Carbon nanomaterial compound capable of realizing high dispersion stability and preparation method thereof

By combining ultrasonic dispersion and mechanical stirring, a low-dimensional multi-scale structure of graphene/carbon nanotubes/conductive carbon black is built, which solves the problem of poor dispersion and stability of carbon nanomaterials and achieves high dispersion stability and structural integrity. , simplifying the dispersion process and expanding the application fields.

CN118744985AActive Publication Date: 2024-10-08BEIJING UNIV OF TECH

Patent Information

Application Number
CN202410714906.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-08
Estimated Expiration
2044-06-04

AI Technical Summary

Technical Problem

The dispersion process of existing carbon nanomaterials is complex, the dispersion is poor and unstable, and the commonly used solvents are mostly toxic liquids, which are not conducive to transportation and storage.

Method used

Through four steps of impurity removal, dispersion, drying and use, a combination of ultrasonic dispersion and mechanical stirring is used to build a low-dimensional multi-scale three-dimensional structure of graphene/carbon nanotubes/conductive carbon black to form a carbon with high dispersion stability. Nanomaterial composite powder is suitable for re-dispersion in different solvents.

Benefits of technology

It achieves high dispersion stability without the addition of dispersants and without loss of structure, simplifies the dispersion process, ensures the excellent mechanical, thermal, and electrical properties of carbon nanomaterials, and expands its application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a carbon nanomaterial compound capable of realizing high dispersion stability and a preparation method thereof, and belongs to the field of dispersion processes of carbon nanomaterials. The preparation method comprises the following steps: removing impurities from graphene, carbon nanotubes and conductive carbon black, independently preparing a dispersion liquid, carrying out mixed ultrasonic dispersion, heating and stirring until the mixture is pasty, and carrying out vacuum drying, grinding and re-dispersion. Unique geometric structures of graphene, carbon nanotubes and conductive carbon black are mutually dispersed, the carbon tubes are connected with wide gaps between the carbon tubes, between the carbon tubes and the graphene and between the graphene, and the conductive carbon black is dispersed around and fills residual narrow gaps to form a stable three-dimensional network structure, so that high dispersion stability of the carbon nanomaterial is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of dispersion of carbon nanomaterials, and in particular relates to a carbon nanomaterial (graphene / carbon nanotube / conductive carbon black) composite capable of achieving high dispersion stability and a preparation method thereof. Background Art

[0002] Carbon nanomaterials such as graphene have good mechanical, electrical and thermal properties and are a good choice as reinforcements for metal-based composites. However, carbon nanomaterials tend to aggregate during use, which limits their application. Take graphene as an example. Its unique thin-layer two-dimensional structure makes it very easy to aggregate in its natural state. Its unique mechanical properties and excellent thermal and electrical conductivity will rapidly decrease as the flakes aggregate.

[0003] In recent years, the main methods to solve graphene dispersion are as follows:

[0004] 1) Physical dispersion method

[0005] The van der Waals forces between the sheets are broken by external force to achieve the dispersion effect. Common methods include mechanical dispersion, ultrasound and microwave radiation.

[0006] 2) Chemical dispersion method

[0007] Graphene is usually dispersed in an aqueous solution or organic solution containing a modifier. The surface of graphene is embedded with modified molecules, and the inter-sheet van der Waals forces are overcome by electrostatic forces or intermolecular forces. Chemical dispersion methods are divided into the following two categories:

[0008] a) Covalent Bond Method

[0009] The edges of graphene oxide often have defects, which can react chemically with other functional groups, such as isocyanate-modified graphene oxide, thereby improving dispersibility.

[0010] b) Non-covalent bond method

[0011] The interaction between the modifier and graphene is utilized to modify the graphene without destroying its structure. Common methods include combining graphene with functional molecules through π-π bonds, ionic bonds, hydrogen bonds or other non-covalent bonds.

[0012] Chinese invention patent (application number CN113200538A) discloses adding dispersant, supplemented by stirring, ball milling and other physical methods, so as to prepare graphene aqueous phase dispersion, but it is difficult to remove dispersant by centrifugal method alone, and the ball milling method may destroy the structure of graphene. Chinese invention patent (application number CN113184841A) discloses solving the dispersion problem of graphene by adding a small amount of organic solvent under mild conditions, but the presence of organic solvent may affect the subsequent application of graphene dispersion. Chinese invention patent (application number CN213913491U) discloses a double planetary stirring ultrasonic dispersion device for graphene slurry, which can effectively improve the stirring rate of the device and ensure stirring uniformity, but it will produce higher cost. Some existing carbon nano material dispersions on the market are all in liquid form, and their solvents are mostly toxic liquids, which are not conducive to transportation and preservation. In actual experiments and production, it is required that the dispersion process is simpler, and the solvent is more common and safe and environmentally friendly. Therefore, it is urgent to develop a carbon nano material dispersion method with good dispersibility and stability. Summary of the invention

[0013] The technical purpose of the present invention is mainly to address the current problems of poor dispersibility of carbon nanomaterials, difficulty in ensuring dispersion stability, and complex dispersion processes, and to develop a carbon nanomaterial dispersion method with good dispersibility and stability, no dispersant addition, and no structural damage. When used in accordance with the instructions while being easy to transport, a carbon nanomaterial composite powder with high dispersion stability can be achieved. The powder can achieve high dispersion stability again in different solvents and is suitable for various occasions where the excellent mechanical, thermal, and electrical properties of carbon nanomaterials need to be utilized, and can achieve high dispersion composites with other materials, thereby maximizing the performance advantages of carbon nanomaterials.

[0014] A carbon nanomaterial composite with high dispersion stability and a preparation method thereof are achieved by the following technical scheme. The steps are:

[0015] 1) Remove impurities; 2) Disperse; 3) Dry; 4) Use.

[0016] The details are as follows:

[0017] 1) impurity removal: the carbon nanomaterials graphene, carbon nanotubes, and conductive carbon black are respectively washed with deionized water by centrifugation until neutral, centrifuged, and dried in a vacuum oven, and the obtained carbon nanomaterial powders are respectively placed in an inert atmosphere for annealing treatment;

[0018] 2) Dispersion: placing carbon nanomaterials graphene, carbon nanotubes, and conductive carbon black in a certain solvent for a first-stage ultrasonic dispersion, and intermittently performing mechanical stirring to obtain graphene, carbon nanotubes, and conductive carbon black dispersions; subsequently, mixing the graphene dispersion, carbon nanotube dispersion, and conductive carbon black dispersion according to a mass ratio of graphene / carbon nanotubes / conductive carbon black of (1-15):1:(0-5), and then performing a second-stage ultrasonic dispersion treatment, and intermittently performing mechanical stirring;

[0019] 3) Drying: Drying: The obtained dispersion is placed in a water bath at a certain temperature and heated, accompanied by magnetic stirring until it becomes a paste, and then placed in a vacuum oven for drying, the obtained composite is ground into powder, and vacuum-sealed for storage;

[0020] 4) Use: The complex is ultrasonically dispersed in a target solvent (deionized water, one or more organic solvents such as alcohols, ketones, esters, amines, etc., or containing solutes) at a certain concentration to obtain a carbon nanomaterial system with high dispersion stability.

[0021] The graphene in step (1) has a size of 6-100 μm, a number of layers <10, a thickness of 1-3 nm, and a purity >95%; the carbon nanotubes are single-walled, double-walled or multi-walled carbon nanotubes without functional groups, with a length of 0.5-10 μm, a diameter of 4-100 nm, and a purity >95%; and the conductive carbon black particle size is 30-40 nm;

[0022] In the further impurity removal process in step 1), the centrifugal speed is 4000-8000 r min -1 ; The oven drying temperature is 60-100°C; during the impurity removal process, the annealing atmosphere is N2 or Ar, the annealing temperature is 300-600°C, and the annealing time is 2-4h.

[0023] Furthermore, in the ultrasonic dispersion process of step (2), the solvent used is deionized water or ethanol, the concentration of the carbon nanomaterial in the solvent is 1g / (2000-10000)ml, the ultrasonic power of the ultrasonic dispersion treatment is 200-600W, and the solution temperature is controlled at 20-30°C; the ultrasonic time of the first stage is 5-15min, and the time interval of intermittent mechanical stirring is 2-5min; the ultrasonic time of the second stage is 35-100min, and the time interval of intermittent mechanical stirring is 5-10min.

[0024] Step 2) The graphene size S and the carbon nanotube diameter OD should be maintained at S / OD=1±0.6, and when S≤50μm, the mass ratio of graphene / carbon nanotube / conductive carbon black is (9-15):1:(0-3); when S>50μm, the mass ratio of graphene / carbon nanotube / conductive carbon black is (1-9):1:(3-5).

[0025] In a further step 3), during the drying process, the temperature t of the water bath is 60-100°C, and the magnetic stirring speed v ranges from 500-2500 r / min. During this period, the water bath temperature is set according to the degree of evaporation of the solution, and the magnetic stirring speed satisfies the following relationship v=-50t+5000;

[0026] Step 3) During the drying process, the initial temperature of the vacuum oven is consistent with the final temperature of the water bath until the solution is dried. The oven temperature is reduced by 5-10°C for every 1h of extension of the drying process;

[0027] Step 4) During use, the target solvent can be selected according to the actual application situation. The concentration of the carbon nanomaterial composite in the target solvent is 1g / (1000-5000)ml, the ultrasonic power of the carbon nanomaterial composite is 200-600W, the ultrasonic time is 10-30min, and the ultraviolet absorbance of the obtained dispersion liquid after standing for 30 days is reduced by no more than 20% compared with the ultraviolet absorbance of the dispersion liquid before standing;

[0028] The carbon nanomaterial composite with high dispersion stability provided by the present invention has significant advantages:

[0029] The present invention utilizes the advantageous characteristics of three carbon nanomaterials, graphene / carbon nanotubes / conductive carbon black, in different dimensions to build a stable low-dimensional multi-scale three-dimensional structure. The carbon nanomaterials are dispersed with each other without adding any dispersant, and the operating conditions are mild, thereby ensuring the structural integrity of the carbon nanomaterials. The obtained carbon nanomaterial composite is a powder material, which is easy to transport and can be used in various occasions that require the excellent performance of carbon nanomaterials. Under the premise of ensuring its dispersion stability, the advantageous performance of carbon nanomaterials is fully utilized, thereby further expanding the application field of carbon nanomaterials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 (a) is a macroscopic photograph of the graphene / carbon nanotube / conductive carbon black dispersion prepared in Example 4 left to stand at room temperature for 30 days. Figure 1 (b) is a macroscopic photograph of the graphene / carbon nanotube / conductive carbon black dispersion prepared in Example 4, which was centrifuged for 30 minutes after standing at room temperature for 30 days.

[0031] Figure 2 (a) is a transmission electron microscope image of the graphene dispersion in Example 4 after being left to stand for 30 days and a macroscopic photograph of the dispersion. Figure 2 (b) is a transmission electron microscope image of the carbon nanotube dispersion in Example 4 after it was left to stand for 30 days and a macroscopic photograph of the dispersion. Figure 2 (c) is a transmission electron microscope image of the carbon black dispersion in Example 4 after standing for 30 days and a macroscopic photograph of the dispersion. Figure 2(d) is a transmission electron microscope image of the graphene / carbon nanotube / conductive carbon black dispersion in Example 4 after being left to stand for 30 days and a macroscopic photograph of the dispersion.

[0032] Figure 3 It is the ultraviolet spectra of the graphene / carbon nanotube / conductive carbon black dispersion in Example 4 after standing for 0 days and 30 days. DETAILED DESCRIPTION

[0033] The present invention will be further described below in conjunction with embodiments, but the present invention is not limited to the following embodiments.

[0034] Embodiment 1:

[0035] 1) Impurity removal: The carbon nanomaterials (graphene, carbon nanotubes, conductive carbon black, wherein the graphene size is 6 μm, the number of layers is less than 10, the thickness is 1-3 nm, and the purity is >95%; the carbon nanotubes are single-walled, double-walled or multi-walled carbon nanotubes without functional groups, the length is 0.5 μm, the diameter is 4 nm, and the purity is >95%; the conductive carbon black particle size is 30-40 nm) are respectively washed by centrifugation with deionized water until neutral, and the centrifugal speed is 4000 r min -1 , and dried in a vacuum oven (temperature of 60°C), and the obtained carbon nanomaterial powders were placed in a N2 inert atmosphere and annealed at 300°C for 4h;

[0036] 2) Dispersion: The carbon nanomaterials were placed in deionized water at a concentration of 1 g / 2000 ml, and the first stage of ultrasonic dispersion treatment was carried out at a power of 600 W and a solution temperature of 20° C., and mechanical stirring was performed intermittently. The ultrasonic time was 5 min, and the time interval of the intermittent mechanical stirring was 2 min. Subsequently, the carbon nanomaterials were mixed with a dispersion liquid according to a mass ratio of graphene / carbon nanotubes / conductive carbon black of 15:1:1, and then the second stage of ultrasonic dispersion treatment was carried out, and mechanical stirring was performed intermittently. The ultrasonic time was 100 min, and the time interval of the intermittent mechanical stirring was 5 min.

[0037] 3) Drying: The obtained dispersion is heated in a water bath at 60°C and stirred with a magnetic force at 2000 r / min until it becomes a paste, and then dried in a vacuum oven, the initial temperature of which is consistent with the final temperature of the water bath, until the solution is dried, and the oven temperature is reduced by 5°C for every 1 h of the drying process, and then the obtained composite is ground into powder and stored in a vacuum seal;

[0038] 4) Use: The complex was mixed in deionized water at a concentration of 1 g / 1000 ml and ultrasonically dispersed (ultrasonic power of 600 W, ultrasonic time of 30 min) to obtain a dispersion, the ultraviolet absorbance of which was 2.598 on day 0. After the dispersion was allowed to stand for 30 days, the ultraviolet absorbance was 2.133, which was 17.9% lower than that of the dispersion before standing.

[0039] Embodiment 2:

[0040] 1) Impurity removal: The carbon nanomaterials (graphene, carbon nanotubes, conductive carbon black, wherein the graphene size is 30 μm, the number of layers is less than 10, the thickness is 1-3 nm, and the purity is >95%; the carbon nanotubes are single-walled, double-walled or multi-walled carbon nanotubes without functional groups, the length is 0.5 μm, the diameter is 40 nm, and the purity is >95%; the conductive carbon black particle size is 30-40 nm) are respectively washed by centrifugation with deionized water until neutral, and the centrifugal speed is 5000 r min -1 , and dried in a vacuum oven (temperature of 70°C), and the obtained carbon nanomaterial powders were placed in a N2 inert atmosphere and annealed at 400°C for 4h;

[0041] 2) Dispersion: The carbon nanomaterials were placed in deionized water at a concentration of 1 g / 4000 ml, and the first stage of ultrasonic dispersion treatment was carried out at a power of 500 W and a solution temperature of 25°C, and mechanical stirring was performed intermittently. The ultrasonic time was 8 minutes, and the time interval of the intermittent mechanical stirring was 2 minutes. Subsequently, the carbon nanomaterials were mixed with a dispersion liquid according to a mass ratio of graphene / carbon nanotubes / conductive carbon black of 11:1:2, and then the second stage of ultrasonic dispersion treatment was carried out, and mechanical stirring was performed intermittently. The ultrasonic time was 80 minutes, and the time interval of the intermittent mechanical stirring was 6 minutes;

[0042] 3) Drying: The obtained dispersion is heated in a water bath at 60°C and stirred with a magnetic force at 2000 r / min until it becomes a paste, and then dried in a vacuum oven, the initial temperature of which is consistent with the final temperature of the water bath, until the solution is dried, and the oven temperature is reduced by 6°C for every 1 h of the drying process, and then the obtained composite is ground into powder and stored in a vacuum seal;

[0043] 4) Use: The complex was mixed in isopropanol at a concentration of 1 g / 2000 ml and ultrasonically dispersed (ultrasonic power of 500 W, ultrasonic time of 25 min) to obtain a dispersion, whose ultraviolet absorbance on day 0 was 2.673. After the obtained dispersion was allowed to stand for 30 days, its ultraviolet absorbance was 2.213, which was 17.2% lower than the ultraviolet absorbance of the dispersion before standing.

[0044] Embodiment 3:

[0045] 1) Impurity removal: The carbon nanomaterials (graphene, carbon nanotubes, conductive carbon black, wherein the graphene size is 50 μm, the number of layers is less than 10, the thickness is 1-3 nm, and the purity is >95%; the carbon nanotubes are single-walled, double-walled or multi-walled carbon nanotubes without functional groups, the length is 0.5 μm, the diameter is 50 nm, and the purity is >95%; the conductive carbon black particle size is 30-40 nm) are respectively washed by centrifugation with anhydrous ethanol until neutral, and the centrifugal speed is 6000 r min-1 , and dried in a vacuum oven (temperature of 80°C), and the obtained carbon nanomaterial powders were placed in an Ar inert atmosphere and annealed at 450°C for 3h;

[0046] 2) Dispersion: The carbon nanomaterials were placed in deionized water at a concentration of 1 g / 6000 ml, and the first stage of ultrasonic dispersion treatment was carried out at a power of 400 W and a solution temperature of 25° C., and mechanical stirring was performed intermittently. The ultrasonic time was 10 min, and the time interval of the intermittent mechanical stirring was 2 min. Subsequently, the carbon nanomaterials were mixed with a dispersion liquid according to a mass ratio of graphene / carbon nanotubes / conductive carbon black of 9:1:3, and then the second stage of ultrasonic dispersion treatment was carried out, and mechanical stirring was performed intermittently. The ultrasonic time was 60 min, and the time interval of the intermittent mechanical stirring was 7 min.

[0047] 3) Drying: The obtained dispersion is heated in a water bath at 70°C and stirred with a magnetic force at 1500 r / min until it becomes a paste, and then dried in a vacuum oven, the initial temperature of which is consistent with the final temperature of the water bath, until the solution is dried, and the oven temperature is reduced by 7°C for every 1 h of the drying process, and then the obtained composite is ground into powder and stored in a vacuum seal;

[0048] 4) Use: The complex was dissolved in an aqueous solution of sodium dodecylbenzene sulfate (concentration of 4×10 -3 mol / L) at a concentration of 1 g / 3000 ml and subjected to ultrasonic dispersion (ultrasonic power of 400 W, ultrasonic time of 20 min) to obtain a dispersion, the ultraviolet absorbance of which on day 0 was 2.696. After the dispersion was allowed to stand for 30 days, the ultraviolet absorbance of the dispersion was 2.270, which was 15.8% lower than that of the dispersion before the standing.

[0049] Embodiment 4:

[0050] 1) Impurity removal: The carbon nanomaterials (graphene, carbon nanotubes, conductive carbon black, wherein the graphene size is 80 μm, the number of layers is less than 10, the thickness is 1-3 nm, and the purity is >95%; the carbon nanotubes are single-walled, double-walled or multi-walled carbon nanotubes without functional groups, the length is 0.5 μm, the diameter is 60 nm, and the purity is >95%; the conductive carbon black particle size is 30-40 nm) are respectively washed by centrifugation with anhydrous ethanol until neutral, and the centrifugal speed is 7000 r min -1 , and dried in a vacuum oven (temperature of 90°C), and the obtained carbon nanomaterial powders were placed in an Ar inert atmosphere and annealed at 500°C for 2h;

[0051] 2) Dispersion: The carbon nanomaterials were placed in deionized water at a concentration of 1 g / 8000 ml, and the first stage of ultrasonic dispersion treatment was carried out at a power of 300 W and a solution temperature of 25°C, and mechanical stirring was performed intermittently. The ultrasonic time was 12 min, and the time interval of the intermittent mechanical stirring was 2 min. Subsequently, the carbon nanomaterials were mixed with a dispersion liquid according to a mass ratio of graphene / carbon nanotubes / conductive carbon black of 3:1:4, and then the second stage of ultrasonic dispersion treatment was carried out, and mechanical stirring was performed intermittently. The ultrasonic time was 50 min, and the time interval of the intermittent mechanical stirring was 8 min.

[0052] 3) Drying: The obtained dispersion is heated in a water bath at 80°C and stirred with a magnetic force at 1000 r / min until it becomes a paste, and then dried in a vacuum oven, the initial temperature of which is consistent with the final temperature of the water bath, until the solution is dried, and the oven temperature is reduced by 8°C for every 1 h of the drying process, and then the obtained composite is ground into powder and stored in a vacuum seal;

[0053] 4) Use: The complex was mixed in anhydrous ethanol solvent at a concentration of 1 g / 4000 ml and ultrasonically dispersed (ultrasonic power of 300 W, ultrasonic time of 15 min) to obtain a dispersion, whose ultraviolet absorbance on day 0 was 2.967. After the obtained dispersion was allowed to stand for 30 days, its ultraviolet absorbance was 2.564, which was 13.6% lower than the ultraviolet absorbance of the dispersion before standing.

[0054] Embodiment 5:

[0055] 1) Impurity removal: The carbon nanomaterials (graphene, carbon nanotubes, conductive carbon black, wherein the graphene has a size of 100 μm, a layer number of <10 layers, a thickness of 1-3 nm, and a purity of >95%; the carbon nanotubes are single-walled, double-walled or multi-walled carbon nanotubes without functional groups, with a length of 0.5 μm, a diameter of 100 nm, and a purity of >95%; the conductive carbon black particle size is 30-40 nm) are respectively centrifuged and washed with anhydrous ethanol until neutral, and the centrifugal speed is 8000 r min -1 , and dried in a vacuum oven (temperature of 100°C), and the obtained carbon nanomaterial powders were placed in an Ar inert atmosphere and annealed at 600°C for 2h;

[0056] 2) Dispersion: The carbon nanomaterials were placed in deionized water at a concentration of 1 g / 10000 ml, and the first stage of ultrasonic dispersion treatment was carried out at a power of 200 W and a solution temperature of 20° C., and mechanical stirring was performed intermittently. The ultrasonic time was 15 min, and the time interval of the intermittent mechanical stirring was 2 min. Subsequently, the carbon nanomaterials were dispersed in a dispersion solution with a mass ratio of graphene / carbon nanotubes / conductive carbon black of 2:1:3, and then the second stage of ultrasonic dispersion treatment was carried out, and mechanical stirring was performed intermittently. The ultrasonic time was 35 min, and the time interval of the intermittent mechanical stirring was 10 min.

[0057] 3) Drying: The obtained dispersion is heated in a water bath at 90°C and stirred with a magnetic force at 500 r / min until it becomes a paste, and then dried in a vacuum oven, the initial temperature of which is consistent with the final temperature of the water bath, until the solution is dried, and the oven temperature is reduced by 10°C for every 1h of the drying process, and then the obtained composite is ground into powder and stored in a vacuum seal;

[0058] 4) Use: The complex was mixed with a melamine aqueous solution (concentration of 0.2 g / 5000 ml) at a concentration of 1 g / 5000 ml and subjected to ultrasonic dispersion (ultrasonic power of 200 W, ultrasonic time of 10 min) to obtain a dispersion, the ultraviolet absorbance of which was 3.136 on day 0. After the dispersion was allowed to stand for 30 days, the ultraviolet absorbance was 2.521, which was 19.6% lower than the ultraviolet absorbance of the dispersion before standing.

Claims

1. A method for preparing a carbon nanomaterial composite having high dispersion stability, characterized in that: The following steps are involved: 1) impurity removal: the carbon nanomaterials graphene, carbon nanotubes, and conductive carbon black are centrifugally washed with deionized water until neutral, centrifuged, and dried in a vacuum oven. The obtained carbon nanomaterial powders are placed in an inert atmosphere for annealing treatment; 2) Dispersion: placing carbon nanomaterials graphene, carbon nanotubes, and conductive carbon black in a certain solvent for a first-stage ultrasonic dispersion, and intermittently performing mechanical stirring to obtain graphene, carbon nanotubes, and conductive carbon black dispersions; subsequently, mixing the graphene dispersion, carbon nanotube dispersion, and conductive carbon black dispersion according to a mass ratio of graphene / carbon nanotubes / conductive carbon black of (1-15):1:(0-5), and then performing a second-stage ultrasonic dispersion treatment, and intermittently performing mechanical stirring; 3) Drying: Drying: The obtained dispersion is placed in a water bath at a certain temperature and heated, accompanied by magnetic stirring until it becomes a paste, and then placed in a vacuum oven for drying, the obtained composite is ground into powder, and vacuum-sealed for storage; 4) Use: The composite is ultrasonically dispersed in a target solvent at a certain concentration to obtain a carbon nanomaterial system with high dispersion stability.

2. The method according to claim 1, characterized in that Step 1) The graphene has a size of 6-100 μm, a layer number of <10 layers, a thickness of 1-3 nm, and a purity of >95%; the carbon nanotubes are single-walled, double-walled or multi-walled carbon nanotubes without functional groups, a length of 0.5-10 μm, a diameter of 4-100 nm, and a purity of >95%; and the conductive carbon black has a particle size of 30-40 nm.

3. The method according to claim 1, characterized in that Step 1) During the impurity removal process, the centrifugal speed is 4000-8000 r min -1 , the drying temperature is 60-100℃.

4. The method according to claim 1, characterized in that Step 1) During the impurity removal process, the annealing atmosphere is N2 or Ar, the annealing temperature is 300-600°C, and the annealing time is 2-4h.

5. The method according to claim 1, characterized in that Step 2) During the dispersion process, the solvent used is deionized water or ethanol, the concentration of the carbon nanomaterial in the solvent is 1g / (2000-10000)ml, the ultrasonic power of the ultrasonic dispersion treatment is 200-600W, the solution temperature is controlled at 20-30°C, the ultrasonic time of the first stage is 5-15min, the time interval of intermittent mechanical stirring is 2-5min, the ultrasonic time of the second stage is 35-100min, and the time interval of intermittent mechanical stirring is 5-10min.

6. The method according to claim 1, characterized in that Step 2) During the dispersion process, the mass ratio of graphene / carbon nanotubes / conductive carbon black satisfies (1-15):1:(0-5), and the graphene size (S) and the carbon nanotube diameter (OD) should be maintained at S / OD=1±0.6, and when S≤50μm, the mass ratio of graphene / carbon nanotubes / conductive carbon black must satisfy (9-15):1:(0-3); when S>50μm, the mass ratio of graphene / carbon nanotubes / conductive carbon black must satisfy (1-9):1:(3-5).

7. The method according to claim 1, characterized in that Step 3) During the drying process, the temperature of the water bath (t) is 60-100°C, and the magnetic stirring speed (v) ranges from 2500-500r / min. During this period, the water bath temperature is set according to the degree of solution evaporation, and its relationship with the magnetic stirring speed is v=-50t+5000.

8. The method according to claim 1, characterized in that Step 3) During the drying process, the initial temperature of the vacuum oven is consistent with the final temperature of the water bath until the solution is dried. The oven temperature is reduced by 5-10°C for every 1h of drying process.

9. The method according to claim 1, characterized in that Step 4) During use, the solvent is selected from deionized water, one or more of alcohols, ketones, esters, amines, or contains a solute; the concentration of the carbon nanomaterial composite in the solvent is 1g / (1000-5000)ml, the ultrasonic power of the carbon nanomaterial composite is 200-600W, the ultrasonic time is 10-30min, and the obtained dispersion is allowed to stand for 30 days, and its ultraviolet absorbance is reduced by no more than 20% compared with the ultraviolet absorbance of the dispersion before standing.

10. A carbon nanomaterial composite with high dispersion stability prepared according to the method of any one of claims 1 to 9.

Citation Information

Patent Citations

  • Physical dispersion method of carbon nanotubes

    CN105771762A

  • Activated carbon / carbon nanotube / graphene composite material and preparation method and application thereof

    CN107331523A

  • Conductive paste prepared by compounding carbon nanotubes, graphene and conductive carbon black, and preparation method thereof

    CN108183223A

  • Graphene / nano carbon black / carbon nanotube composite conductive powder and preparation method thereof

    CN113793717A

  • Preparation method of high-performance composite conductive paste for lithium battery

    CN114725309A

Cited By

  • Self-collision dispersion process without destroying morphology of nano cerium oxide

    CN120664579A