Method for decomposing tungsten-nickel-containing diamond wire

Through mixed acid decomposition and alkali treatment with a mixed solution of phosphoric acid, nitric acid and citric acid, the problem of complexity and pollution in the treatment of tungsten-containing nickel diamond wire in the existing technology has been successfully solved, and the efficient separation and recovery of tungsten and nickel have been achieved, which is suitable for industrial production. .

CN118744987AActive Publication Date: 2024-10-08GUANGDONG XIANGLU TUNGSTEN +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410868534.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-08
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

When the existing technology processes tungsten-nickel diamond wire, the processing process is complicated, dangerous, and cannot effectively separate tungsten and nickel elements, resulting in resource waste and environmental pollution.

Method used

A mixed solution of phosphoric acid, nitric acid and citric acid is used for mixed acid decomposition, and nickel hydroxide and tungstate are separated through alkali treatment to achieve effective separation and recovery of tungsten and nickel.

Benefits of technology

It achieves process simplification, low consumption, and efficient product utilization, reducing environmental protection and cost pressures. It can quickly decompose tungsten-containing nickel diamond wire under normal pressure, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for decomposing a tungsten-nickel-containing diamond wire, which comprises the following steps: performing mixed acid decomposition on the tungsten-nickel-containing diamond wire by using a phosphoric acid, nitric acid and citric acid mixed solution to obtain diamond precipitate and a first dissolving solution, treating the first dissolving solution by using an alkaline solution, and filtering to obtain nickel hydroxide precipitate and a tungsten salt solution. The concentration of the phosphoric acid is 0.15-0.4 mol / L, the concentration of the nitric acid is 0.1-0.6 mol / L, and the concentration of the citric acid is 0.05-0.1 mol / L. The method provided by the invention is simple in process, short in consumed time, low in cost and high in product utilization rate, the diamond precipitate, the nickel hydroxide precipitate and the tungsten salt solution obtained after separation can be put into industrial production for recycling, the dosage of the mixed acid solution is small, the environmental protection pressure is small, and market popularization and application are extremely easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of decomposition and utilization of tungsten-nickel-containing diamond wires, and more particularly to a method for decomposing tungsten-nickel-containing diamond wires. Background Art

[0002] Diamond wire is a product that consolidates diamond micropowder particles on high-strength steel wire. It is mainly used for cutting hard and brittle materials, such as photovoltaic silicon wafers, sapphire, etc. Diamond wire is mainly used for photovoltaic silicon wafer cutting and is an upstream product in the photovoltaic industry. Under the background of "dual carbon", the photovoltaic industry has become a key development industry in the country. With the rapid growth of photovoltaic installed capacity, the demand for diamond wire has continued to increase. Diamond wire is a diamond cutting wire or diamond wire with doped tungsten wire as the mother wire / substrate. It consists of doped tungsten wire, pre-nickel plating layer, sand nickel layer and solid sand nickel layer. The diamond wire industry is facing challenges and opportunities of technological updates and iterations such as high efficiency and low cost. Tungsten wire has the characteristics of high tensile strength, good toughness, high breaking force, fatigue resistance and corrosion resistance. Decomposing tungsten-nickel diamond wire can promote the reuse of tungsten and nickel resources. A Chinese patent with application number 202211128838.X discloses a method for recovering tungsten-containing materials by decomposing them using a phosphorus-nitric acid mixed acid. Although the decomposition is done using a phosphorus-nitric acid mixed acid, the processing process of this method is too complicated and dangerous and needs to be completed under high temperature and high pressure. Moreover, the application cannot completely dissolve the tungsten-nickel components in the diamond wire.

[0003] The main treatment methods for traditional nickel-containing sludge are landfill and resource utilization. Landfill requires excavation of underground soil and construction of large anti-corrosion and anti-seepage pools, which occupies a large area, has a high risk of leakage, and wastes resources. The main treatment methods for resource utilization are pyrometallurgy, smelting process, wet extraction process, and pyrometallurgy-wet extraction process. Chinese patent application number 202211558488.0 discloses a method for treating nickel-containing sludge in diamond wire and its application, including electrolytic recovery of nickel after dissolution with sulfuric acid. The patent requires a large amount of sulfuric acid for the treatment of diamond wire. 1kg of nickel-containing sludge in diamond wire requires 4 to 6L of sulfuric acid solution. These acidic wastewaters are prone to waste resources and environmental pollution, and cannot achieve the purpose of separating and utilizing tungsten and nickel elements in diamond wire. Summary of the invention

[0004] In view of the above technical problems, the present invention provides a method for decomposing tungsten-nickel diamond wire, which has the advantages of short process flow, short time, small amount of acid used, high product utilization rate, etc.

[0005] In order to achieve the above objectives, this application adopts the following technical solutions:

[0006] A method for decomposing a tungsten-nickel diamond wire comprises: using a mixed solution of phosphoric acid, nitric acid and citric acid to perform mixed acid decomposition on the tungsten-nickel diamond wire to obtain a diamond solid and a first dissolving solution, wherein the first solution comprises a nickel salt and phosphotungstic acid, an alkaline solution is added to the first dissolving solution for alkaline treatment to obtain a nickel hydroxide precipitate and a second dissolving solution, and the second solution is filtered to obtain a tungstate solution.

[0007] The principle of the mixed acid decomposition chemical reaction is that tungsten reacts with acid to generate a soluble heteropoly acid, namely phosphotungstic acid. After the nickel in the diamond wire reacts with the acid, a salt soluble in water is generated. The ion reaction is: W+HNO 3 +H 3 PO 4 →H 3 PW 12 O 40 , Ni+2H + →Ni 2+ Citric acid can assist nitrophosphoric acid in complexing tungsten, making the complexation more complete and ensuring that the tungsten ions generated in the acid solution for a short time do not turn into tungstic acid;

[0008] Alkali treatment is the reaction of nickel salt with alkaline solution to form nickel hydroxide precipitate. The reaction of phosphotungstic acid with sodium hydroxide will produce products such as sodium tungstate which is easily soluble in water. The ion reaction is Ni 2+ +2OH - =Ni(OH) 2 ↓, H 3 PW 12 O 40 +27OH - =PO 4 3- +12WO 4 2- +15H 2 O.

[0009] Furthermore, the concentration of the phosphoric acid solution is 0.15-0.4 mol / L, the concentration of the nitric acid solution is 0.1-0.6 mol / L, and the concentration of the citric acid solution is 0.05-0.1 mol / L.

[0010] Furthermore, the concentration of the phosphoric acid solution is 0.162 mol / L, the concentration of the nitric acid solution is 0.440 mol / L, and the concentration of the citric acid solution is 0.076 mol / L.

[0011] Furthermore, the concentration of nitric acid is 0.377 mol / L, the concentration of phosphoric acid is 0.139 mol / L, and the concentration of citric acid is 0.076 mol / L.

[0012] Furthermore, the temperature of the mixed acid decomposition is maintained at 80-95° C., and the decomposition reaction time is 1-2 hours.

[0013] Furthermore, the alkaline solution is a sodium hydroxide solution.

[0014] The reaction between phosphotungstic acid and sodium hydroxide will generate products such as sodium tungstate that are easily soluble in water. Impurities such as nickel hydroxide precipitation can be removed by filtration. The chemical reaction formula is:

[0015] H 3 PW 12 O 40 +27NaOH=Na 3 PO 4 +12Na 2 WO 4 +15H 2 O

[0016] Furthermore, the reaction temperature of the alkali treatment is maintained at 80-95° C., the concentration is 1.73-2.5 mol / L, and the reaction time is 1-2 h.

[0017] Furthermore, the tungsten-nickel diamond wire is a tungsten-nickel diamond wire cut for photovoltaic use, with a diameter of 0.030-0.038 mm.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The mixed acid ratio used in the present invention can well decompose the tungsten-nickel components in the tungsten-nickel diamond wire into a solution, and the amount of mixed acid used to decompose the tungsten-nickel diamond wire is small. Chinese patent application number 202211558488.0 discloses a method for treating nickel-containing sludge in diamond wire and its application. 1kg of nickel-containing sludge in diamond wire requires 4 to 6L of sulfuric acid solution; Chinese patent application number 202211128838.X discloses a method for decomposing and recovering tungsten-containing materials using phosphorus-nitric acid mixed acid. The molar concentration of nitric acid used is generally 6 to 15 mol / L, and the molar concentration of phosphoric acid is 2 to 5.5 mol / L. In this application, the concentration of phosphoric acid solution is 0.15-0.4 mol / L, the concentration of nitric acid solution is 0.1-0.6 mol / L, and the concentration of citric acid solution is 0.05-0.1 mol / L. The amount of mixed acid used is small, and environmental protection pressure and cost pressure are also reduced.

[0020] (2) The method provided by the present invention has a simple process and a short time. It can be directly used for reaction under normal pressure without the need to purchase high-voltage equipment. It can quickly produce tungsten-nickel diamond wire with high strength and toughness, and is very easy to carry out industrial production and promotion.

[0021] The tungsten-nickel diamond wire includes tungsten, nickel and diamond particles. When the mixed acid decomposition is carried out, a mixed solution of phosphoric acid, nitric acid and citric acid is used for decomposition. In the mixed acid decomposition process, the diamond wire reacts chemically with phosphoric acid and nitric acid under the action of citric acid to form phosphotungstic acid, which can be dissolved in the first dissolving solution, so that tungsten exists in the form of a solution; at the same time, the nickel alloy exists in the mixed acid solution in the form of a soluble salt such as nickel nitrate or nickel phosphate; only diamond exists in the first dissolving solution in a solid form, and the diamond can be separated from the first dissolving solution by filtering and other operations.

[0022] Among them, citric acid can assist nitric acid and phosphoric acid in complexing tungsten, preventing tungsten from producing tungstic acid in the mixed acid solution. Tungstic acid is insoluble in acid solution and will be in the solution in the form of solid. It will be entrained in the diamond filtrate during subsequent filtration, making it difficult to distinguish later. After adding citric acid, the mixed acid can make the tungsten and nickel of the diamond wire exist in the form of solution, and the diamond exists in the solid form, which is helpful to separate the diamond from the tungsten-nickel diamond wire.

[0023] During the alkaline treatment process, nickel salts such as nickel nitrate and nickel phosphate can react with alkaline solutions to form nickel hydroxide precipitates, and the reaction of phosphotungstic acid and sodium hydroxide will produce products such as sodium tungstate that are easily soluble in water. Through filtration and other operations, the nickel hydroxide precipitate and tungsten salt can be separated into solid-liquid separation, thereby achieving the separation of tungsten and nickel in tungsten-nickel diamond wire.

[0024] (3) The present application can not only quickly separate diamond, nickel and tungsten from tungsten-nickel diamond wire, but also ensure that the products after separation can be recycled to generate higher economic value. The products finally separated by the present application include diamond, nickel hydroxide, nickel salt, tungsten salt, etc., which can be recycled again. Diamond can be directly recycled and continue to be used in different fields such as manufacturing abrasives, diamond processing, and electronic manufacturing. Nickel hydroxide is an inorganic compound with a very wide range of uses. It can be used as a catalyst for various chemical reactions, as a battery material, for the preparation of energy storage devices, for the preparation of high temperature, gas sensors, catalyst carriers, and also for applications in the fields of medicine, cosmetics, glass, etc. The sodium tungstate solution obtained by the present application can be directly evaporated and crystallized to obtain sodium tungstate products. The application range of sodium tungstate covers many aspects from the metallurgical industry to the medical field. It can be used to manufacture metal tungsten, tungstic acid, tungstates, as a coating preservative, for the preparation of some antioxidants, and for the preparation of some drugs that are beneficial to the nervous system. The ammonium tungstate solution can also be obtained by ion exchange process or extraction process. The ammonium tungstate solution can be evaporated and crystallized to obtain APT product (ammonium paratungstate). Ammonium paratungstate can be directly used as a raw material for producing metallic tungsten, and can be used as a precursor for synthesizing various tungsten compounds such as tungsten carbide, tungsten oxide and tungsten oxide. It is used to produce tungsten-based alloys and coatings in the aerospace industry and to produce tungsten-based catalysts in the chemical industry. For example, ammonium paratungstate can also be used to produce tungsten oxide products through an ammonia process. Tungsten oxide can be directly reduced to obtain tungsten powder, and tungsten powder can be carbonized to obtain tungsten carbide products, thereby realizing efficient and thorough recycling of tungsten. DETAILED DESCRIPTION

[0025] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Modifications or substitutions made to the methods, steps or conditions of the present invention without departing from the spirit and essence of the present invention are within the scope of protection of the present invention. Unless otherwise specified, the experimental materials, reagents, instruments, etc. used in the examples of the present invention are all commercially available; unless otherwise specified, all technical means in the examples of the present invention are conventional means well known to those skilled in the art.

[0026] The present application provides a method for decomposing a tungsten-nickel diamond wire, comprising:

[0027] S1: Using a mixed solution of phosphoric acid, nitric acid and citric acid to decompose the tungsten-nickel diamond wire, a diamond solid and a first solution are obtained, wherein the first solution includes a nickel salt and phosphotungstic acid. The diamond solid, the nickel salt and the tungsten salt are separated by filtering and other operations.

[0028] The tungsten-nickel diamond wire comprises diamond particles, a tungsten wire mother wire and a nickel-plated layer. The diameter of the tungsten-nickel diamond wire is 0.030-0.038 mm.

[0029] The concentration of the phosphoric acid solution is 0.15-0.4 mol / L, the concentration of the nitric acid solution is 0.1-0.6 mol / L, and the concentration of the citric acid solution is 0.05-0.1 mol / L.

[0030] Preferably, the concentration of the phosphoric acid solution is 0.162 mol / L, the concentration of the nitric acid solution is 0.440 mol / L, and the concentration of the citric acid solution is 0.076 mol / L.

[0031] Preferably, the nitric acid concentration is 0.377 mol / L, the phosphoric acid concentration is 0.139 mol / L, and the citric acid concentration is 0.076 mol / L.

[0032] The temperature of the mixed acid decomposition is maintained at 80-95° C., and the decomposition reaction time is 1-2 hours.

[0033] Specific process and chemical formula:

[0034] The principle of the mixed acid decomposition chemical reaction is that tungsten reacts with acid to generate a soluble heteropoly acid, namely phosphotungstic acid. After the nickel in the diamond wire reacts with the acid, it generates a salt that is soluble in water. The ion reaction is: W+HNO 3 +H 3 PO 4 →H 3 PW 12 O 40 , Ni+2H + →Ni 2+ Citric acid can assist nitrophosphoric acid in complexing tungsten, making the complexation more complete and ensuring that the tungsten ions generated in the acid solution for a short time do not turn into tungstic acid; tungstic acid is insoluble in acid solution and will be in the solution in the form of solid. It will be entrained in the diamond filtrate during subsequent filtration, making it difficult to distinguish later. After adding citric acid, the mixed acid can make the tungsten alloy and nickel alloy exist in the form of solution, and the diamond exists in the form of solid, which is helpful to separate the diamond from the tungsten-nickel diamond wire.

[0035] S2: adding an alkaline solution to the first dissolving solution for alkaline treatment to obtain a nickel hydroxide precipitate and a second dissolving solution, wherein the second dissolving solution is a tungsten salt solution.

[0036] The alkaline solution is a sodium hydroxide solution.

[0037] The reaction temperature of the alkali treatment is maintained at 80-95° C., the concentration of the alkaline solution is 1.73-2.5 mol / L, and the reaction time is 1-2 h.

[0038] Specific process and chemical formula:

[0039] Alkali treatment is the reaction of nickel salt with alkaline solution to form nickel hydroxide precipitate, and the reaction of phosphotungstic acid with sodium hydroxide will produce products such as sodium tungstate that is easily soluble in water. The ion reaction is: Ni2+ +2OH - =Ni(OH) 2 ↓, H 3 PW 12 O 40 +27OH - =PO 4 3- +12WO 4 2- +15H 2 O.

[0040] The reaction of phosphotungstic acid and sodium hydroxide will generate products such as sodium tungstate that are easily soluble in water. Impurities such as nickel hydroxide precipitation can be removed by filtration. The obtained sodium tungstate solution can be directly evaporated and crystallized to obtain sodium tungstate products, or ion exchange or extraction processes can be used to obtain ammonium tungstate solution. The ammonium tungstate solution is evaporated and crystallized to obtain APT products (ammonium paratungstate). The chemical reaction formula is: H 3 PW 12 O 40 +27NaOH=Na 3 PO 4 +12Na 2 WO 4 +15H 2 O.

[0041] The present application adopts sodium hydroxide as the alkaline treatment solution, so that tungsten exists in the form of sodium tungstate, and sodium tungstate can be easily converted into ammonium paratungstate, which is conducive to the efficient recycling of tungsten.

[0042] S3: Filter to obtain tungsten salt solution

[0043] The precipitate after alkali treatment is nickel hydroxide, which can be filtered to obtain a tungsten salt solution.

[0044] S4: Diamond, nickel hydroxide and tungsten salt are recycled.

[0045] The products obtained after each step of the reaction in this application can be recycled and reused, and the product utilization rate is high. Diamond can be directly recycled and continued to be used in different fields such as manufacturing abrasives, diamond processing, and electronic manufacturing. Nickel hydroxide is an inorganic compound with a very wide range of uses. It can be used as a catalyst for various chemical reactions, as a battery material, for the preparation of energy storage devices, for the preparation of high temperature, gas sensors, catalyst carriers, and applications in the fields of medicine, cosmetics, glass, etc. The sodium tungstate solution obtained in this application can be directly used for evaporation and crystallization to obtain sodium tungstate products. The application range of sodium tungstate covers many aspects from the metallurgical industry to the medical field. It can be used to manufacture metal tungsten, tungstic acid, tungstates, as a coating preservative, for the preparation of some antioxidants, and for the preparation of some drugs that are beneficial to the nervous system. The ammonium tungstate solution can also be obtained by ion exchange process or extraction process. The ammonium tungstate solution can be evaporated and crystallized to obtain APT product (ammonium paratungstate). Ammonium paratungstate can be used as a raw material for producing metallic tungsten, and can be used as a precursor for synthesizing various tungsten compounds such as tungsten carbide, tungsten oxide and tungsten oxide. It is used to produce tungsten-based alloys and coatings in the aerospace industry and to produce tungsten-based catalysts in the chemical industry. For example, ammonium paratungstate can also be used to produce tungsten oxide products through ammonia process. Tungsten oxide can be directly reduced to obtain tungsten powder, and tungsten powder can be carbonized to obtain tungsten carbide products, thereby realizing efficient and thorough recycling of tungsten.

[0046] The method provided in this application is simple in process, short in time, low in cost, and environmentally friendly. It can quickly produce tungsten-nickel diamond wire with high strength and toughness, and can achieve efficient recovery and reuse of the decomposition products of tungsten-nickel diamond (diamond, nickel hydroxide, and tungsten salt). It has good market promotion prospects and application value.

[0047] Example 1 Main components of tungsten-nickel diamond wire: W / %: 84.82%, Ni 13.72%

[0048] A method for decomposing a tungsten-nickel diamond wire, comprising:

[0049] S0: weigh 20g of tungsten-nickel diamond wire;

[0050] S1: Prepare a mixed acid with a nitric acid concentration of 0.377 mol / L, a phosphoric acid concentration of 0.139 mol / L, and a citric acid concentration of 0.076 mol / L, and heat it in a water bath to 90°C for 2 hours to decompose. After the reaction, there is no residual filament in the solution, and a green first dissolving solution and diamond solids are obtained. The diamond solids are removed by filtration, and the remaining first dissolving solution of nickel salt and tungsten salt is:

[0051] Tungsten reacts with acid to form soluble heteropolyacid, namely phosphotungstic acid. The nickel in the diamond wire reacts with the acid to form a salt soluble in water. The ion reaction is: W+HNO 3 +H 3 PO4 →H 3 PW 12 O 40 , Ni+2H + →Ni 2+ . Citric acid can assist nitrophosphoric acid in complexing tungsten, making the complexation more complete and ensuring that the tungsten ions generated in the acid solution in a short time do not turn into tungstic acid; tungstic acid is insoluble in acid solution and will be in the solution in the form of a solid. It will be entrained in the diamond filtrate during subsequent filtration, making it difficult to distinguish later. The mixed acid after adding citric acid can make the tungsten and nickel of the diamond wire exist in the form of a solution, and the diamond exists in a solid form, which is helpful to separate the diamond from the tungsten-nickel diamond wire.

[0052] S2: Add sodium hydroxide solution to the first solution for alkaline treatment to obtain nickel hydroxide precipitate and second solution; specifically, the first solution is added to 2.5 mol / L sodium hydroxide solution for reaction, and heated in a water bath at 90°C for 2 hours. After alkaline decomposition, a large amount of precipitate is generated in the green first solution, which is nickel hydroxide precipitate. After filtering, a slightly yellow clear second solution is obtained;

[0053] The reaction process is: nickel salt reacts with in alkaline solution to form nickel hydroxide precipitate, and phosphotungstic acid reacts with sodium hydroxide to produce products such as sodium tungstate that is easily soluble in water. The ion reaction is: Ni 2+ +2OH - =Ni(OH) 2 ↓, H 3 PW 12 O 40 +27OH - =PO 4 3- +12WO 4 2- +15H 2 O.

[0054] S3: The second solution is subjected to evaporation and crystallization to obtain a sodium tungstate product.

[0055] S4: The diamond obtained after filtering the first solution is used to manufacture abrasives, the nickel hydroxide obtained after filtering the second solution is used to manufacture nickel-hydrogen batteries and nickel-cadmium batteries; sodium tungstate is used to manufacture metallic tungsten and antioxidants.

[0056] Example 2 Main components of tungsten-nickel diamond wire: W / %: 92.56%, Ni 5.48%

[0057] S0: weigh 40 g of tungsten-nickel diamond wire;

[0058] S1: prepare a mixed acid with a nitric acid concentration of 0.440 mol / L, a phosphoric acid concentration of 0.162 mol / L, and a citric acid concentration of 0.076 mol / L, heat it in a water bath to 90°C for 2 hours, and decompose it. After the reaction, there is no residual filament in the solution, and a green first dissolving solution and diamond solids are obtained. The diamond solids are removed by filtering, and the remaining first dissolving solution is a mixture of nickel salt and tungsten salt;

[0059] S2: Add sodium hydroxide solution to the first solution for alkali treatment to obtain nickel hydroxide precipitate and the second solution; specifically, add the first solution to 2.5 mol / L sodium hydroxide solution for reaction, and heat in a water bath at 90°C for 2 hours. After alkalization and decomposition, a large amount of precipitate is generated in the green first solution, which is nickel hydroxide precipitate. After filtering, a slightly yellowish clear second solution is obtained.

[0060] S3: The second solution is subjected to an extraction process to obtain an ammonium tungstate solution, and the ammonium tungstate solution is evaporated and crystallized to obtain an APT product (ammonium paratungstate).

[0061] S4: The diamond obtained after filtering the first solution is used for masonry processing, and the nickel hydroxide obtained after filtering the second solution is used as a catalyst for chemical reactions; APT products (ammonium paratungstate) can be produced through an ammonia process to obtain tungsten oxide products, and tungsten oxide can be directly reduced to obtain tungsten powder, which can be carbonized to obtain tungsten carbide products, thereby achieving efficient recycling of tungsten.

[0062] Example 3 Main components of tungsten-nickel diamond wire: W / %: 92.76%, Ni 5.39%

[0063] S0: weigh 40 g of tungsten-nickel diamond wire;

[0064] S1: prepare a mixed acid with a nitric acid concentration of 0.377 mol / L, a phosphoric acid concentration of 0.139 mol / L, and a citric acid concentration of 0.076 mol / L, heat it in a water bath to 90°C for 2 hours, and decompose it. After the reaction, there is no residual filament in the solution, and a green first dissolving solution and diamond solids are obtained. The diamond solids are removed by filtering, and the remaining first dissolving solution is a mixture of nickel salt and tungsten salt;

[0065] S2: Add sodium hydroxide solution to the first solution for alkali treatment to obtain nickel hydroxide precipitate and the second solution; specifically, add the first solution to 2.5 mol / L sodium hydroxide solution for reaction, and heat in a water bath at 90°C for 2 hours. After alkalization and decomposition, a large amount of precipitate is generated in the green first solution, which is nickel hydroxide precipitate. After filtering, a slightly yellowish clear second solution is obtained.

[0066] S3: The second solution is subjected to an extraction process to obtain an ammonium tungstate solution, and the ammonium tungstate solution is evaporated and crystallized to obtain an APT product.

[0067] Example 4 Main components of tungsten-nickel diamond wire: W / %: 80.06%, Ni 16.80%

[0068] S0: weigh 30 g of tungsten-nickel diamond wire;

[0069] S1: prepare a mixed acid with a nitric acid concentration of 0.377 mol / L, a phosphoric acid concentration of 0.139 mol / L, and a citric acid concentration of 0.076 mol / L, heat it in a water bath to 90°C for 2 hours, and decompose it. After the reaction, there is no residual filament in the solution, and a green first dissolving solution and diamond solids are obtained. The diamond solids are removed by filtering, and the remaining first dissolving solution is a mixture of nickel salt and tungsten salt;

[0070] S2: Add sodium hydroxide solution to the first solution for alkali treatment to obtain nickel hydroxide precipitate and the second solution; specifically, add the first solution to 2.5 mol / L sodium hydroxide solution for reaction, and heat in a water bath at 90°C for 2 hours. After alkalization and decomposition, a large amount of precipitate is generated in the green first solution, which is nickel hydroxide precipitate. After filtering, a slightly yellowish clear second solution is obtained.

[0071] S3: The second solution is subjected to an ion exchange process to obtain an ammonium tungstate solution, and the ammonium tungstate solution is evaporated and crystallized to obtain an APT product.

[0072] Example 5 Main components of tungsten-nickel diamond wire: W / %: 84.82%, Ni 13.72%

[0073] S0: weigh 40 g of tungsten-nickel diamond wire;

[0074] S1: prepare a mixed acid with a nitric acid concentration of 0.60 mol / L, a phosphoric acid concentration of 0.15 mol / L, and a citric acid concentration of 0.1 mol / L, heat it in a water bath to 90°C for 2 hours, and decompose it. After the reaction, there is no residual filament in the solution, and a green first dissolving solution and diamond solids are obtained. The diamond solids are removed by filtering, and the remaining first dissolving solution is a mixture of nickel salt and tungsten salt;

[0075] S2: Adding sodium hydroxide solution to the first solution for alkali treatment to obtain nickel hydroxide precipitate and a second solution; specifically, adding the first solution to a 1.73 mol / L sodium hydroxide solution for reaction, heating in a water bath at 90°C for 2 hours. After alkalization and decomposition, a large amount of precipitate is generated in the green first solution, which is nickel hydroxide precipitate. After filtering, a slightly yellowish clear second solution is obtained.

[0076] S3: The second solution is subjected to an extraction process to obtain an ammonium tungstate solution, and the ammonium tungstate solution is evaporated and crystallized to obtain an APT product.

[0077] Example 6 Main components of tungsten-nickel diamond wire: W / %: 84.82%, Ni 13.72%

[0078] S0: weigh 40 g of tungsten-nickel diamond wire;

[0079] S1: prepare a mixed acid with a nitric acid concentration of 0.10 mol / L, a phosphoric acid concentration of 0.4 mol / L, and a citric acid concentration of 0.05 mol / L, heat it in a water bath to 90°C for 2 hours, and decompose it. After the reaction, there is no residual filament in the solution, and a green first dissolving solution and diamond solids are obtained. The diamond solids are removed by filtering, and the remaining first dissolving solution is a mixture of nickel salt and tungsten salt;

[0080] S2: Add sodium hydroxide solution to the first solution for alkali treatment to obtain nickel hydroxide precipitate and a second solution; specifically, add the first solution to a 2.0 mol / L sodium hydroxide solution for reaction, and heat in a water bath at 90°C for 2 hours. After alkalization and decomposition, a large amount of precipitate is generated in the green first solution, which is nickel hydroxide precipitate. After filtration, a slightly yellowish clear second solution is obtained.

[0081] S3: The second solution is subjected to an extraction process to obtain an ammonium tungstate solution, and the ammonium tungstate solution is evaporated and crystallized to obtain an APT product.

[0082] Comparative Example 1 The main components of the tungsten-nickel diamond wire are as follows: W / %: 84.82%, Ni 13.72%. The difference between this comparative example and Example 1 is that nitric acid is replaced with hydrochloric acid, and the other steps are the same as Example 1. As a result, the tungsten-nickel diamond wire is basically insoluble.

[0083] Comparative Example 2 The main components of the tungsten-nickel diamond wire are as follows: W / %: 84.82%, Ni 13.72%. The difference between this comparative example and Example 1 is that nitric acid is replaced with sulfuric acid, and the other steps are the same as Example 1. As a result, the tungsten-nickel diamond wire is basically insoluble.

[0084] Comparative Example 3 The main components of the tungsten-nickel diamond wire are as follows: W / %: 84.82%, Ni 13.72%. The difference between this comparative example and Example 1 is that no citric acid is added to the mixed acid, and the other steps are the same as Example 1. As a result, the tungsten-nickel diamond wire is not fully dissolved.

[0085] It can be seen from the comparative examples and embodiments that the beneficial effects of the present invention are:

[0086] (1) The mixed acid ratio used in the present invention can well decompose the tungsten-nickel components in the tungsten-nickel diamond wire into a solution, and the amount of mixed acid used to decompose the tungsten-nickel diamond wire is small. Chinese patent application number 202211558488.0 discloses a method for treating nickel-containing sludge in diamond wire and its application. 1kg of nickel-containing sludge in diamond wire requires 4 to 6L of sulfuric acid solution; Chinese patent application number 202211128838.X discloses a method for decomposing and recovering tungsten-containing materials using phosphorus-nitric acid mixed acid. The molar concentration of nitric acid used is generally 6 to 15 mol / L, and the molar concentration of phosphoric acid is 2 to 5.5 mol / L. In this application, the concentration of phosphoric acid solution is 0.15-0.4 mol / L, the concentration of nitric acid solution is 0.1-0.6 mol / L, and the concentration of citric acid solution is 0.05-0.1 mol / L. The amount of mixed acid used is small, and environmental protection pressure and cost pressure are also reduced.

[0087] (2) The method provided by the present invention has a simple process and a short time. It can be directly used for reaction under normal pressure without the need to purchase high-voltage equipment. It can quickly produce tungsten-nickel diamond wire with high strength and toughness, and is very easy to carry out industrial production and promotion.

[0088] The tungsten-nickel diamond wire includes tungsten, nickel and diamond particles. When the mixed acid decomposition is carried out, a mixed solution of phosphoric acid, nitric acid and citric acid is used for decomposition. In the mixed acid decomposition process, the diamond wire reacts chemically with phosphoric acid and nitric acid under the action of citric acid to form phosphotungstic acid, which can be dissolved in the first dissolving solution, so that tungsten exists in the form of a solution; at the same time, the nickel alloy exists in the mixed acid solution in the form of a soluble salt such as nickel nitrate or nickel phosphate; only diamond exists in the first dissolving solution in a solid form, and the diamond can be separated from the first dissolving solution by filtering and other operations.

[0089] Among them, citric acid can assist nitric acid and phosphoric acid in complexing tungsten, preventing tungsten from producing tungstic acid in the mixed acid solution. Tungstic acid is insoluble in acid solution and will be in the solution in the form of solid. It will be entrained in the diamond filtrate during subsequent filtration, making it difficult to distinguish later. After adding citric acid, the mixed acid can make the tungsten and nickel of the diamond wire exist in the form of solution, and the diamond exists in the solid form, which is helpful to separate the diamond from the tungsten-nickel diamond wire.

[0090] During the alkaline treatment process, nickel salts such as nickel nitrate and nickel phosphate can react with alkaline solutions to form nickel hydroxide precipitates, and the reaction of phosphotungstic acid and sodium hydroxide will produce products such as sodium tungstate that are easily soluble in water. Through filtration and other operations, the nickel hydroxide precipitate and tungsten salt can be separated into solid-liquid separation, thereby achieving the separation of tungsten and nickel in tungsten-nickel diamond wire.

[0091] (3) The present application can not only quickly separate diamond, nickel and tungsten from tungsten-nickel diamond wire, but also ensure that the products after separation can be recycled to generate higher economic value. The products finally separated by the present application include diamond, nickel hydroxide, nickel salt, tungsten salt, etc., which can be recycled again. Diamond can be directly recycled and continued to be used in different fields such as manufacturing abrasives, diamond processing, and electronic manufacturing. Nickel hydroxide is an inorganic compound with a very wide range of uses. It can be used as a catalyst for various chemical reactions, as a battery material, for the preparation of energy storage devices, for the preparation of gas sensors, catalyst carriers, and also in the fields of medicine, cosmetics, glass, etc. The sodium tungstate solution obtained by the present application can be directly evaporated and crystallized to obtain sodium tungstate products. The application range of sodium tungstate covers many aspects from the metallurgical industry to the medical field. It can be used to manufacture metal tungsten, tungstic acid, tungstates, as a coating preservative, for the preparation of some antioxidants, and for the preparation of some drugs that are beneficial to the nervous system. The ammonium tungstate solution can also be obtained by ion exchange process or extraction process. The ammonium tungstate solution can be evaporated and crystallized to obtain APT product (ammonium paratungstate). Ammonium paratungstate can be used as a raw material for producing metallic tungsten, and can be used as a precursor for synthesizing various tungsten compounds such as tungsten carbide, tungsten oxide and tungsten oxide. It is used to produce tungsten-based alloys and coatings in the aerospace industry and to produce tungsten-based catalysts in the chemical industry. For example, ammonium paratungstate can also be used to produce tungsten oxide products through ammonia process. Tungsten oxide can be directly reduced to obtain tungsten powder, and tungsten powder can be carbonized to obtain tungsten carbide products, thereby realizing efficient and thorough recycling of tungsten.

[0092] The above embodiments only express the preferred implementation modes of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the patent scope of the present invention. It should be pointed out that, for ordinary technicians in this field, the above technical features can be freely combined without departing from the concept of the present invention, and several deformations and improvements can be made, which all belong to the protection scope of the present invention. Therefore, all equivalent changes and modifications made to the scope of the claims of the present invention should belong to the coverage of the claims of the present invention.

Claims

1. A method for decomposing a tungsten-nickel diamond wire, characterized in that: include: Using a mixed solution of phosphoric acid, nitric acid and citric acid to decompose the tungsten-nickel diamond wire to obtain a diamond solid and a first dissolving solution, wherein the first solution includes a nickel salt and phosphotungstic acid; adding an alkaline solution to the first dissolving solution for alkaline treatment to obtain a nickel hydroxide precipitate and a second dissolving solution; The second dissolved liquid is filtered to obtain a tungsten salt solution.

2. The method for decomposing a tungsten-nickel diamond wire according to claim 1, characterized in that: The concentration of the phosphoric acid is 0.15-0.4 mol / L, the concentration of the nitric acid is 0.1-0.6 mol / L, and the concentration of the citric acid is 0.05-0.1 mol / L.

3. The method for decomposing a tungsten-nickel diamond wire according to claim 2, characterized in that: The concentration of the phosphoric acid is 0.162 mol / L, the concentration of the nitric acid is 0.440 mol / L, and the concentration of the citric acid is 0.076 mol / L.

4. The method for decomposing a tungsten-nickel diamond wire according to claim 2, characterized in that: The concentration of the nitric acid is 0.377 mol / L, the concentration of the phosphoric acid is 0.139 mol / L, and the concentration of the citric acid is 0.076 mol / L.

5. The method for decomposing a tungsten-nickel diamond wire according to claim 1, characterized in that: The temperature of the mixed acid decomposition is maintained at 80-95° C., and the decomposition reaction time is 1-2 hours.

6. The method for decomposing a tungsten-nickel diamond wire according to claim 1, characterized in that: The alkaline solution is a sodium hydroxide solution.

7. The method for decomposing a tungsten-nickel diamond wire according to claim 1, characterized in that: The reaction temperature of the alkali treatment is maintained at 80-95° C., the concentration of the alkaline solution is 1.73-2.5 mol / L, and the reaction time is 1-2 h.

8. The method according to any one of claims 1 to 7, characterized in that: The diameter of the tungsten-nickel diamond wire is 0.030-0.038 mm.

Citation Information

Patent Citations

  • Method for decomposing and recycling tungsten-containing waste by using phosphorus-nitrate mixed acid

    CN115305364A

  • Diamond wire nickel-containing sludge treatment method and application thereof

    CN116043031A

  • Method for recycling diamond wire sawing waste of sapphire

    CN106745134A