084] Fig.17 The wave absorption performance curve of the metal single atom doped graphene material (Fe-N-RGO) obtained in step 5 of Example 1 is shown in Fig. 1. Curve 1 represents a thickness of 1.0 mm, curve 2 represents a thickness of 1.5 mm, curve 3 represents a thickness of 2.0 mm, curve 4 represents a thickness of 2.5 mm, curve 5 represents a thickness of 3.0 mm, curve 6 represents a thickness of 3.5 mm, curve 7 represents a thickness of 4.0 mm, curve 8 represents a thickness of 4.5 mm, curve 9 represents a thickness of 5.0 mm, and curve 10 represents a thickness of 5.5 mm. It can be seen that the wave absorption strength is strong. When the matching thickness is 2.0 mm, the filling amount is 1 wt%, and the frequency is 12.22 GHz, the maximum reflection loss is -74.05 dB, and the effective absorption bandwidth is 4.34 GHz (10.67-15.01 GHz).
Claims
1. A method for preparing a metal single atom doped graphene absorbing material, Features The method is specifically carried out in the following steps: Step 1: placing graphene oxide powder in deionized water and ultrasonically stirring to obtain a graphene oxide suspension; Step 2: adding urea powder into the graphene oxide suspension obtained in step 1, and stirring with magnetic force to obtain a graphene oxide mixed solution; Step 3, placing ferric chloride hexahydrate into deionized water and stirring it magnetically until it is completely dissolved to obtain a ferric chloride solution; Step 4: adding the ferric chloride solution obtained in step 3 to the graphene oxide mixed solution obtained in step 2, and magnetically stirring to obtain a uniformly dispersed metal salt graphene oxide mixed solution containing a nitrogen source; Step 5: Freeze the metal salt graphene oxide mixed solution containing a nitrogen source obtained in step 4 into a solid, and then place it in a freeze dryer for freeze drying; then place it in a tubular furnace for thermal reduction under an inert protective atmosphere to obtain a black solid powder, which is the metal single atom doped graphene absorbing material, and the preparation is completed.
2. The method for preparing a metal single atom doped graphene absorbing material according to claim 1, Features The concentration of the graphene oxide suspension in step 1 is 4-10 mg / mL.
3. The method for preparing a metal single atom doped graphene absorbing material according to claim 1, Features In the ultrasonic stirring process of step 1, the ultrasonic time is controlled to be 1 to 3 hours, the power is 500 to 100 W, the magnetic stirring is 1 to 4 hours, and the stirring speed is 300 to 500 r / min.
4. The method for preparing a metal single atom doped graphene absorbing material according to claim 1, Features The mass ratio of the urea powder in step 2 to the graphene oxide in the graphene oxide suspension is (1-3):
1.
5. The method for preparing a metal single atom doped graphene absorbing material according to claim 1, Features The magnetic stirring time in step 2 is 1 to 4 hours, and the stirring speed is 300 to 500 r / min.
6. The method for preparing a metal single atom doped graphene absorbing material according to claim 1, Features The addition concentration of ferric chloride hexahydrate in step 3 is 2-10 mg / mL.
7. The method for preparing a metal single atom doped graphene absorbing material according to claim 1, Features In the stirring process of step 3, the magnetic stirring time is controlled to be 0.5 to 1 h, and the stirring speed is controlled to be 300 to 500 r / min.
8. The method for preparing a metal single atom doped graphene absorbing material according to claim 1, Features The mass ratio of the ferric chloride hexahydrate in the ferric chloride solution and the graphene oxide in the graphene oxide mixed solution in step 4 is 0.06:
1.
9. The method for preparing a metal single atom doped graphene absorbing material according to claim 1, Features The magnetic stirring time in step 4 is 3 to 6 hours, and the magnetic stirring speed is 300 to 500 r / min.
10. The method for preparing a metal single atom doped graphene absorbing material according to claim 1, Features The freeze-drying time in step 5 is 24 to 48 hours, the temperature is -60°C, and the pressure is 0.1 Pa; during the thermal reduction process, the inert protective atmosphere is a nitrogen atmosphere or an argon atmosphere, the heating rate is controlled at 5 to 10°C / min, the temperature is 600 to 900°C, and the insulation time is 1 to 3 hours.
Citation Information
Patent Citations
Method for preparing nitrogen doped reduced graphene oxide aerogel wave-absorbing material
CN108946711A
Preparation method of iron-doped graphite-like carbon nitride / graphene multifunctional nano-composite material
CN111453804A
Nitrogen-doped graphene nickel ferrite composite wave-absorbing material and preparation method thereof
CN112375541A
Preparation method of doped graphene
CN113912051A
Microwave preparation and application of metal monatomic doped reduced graphene oxide dielectric material
CN116750754A
Cited By
Graphene-based metal composite wave-absorbing material as well as preparation method and application thereof
CN119873805A