Dehydration method of bischofite
By using a rotary fluidized reactor and appropriate process parameters in the hydrochlorite dehydration process, the problems of material agglomeration and poor mass and heat transfer were solved, high-efficiency, low-energy consumption catalytic dehydration was achieved, and the magnesium chloride production rate was significantly improved. The purity and yield provide the basis for industrial-level production.
Patent Information
- Application Number
- CN202410863817.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-29
- Publication Date
- 2024-10-08
AI Technical Summary
In the existing hydrochlorite catalytic coupling dehydration reaction, materials are easy to agglomerate and have poor mass and heat transfer, resulting in problems such as high water content and low purity of magnesium chloride products.
A rotary fluidized reactor is used for catalytic dehydration. By adjusting the reactor speed, bed pressure and tilt angle, combined with the type of feed gas and gas flow rate, it is ensured that the solid material is in full contact with the feed gas to avoid agglomeration and is pre-prepared. Processing improves reaction efficiency.
It significantly reduces the water content and by-product content of magnesium chloride products, improves the purity of magnesium chloride, reduces energy consumption and equipment corrosion, and achieves a more efficient catalytic dehydration reaction, which is suitable for industrial-level production.
Smart Images

Figure CN118744995A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic salts, and in particular to a dehydration method of bischofite. Background Art
[0002] Magnesium metal is an important strategic resource with a wide range of applications. Using hydrochloric acid bischofite to dehydrate anhydrous magnesium chloride and then electrolyze it to generate magnesium metal is considered to be the most ideal reaction route for producing magnesium resources. However, the traditional dehydration process faces problems such as high energy consumption, easy hydrolysis, and equipment corrosion. Therefore, how to improve the quality and reduce consumption of the dehydration process and reduce equipment corrosion has attracted widespread attention. The OH bond of the crystal water in magnesium chloride hydrate has the possibility of being activated and thus participating in chemical reactions. How to utilize this chemical reaction activity is of great significance to the creation of new dehydration processes.
[0003] The prior art discloses a new catalytic coupling dehydration method for preparing low-water magnesium chloride by reacting low-carbon small molecules with magnesium chloride for dehydration. The method uses the characteristic that the crystal water coordinated and bonded by metal cations is more easily activated, and the coupling of low-carbon small molecules further promotes the reaction to occur in the forward direction, thereby reducing the dehydration temperature and avoiding the corrosion of HCl gas to the equipment. However, the dehydration method adopts a fixed bed process, which has poor mass and heat transfer effects, has strict requirements on the particle size of raw materials, is prone to incomplete reaction and easy accumulation and agglomeration of materials, has limitations in scale-up production, and from the perspective of the economic efficiency of the process, the method is further unable to achieve material recycling. Summary of the invention
[0004] The main purpose of the present invention is to provide a dehydration method of bischofite, so as to solve the problem in the prior art that the materials in the bischofite catalytic coupled dehydration reaction are easy to agglomerate and the mass and heat transfer are poor, resulting in a magnesium chloride product with high water content and low purity.
[0005] In order to achieve the above object, according to one aspect of the present invention, a dehydration method of bischofite is provided, comprising the following steps: step S1, feeding bischofite into a rotating fluidized reactor; step S2, evacuating the rotating fluidized reactor and then introducing raw gas to carry out catalytic dehydration reaction to obtain reaction products and tail gas; step S3, cooling the reaction product to obtain low-water magnesium chloride, wherein the average molar number of crystal water contained in each low-water magnesium chloride molecule is ≤2; wherein the raw gas comprises carbon monoxide and / or methane; the rotation speed of the rotating fluidized reactor is 1-200 r / min, the bed pressure is 0.1-1 MPa, the bed is inclined upward from the material inlet to the material outlet, and the inclination angle is 0-60°; the reaction temperature of the catalytic dehydration reaction is 50-300°C.
[0006] Furthermore, in step S2, the gas flow rate of the raw gas is 0.1 to 20 L / min, preferably 1 to 10 L / min.
[0007] Furthermore, in step S2, auxiliary gas is introduced at the same time as the raw gas, and the auxiliary gas includes one or more of hydrogen, nitrogen and carbon dioxide; preferably, the volume ratio of the raw gas to the auxiliary gas is (0.1-19):1.
[0008] Furthermore, in step S2, the vacuum degree of the rotating fluidized state reactor is -0.1 to 0 MPa; and / or the rotation speed of the rotating fluidized state reactor is 2 to 100 r / min; and / or the bed pressure of the rotating fluidized state reactor is 0.1 to 0.5 MPa; and / or the bed of the rotating fluidized state reactor is inclined upward from the material inlet to the material outlet, and the inclination angle is 0 to 45°.
[0009] Furthermore, in step S2, the reaction temperature of the catalytic dehydration reaction is 80-300°C, the reaction time is 3-30h, and the heating rate is 1-50°C / min.
[0010] Furthermore, in step S1, the amount of bischofite charged into the rotating fluidized bed reactor is 0.1 to 2000 g, preferably 1 to 1000 g.
[0011] Further, step S1 also includes the step of subjecting the bischofite to a first pretreatment, the first pretreatment including: subjecting the bischofite to a first drying, grinding, particle size screening and a second drying in sequence to obtain a pretreated bischofite, wherein the average molar number of crystalline water contained in each pretreated bischofite molecule is 3 to 5; preferably, the first drying temperature is 50 to 120° C., and the time is 1 to 8 hours; and / or the screening mesh number of the particle size screening is 20 to 500 mesh; and / or the second drying temperature is 50 to 120° C., and the time is 1 to 8 hours; more preferably, the first drying temperature is 60 to 100° C.; and / or the screening mesh number of the particle size screening is 30 to 300 mesh; and / or the second drying temperature is 60 to 100° C.
[0012] Furthermore, step S2 also includes the step of subjecting the raw gas to a second pretreatment, the second pretreatment including: subjecting the raw gas to gas dehydration and gas deoxygenation in sequence; preferably, using one or more of spherical calcium chloride, spherical molecular sieve and color-changing silica gel for gas dehydration; and / or using one or more of 401 deoxidizer, PSN deoxidizer and PSE deoxidizer for gas deoxidation; more preferably, the dehydration method also includes the step of returning the tail gas to the second pretreatment.
[0013] Further, in step S3, the reaction product is cooled under an inert gas atmosphere, and the inert gas includes N2 and / or Ar; preferably, the flow rate of the inert gas is 0.1 to 10 L / min, and more preferably 0.2 to 8 L / min.
[0014] Furthermore, in the low-hydrated magnesium chloride, the weight percentage of basic magnesium chloride impurities is ≤5%; preferably, the average molar number of crystal water contained in each low-hydrated magnesium chloride molecule is ≤1, and the weight percentage of basic magnesium chloride impurities is ≤3%.
[0015] The present invention provides a new method for catalytic dehydration of bischofite using a rotating fluidized reactor, with catalytic coupled dehydration as the basic principle, and process optimization is performed in combination with a fluidized reactor. By using a rotating fluidized reactor and controlling the process parameters of the reactor, the solid material in the reactor can be fully contacted with the feed gas and maintained in an expanded state, and the mass transfer and heat transfer effect is good, avoiding the agglomeration phenomenon caused by the dehydration shrinkage of the material during the amplification reaction, and ensuring the uniformity of the product. At the same time, specific reaction parameters enable the catalytic dehydration reaction to be fully and efficiently carried out, and with lower energy consumption, more convenient operation, and milder reaction conditions, a larger yield and higher quality of low-water magnesium chloride are obtained, which provides a basis for realizing industrial-grade production amplification and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0017] Figure 1 A process flow chart according to an embodiment of the present invention is shown; and
[0018] Figure 2 A process apparatus diagram according to an embodiment of the present invention is shown.
[0019] The above drawings include the following reference numerals:
[0020] 1-1 and 1-2, electric blast drying oven; 2, mortar; 3, sieve; 4-1 and 4-2, gas cylinder; 5-1 and 5-2, safety valve; 6-1 and 6-2, flow meter; 7-1 and 7-2, one-way valve; 8, gas storage tank; 9, dehydration and deoxygenation device; 10, rotor flow meter; 11, rotating fluidized bed reactor; 12, sieve plate; 13, electric motor; 14, control panel; 15, vacuum pump. DETAILED DESCRIPTION
[0021] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0022] As described in the background of the present invention, there is a problem in the prior art that the material of the bischofite catalytic coupled dehydration reaction is easy to agglomerate, and the mass transfer and heat transfer are poor, resulting in a high water content and low purity of the magnesium chloride product. In order to solve the above problems, in a typical embodiment of the present invention, a dehydration method of bischofite is provided, comprising the following steps: step S1, feeding the bischofite into a rotating fluidized reactor; step S2, vacuumizing the rotating fluidized reactor, and then passing the raw gas to carry out a catalytic dehydration reaction to obtain a reaction product and tail gas; step S3, cooling the reaction product to obtain low-water magnesium chloride, and the average molar number of crystal water contained in each low-water magnesium chloride molecule is ≤2; wherein the raw gas includes carbon monoxide and / or methane; the rotation speed of the rotating fluidized reactor is 1-200r / min, the bed pressure is 0.1-1MPa, and the bed is inclined upward from the material inlet to the material outlet, and the inclination angle is 0-60°; the reaction temperature of the catalytic dehydration reaction is 50-300°C.
[0023] Specifically, bischofite is first sent into a rotating fluidized reactor, and a raw gas including carbon monoxide and / or methane is introduced after vacuuming, and the bed pressure, the rotating speed of the reactor, and the bed inclination angle are adjusted, and the temperature control program is adjusted to carry out catalytic dehydration reaction. During the reaction, the oxygen atom of the crystal water in bischofite can be used as a site for adsorbing raw gas molecules, such as CO, which is used as raw gas. After charge redistribution, dissociation and reorganization will form a formic acid intermediate, and further coupling catalytic dehydration occurs through the formic acid intermediate to obtain a dehydration reaction product and tail gas. In this process, the bischofite solid material can be fully contacted with the raw gas and maintain an expanded state, and the mass transfer and heat transfer effect is good, and it is not easy to cause uneven heating to cause material dehydration and agglomeration. Finally, the reaction product is cooled to obtain the low-water magnesium chloride having an average molar number of crystal water contained in each molecule ≤2.
[0024] The rotating fluidized bed reactor has a certain effect of improving mass transfer and heat transfer, but for materials such as bischofite that contain crystal water and the water and magnesium chloride are tightly combined, the corresponding improvement effect is not significant and the crystal water content requirement of high-quality low-water magnesium chloride cannot be achieved.
[0025] The present invention achieves the best experimental condition range by adjusting various parameters in the process. Within the above parameter range, the solid materials evolved in the dehydration process can be fully contacted with the reaction gas and maintained in an expanded state, the temperature in the kiln is balanced, and the problems such as agglomeration caused by dehydration shrinkage of the materials during the amplification reaction are avoided, and a high-quality magnesium chloride product with an average molar number of crystal water contained in each molecule of ≤2 and a byproduct hydroxymagnesium chloride content of ≤2% is obtained. Compared with the magnesium chloride product prepared by a fixed bed, the water content of the low-water magnesium chloride prepared by the dehydration method of the present invention can be reduced by 5-20%, and the content of byproducts (such as hydroxymagnesium chloride / basic magnesium chloride) can be reduced by about 0.2-1%.
[0026] The invention provides a novel method for catalytic dehydration of bischofite using a rotating fluidized reactor, with catalytic coupled dehydration as the basic principle, combined with a fluidized reactor for process optimization, gas-solid materials in the rotating fluidized reactor can be fully contacted, greatly improving the problems of material agglomeration and poor mass and heat transfer in the catalytic dehydration reaction, making the catalytic dehydration reaction fully efficient, and significantly reducing the water content of the magnesium chloride product, and improving the purity of the magnesium chloride product. At the same time, the method of the present invention can also reduce the energy consumption and equipment corrosion of magnesium chloride dehydration, while achieving full dehydration of bischofite, reducing the occurrence of hydrolysis side reactions, greatly reducing the cost of magnesium chloride dehydration, providing a basis for realizing industrial-grade production amplification, and having reference significance for the dehydration of other inorganic salts, and having broad application prospects.
[0027] In order to further promote the contact between the raw gas and the bischofite material and accelerate the catalytic dehydration reaction rate, in a preferred embodiment, in step S2, the gas flow rate of the raw gas is 0.1 to 20 L / min, preferably 1 to 10 L / min.
[0028] In order to provide a more suitable gas environment and further avoid the effect of impurities in the air on the catalytic dehydration reaction rate, in a preferred embodiment, in step S2, an auxiliary gas is introduced while the raw gas is introduced, and the auxiliary gas includes one or more of hydrogen, nitrogen and carbon dioxide; preferably, the volume ratio of the raw gas to the auxiliary gas is (0.1-19):1. Under the above conditions, the catalytic dehydration reaction of the raw gas and the hydrochlorobenzene is more sufficient, which is conducive to the preparation of a magnesium chloride product with lower water content and higher purity.
[0029] In a preferred embodiment, in step S2, the vacuum degree of the rotating fluidized reactor is -0.1 to 0 MPa; and / or the rotation speed of the rotating fluidized reactor is 2 to 100 r / min; and / or the bed pressure of the rotating fluidized reactor is 0.1 to 0.5 MPa; and / or the bed of the rotating fluidized reactor is tilted upward from the material inlet to the material outlet, and the tilt angle is 0 to 45°. Under the above parameter conditions, the solid material can be better contacted with the raw gas and maintained in an expanded state, thereby further improving the mass transfer and heat transfer effect, reducing the agglomeration phenomenon, and thus being more conducive to the full progress of the catalytic dehydration reaction.
[0030] In order to further reduce the decomposition of magnesium chloride and the corrosion of equipment caused by the generation of HCl while fully dehydrating the bischofite, in a preferred embodiment, in step S2, the reaction temperature of the catalytic dehydration reaction is 80 to 300° C., the reaction time is 3 to 30 h, and the heating rate is 1 to 50° C. / min, preferably 1 to 30° C. / min.
[0031] In a preferred embodiment, in step S1, the amount of bischofite charged to the rotating fluidized bed reactor is 0.1-2000 g, preferably 1-1000 g, which can avoid material agglomeration while further improving the single material processing capacity of the process, which is conducive to large-scale industrial production.
[0032] In order to further improve the dehydration effect of bischofite, better maintain the fluidized state of the material to avoid agglomeration, and make the process of the present invention applicable to bischofite raw materials of different particle sizes, in a preferred embodiment, step S1 also includes the step of subjecting the bischofite to a first pretreatment, and the first pretreatment includes: subjecting the bischofite to a first drying, grinding, particle size screening and a second drying in sequence to obtain a pretreated bischofite, wherein the average number of moles of crystal water contained in each pretreated bischofite molecule is 3 to 5; preferably, the temperature of the first drying is 50 to 120° C., and the time is 1 to 8 hours; and / or the screening mesh number of the particle size screening is 20 to 500 mesh; and / or the temperature of the second drying is 50 to 120° C., and the time is 1 to 8 hours; more preferably, the temperature of the first drying is 60 to 100° C.; and / or the screening mesh number of the particle size screening is 30 to 300 mesh; and / or the temperature of the second drying is 60 to 100° C. The above pretreatment parameters are more conducive to avoiding agglomeration of the initial bischofite material in a fluidized state, thereby preparing a product with uniform quality and good quality.
[0033] Based on similar reasons, in a preferred embodiment, step S2 also includes the step of subjecting the raw gas to a second pretreatment, and the second pretreatment includes: subjecting the raw gas to gas dehydration and gas deoxygenation in sequence; preferably, using one or more of spherical calcium chloride, spherical molecular sieve and color-changing silica gel for gas dehydration; and / or using one or more of 401 deoxidizer, PSN deoxidizer and PSE deoxidizer for gas deoxidation; more preferably, the dehydration method also includes the step of returning the tail gas to the second pretreatment, which can achieve the recycling of the raw gas and further improve the economy of the overall process.
[0034] In a preferred embodiment, in step S3, the reaction product is cooled under an inert gas atmosphere, wherein the inert gas includes N2 and / or Ar; preferably, the flow rate of the inert gas is 0.1 to 10 L / min, more preferably 0.2 to 8 L / min. Under the above conditions, the increase in water content and the decrease in purity caused by the dehydrated magnesium chloride combining with moisture in the air can be better reduced.
[0035] As described above, the preparation method of the present invention can prepare a magnesium chloride product with low water content and high purity. In a preferred embodiment, in the low-water magnesium chloride, the weight percentage of basic magnesium chloride impurities is ≤5%; preferably, the average molar number of crystal water contained in each low-water magnesium chloride molecule is ≤1, and the weight percentage of basic magnesium chloride impurities is ≤3%, which has higher economic value.
[0036] Specifically, in one embodiment, the process flow chart is as follows: Figure 1 As shown, the bischofite raw material is preliminarily dried, ground into powder of a certain particle size, and then screened for particle size, and then dried again and sent to a rotating fluidized reactor; the raw gas is sent to a rotating fluidized reactor after being treated with dehydration and deoxygenation. If the raw gas uses a variety of gases, the gas raw materials can be mixed before dehydration and deoxygenation; in the rotating fluidized reactor, the bischofite solid material and the raw gas are contacted to perform a catalytic dehydration reaction, and most of the crystal water in the bischofite material is removed to obtain low-water magnesium chloride, and the product quality inspection is performed after the material is discharged.
[0037] Specifically, in one embodiment, the process device diagram is as follows: Figure 2As shown, the bischofite raw material is sent to the electric hot air drying oven 1-1 for preliminary drying, and then the preliminary dried material is ground into a powder of a certain particle size in a mortar 2, and then the particle size is screened using a screen 3, and the screened material is sent to the electric hot air drying oven 1-2 for further drying and further dehydration, and then the material is sent to the rotating fluidized reactor 11 (here refers to the main part of the reactor, which is inclined upward from the material inlet to the material outlet), and the vacuum pump 15 is turned on to control the vacuum degree; the safety valves 5-1 and 5-2, the flow meters 6-1 and 6-2, and the one-way valves 7-1 and 7-2 are turned on, and the raw gas in the gas cylinders 4-1 and 4-2 is sent to the gas storage tank 8 for mixing, and then sent to the dehydration and deoxygenation device 9 for dehydration and deoxygenation treatment, and then the raw gas is sent to the rotating fluidized reactor 11, and the flow of the mixed gas is monitored by the rotor flowmeter 10. In the rotating fluidized reactor 11, the pretreated bischofite and the raw gas enter the reactor through the sieve plate 12, and the reactor rotates under the drive of the motor 13, so that the materials in the reactor are in a fluidized state, and the gas-solid materials are fully contacted to perform a catalytic dehydration reaction, and the reaction parameters are set through the control panel 14. It can be understood that the number of gas cylinders can be adaptively increased or decreased according to the number of types of raw gas.
[0038] Typically but not limiting, in step S2, the rotation speed of the rotating fluidized bed reactor is 1 r / min, 2 r / min, 5 r / min, 10 r / min, 50 r / min, 100 r / min, 150 r / min, 200 r / min or a range consisting of any two of them, the bed pressure is 0.1 MPa, 0.2 MPa, 0.5 MPa, 0.8 MPa, 1 MPa or a range consisting of any two of them, and the bed inclination angle is 0°, 10°, 20°, 30°, 40°, 45°, 50°, 60° or a range consisting of any two of them.
[0039] Typically but not limiting, in step S2, the reaction temperature of the catalytic dehydration reaction is 50°C, 80°C, 100°C, 150°C, 200°C, 250°C, 300°C or a range consisting of any two of them, the reaction time is 3h, 5h, 10h, 15h, 20h, 25h, 30h or a range consisting of any two of them, and the heating rate is 1°C / min, 5°C / min, 10°C / min, 20°C / min, 30°C / min, 40°C / min, 50°C / min or a range consisting of any two of them.
[0040] Typically but not limiting, in step S2, the gas flow rate of the raw gas is 0.1L / min, 1L / min, 5L / min, 10L / min, 15L / min, 20L / min or a range consisting of any two of them; the volume ratio of the raw gas to the auxiliary gas is 0.1:1, 1:1, 5:1, 10:1, 15:1, 19:1 or a range consisting of any two of them.
[0041] Typically but not limitatively, in step S1, in the first pretreatment, the first drying temperature is 50°C, 60°C, 100°C, 150°C, 180°C, 200°C or a range consisting of any two of them, and the time is 1h, 2h, 4h, 6h, 8h or a range consisting of any two of them; the second drying temperature is 50°C, 60°C, 100°C, 150°C, 180°C, 200°C or a range consisting of any two of them, and the time is 1h, 2h, 4h, 6h, 8h or a range consisting of any two of them; the bischofite charge amount of the rotating fluidized bed reactor is 0.1g, 1g, 10g, 100g, 500g, 1000g, 1500g, 2000g or a range consisting of any two of them.
[0042] Typically but not limitatively, in step S3, the flow rate of the inert gas is 0.1 L / min, 0.2 L / min, 1 L / min, 2 L / min, 5 L / min, 8 L / min, 10 L / min or a range consisting of any two of them.
[0043] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0044] Example 1
[0045] Bischofite pretreatment: Weigh 1 g of bischofite (GR, 99.99%) and put it into an oven at 70°C to dry for 2 h. At this time, the sample is in an agglomerated state. After all of it is taken out, it is ground into a mortar. The material of 80 mesh is sieved out with a sieve, and then put into an oven at 70°C to dry for 2 h to obtain pretreated bischofite. The average molar number of crystal water contained in each pretreated bischofite molecule is 3.5;
[0046] Raw gas pretreatment: dehydrate the CO / N2 balance gas (the volume ratio of CO and N2 is 15:1) using spherical calcium chloride and deoxidize the gas using 401 deoxidizer to obtain pretreated CO / N2 balance gas;
[0047] Step S1, taking 10 g of pretreated bischofite, and rapidly adding it into a rotating fluidized bed reactor;
[0048] Step S2, leak detection of the rotating fluidized reactor, close the inlet and outlet valves, evacuate to a vacuum degree of -0.1MPa, then introduce the pre-treated CO / N2 balance gas, and when the bed pressure reaches 0.1MPa, open the tail gas valve. Adjust the gas flow rate to 1L / min, control the bed pressure to 0.1MPa, the reactor speed to 5r / min, the bed inclination angle to 0°, and increase the temperature from room temperature to 130°C at a heating rate of 5°C / min. The reaction time is 8h to carry out catalytic dehydration reaction to obtain reaction products and tail gas. The tail gas is returned to the front process and recycled after pretreatment;
[0049] Step S3, cooling the reaction product to room temperature under the protection of an inert gas flow of N2 at 1 L / min, tilting the rotary fluidized reactor until the material is completely poured out, and obtaining a low-water magnesium chloride product.
[0050] Example 2
[0051] Bischofite pretreatment: 100 g of bischofite (GR, 99.99%) was weighed and placed in an oven at 70° C. for 2 h. At this time, the sample was in an agglomerated state. All of the sample was taken out and ground in a mortar. The material of 80 mesh was sieved out with a sieve and then placed in an oven at 70° C. for 2 h to obtain pretreated bischofite. The average molar number of crystal water contained in each pretreated bischofite molecule was 3.5.
[0052] Raw gas pretreatment: The CO / N2 balance gas (the volume ratio of CO and N2 is 17:1) is sequentially dehydrated using spherical calcium chloride and spherical molecular sieves, and deoxidized using 401 deoxidizer and PSN deoxidizer to obtain pretreated CO / N2 balance gas;
[0053] Step S1, taking 50 g of pretreated bischofite and rapidly adding it into a rotating fluidized bed reactor;
[0054] Step S2, leak detection of the rotating fluidized reactor, close the inlet and outlet valves, evacuate to a vacuum degree of -0.1MPa, then introduce the pre-treated CO / N2 balance gas, and when the bed pressure reaches 0.1MPa, open the tail gas valve. Adjust the gas flow rate to 1L / min, control the bed pressure to 0.1MPa, the reactor speed to 5r / min, the bed inclination angle to 10°, and increase the temperature from room temperature to 130°C at a heating rate of 5°C / min. The reaction time is 8h to carry out catalytic dehydration reaction to obtain reaction products and tail gas, and the tail gas is returned to the front process and recycled after pretreatment;
[0055] Step S3, cooling the reaction product to room temperature under the protection of an inert gas flow of N2 at 1 L / min, tilting the rotary fluidized reactor until the material is completely poured out, and obtaining a low-water magnesium chloride product.
[0056] Example 3
[0057] Bischofite pretreatment: 1000 g of bischofite (GR, 99.99%) was weighed and placed in an oven at 70° C. for 2 h. At this time, the sample was in an agglomerated state. All of the sample was taken out and ground in a mortar. The material of 80 mesh was sieved out with a sieve and then placed in an oven at 70° C. for 2 h to obtain pretreated bischofite. The average molar number of crystal water contained in each pretreated bischofite molecule was 3.5.
[0058] Raw gas pretreatment: The CO / N2 balance gas (the volume ratio of CO and N2 is 16:1) is sequentially dehydrated using spherical calcium chloride, spherical molecular sieve and color-changing silica gel, and the gas is deoxidized using 401 deoxidizer to obtain pretreated CO / N2 balance gas;
[0059] Step S1, taking 250 g of pretreated bischofite, and rapidly adding it into a rotating fluidized bed reactor;
[0060] Step S2, leak detection of the rotating fluidized reactor, close the inlet and outlet valves, evacuate to a vacuum degree of -0.1MPa, then introduce the pre-treated CO / N2 balance gas, and when the bed pressure reaches 0.1MPa, open the tail gas valve. Adjust the gas flow rate to 1L / min, control the bed pressure to 0.1MPa, the reactor speed to 10r / min, the bed inclination angle to 5°, and increase the temperature from room temperature to 130°C at a heating rate of 5°C / min. The reaction time is 8h to carry out catalytic dehydration reaction to obtain reaction products and tail gas, and the tail gas is returned to the front process and recycled after pretreatment;
[0061] Step S3, cooling the reaction product to room temperature under the protection of an inert gas flow of N2 at 1 L / min, tilting the rotary fluidized reactor until the material is completely poured out, and obtaining a low-water magnesium chloride product.
[0062] Example 4
[0063] Bischofite pretreatment: Weigh 40 g of bischofite (GR, 99.99%) and put it into an oven at 70°C to dry for 2 h. At this time, the sample is in an agglomerated state. After all of it is taken out, it is ground into a mortar. The material of 80 mesh is sieved out with a sieve, and then put into an oven at 70°C to dry for 2 h to obtain pretreated bischofite. The average molar number of crystal water contained in each pretreated bischofite molecule is 3.5;
[0064] Raw gas pretreatment: The CO / N2 balance gas (the volume ratio of CO and N2 is 10:1) is sequentially dehydrated using spherical molecular sieves and color-changing silica gel, and deoxidized using 401 deoxidizer, PSN deoxidizer and PSE deoxidizer to obtain pretreated CO / N2 balance gas;
[0065] Step S1, taking 10 g of pretreated bischofite, and rapidly adding it into a rotating fluidized bed reactor;
[0066] Step S2, leak detection of the rotating fluidized reactor, close the inlet and outlet valves, evacuate to a vacuum degree of -0.1MPa, then introduce the pre-treated CO / N2 balance gas, and when the bed pressure reaches 0.1MPa, open the tail gas valve. Adjust the gas flow rate to 2L / min, control the bed pressure to 0.1MPa, the reactor speed to 10r / min, the bed inclination angle to 10°, and increase the temperature from room temperature to 130°C at a heating rate of 5°C / min. The reaction time is 8h to carry out catalytic dehydration reaction to obtain reaction products and tail gas. The tail gas is returned to the front process and recycled after pretreatment;
[0067] Step S3, cooling the reaction product to room temperature under the protection of an inert gas flow of N2 at 1 L / min, tilting the rotary fluidized reactor until the material is completely poured out, and obtaining a low-water magnesium chloride product.
[0068] Example 5
[0069] Bischofite pretreatment: Weigh 200 g of bischofite (GR, 99.99%) and put it into an oven at 70°C to dry for 2 h. At this time, the sample is in an agglomerated state. After all of it is taken out, it is ground into a mortar. The material of 80 mesh is sieved out with a sieve, and then put into an oven at 70°C to dry for 2 h to obtain pretreated bischofite. The average molar number of crystal water contained in each pretreated bischofite molecule is 3.5;
[0070] Raw gas pretreatment: The CO / N2 balance gas (the volume ratio of CO and N2 is 15:1) is sequentially dehydrated using spherical calcium chloride, spherical molecular sieve and color-changing silica gel, and the gas is deoxidized using PSN deoxidizer and PSE deoxidizer to obtain pretreated CO / N2 balance gas;
[0071] Step S1, taking 50 g of pretreated bischofite and rapidly adding it into a rotating fluidized bed reactor;
[0072] Step S2, leak detection of the rotating fluidized reactor, close the inlet and outlet valves, evacuate to a vacuum degree of -0.1MPa, then introduce the pre-treated CO / N2 balance gas, and when the bed pressure reaches 0.1MPa, open the tail gas valve. Adjust the gas flow rate to 2L / min, control the bed pressure to 0.1MPa, the reactor speed to 10r / min, the bed inclination angle to 15°, and increase the temperature from room temperature to 130°C at a heating rate of 5°C / min. The reaction time is 8h to carry out catalytic dehydration reaction to obtain reaction products and tail gas. The tail gas is returned to the front process and recycled after pretreatment;
[0073] Step S3, cooling the reaction product to room temperature under the protection of an inert gas flow of N2 at 1 L / min, tilting the rotary fluidized reactor until the material is completely poured out, and obtaining a low-water magnesium chloride product.
[0074] Example 6
[0075] Bischofite pretreatment: 1000 g of bischofite (GR, 99.99%) was weighed and placed in an oven at 70° C. for 2 h. At this time, the sample was in an agglomerated state. All of the sample was taken out and ground in a mortar. The material of 80 mesh was sieved out with a sieve and then placed in an oven at 70° C. for 2 h to obtain pretreated bischofite. The average molar number of crystal water contained in each pretreated bischofite molecule was 3.5.
[0076] Raw gas pretreatment: The CO / N2 balance gas (the volume ratio of CO and N2 is 15:1) is sequentially dehydrated using spherical calcium chloride and deoxidized using PSN deoxidizer to obtain pretreated CO / N2 balance gas;
[0077] Step S1, taking 250 g of pretreated bischofite, and rapidly adding it into a rotating fluidized bed reactor;
[0078] Step S2, leak detection of the rotating fluidized reactor, close the inlet and outlet valves, evacuate to a vacuum degree of -0.1MPa, then introduce the pre-treated CO / N2 balance gas, and when the bed pressure reaches 0.1MPa, open the tail gas valve. Adjust the gas flow rate to 2L / min, control the bed pressure to 0.1MPa, the reactor speed to 10r / min, the bed inclination angle to 20°, and increase the temperature from room temperature to 130°C at a heating rate of 5°C / min. The reaction time is 8h to carry out catalytic dehydration reaction to obtain reaction products and tail gas. The tail gas is returned to the front process and recycled after pretreatment;
[0079] Step S3, cooling the reaction product to room temperature under the protection of an inert gas flow of N2 at 1 L / min, tilting the rotary fluidized reactor until the material is completely poured out, and obtaining a low-water magnesium chloride product.
[0080] Example 7
[0081] The difference from Example 1 is that
[0082] Bischofite pretreatment: 1000 g of bischofite (GR, 99.99%) was weighed and placed in a 50° C. oven for drying for 8 h. At this time, the sample was in an agglomerated state. All of the sample was taken out and ground in a mortar. The 20-mesh material was sieved out with a sieve and then placed in a 50° C. oven for drying for 8 h to obtain pretreated bischofite. The average molar number of crystal water contained in each pretreated bischofite molecule was 5.
[0083] In step S1, 0.1 g of pretreated bischofite is taken and quickly added into a rotating fluidized bed reactor.
[0084] Example 8
[0085] The difference from Example 1 is that
[0086] Bischofite pretreatment: 1000 g of bischofite (GR, 99.99%) was weighed and placed in an oven at 60° C. for 5 h. At this time, the sample was in an agglomerated state. All of the sample was taken out and ground in a mortar. The 30-mesh material was sieved out with a sieve and then placed in an oven at 60° C. for 5 h to obtain pretreated bischofite. The average molar number of crystal water contained in each pretreated bischofite molecule was 4.5.
[0087] In step S1, 1 g of pretreated bischofite is taken and quickly added into a rotating fluidized bed reactor.
[0088] Example 9
[0089] The difference from Example 1 is that
[0090] Bischofite pretreatment: 1000 g of bischofite (GR, 99.99%) was weighed and placed in an oven at 120° C. for 5 h. At this time, the sample was in an agglomerated state. All of the sample was taken out and ground in a mortar. The 300-mesh material was sieved out with a sieve and then placed in an oven at 120° C. for 5 h to obtain pretreated bischofite. The average molar number of crystal water contained in each pretreated bischofite molecule was 3.5.
[0091] In step S1, 1000 g of pretreated bischofite is taken and quickly added into a rotating fluidized bed reactor.
[0092] Example 10
[0093] The difference from Example 1 is that
[0094] Bischofite pretreatment: 1000 g of bischofite (GR, 99.99%) was weighed and placed in an oven at 100° C. for 1 h. At this time, the sample was in an agglomerated state. All of the sample was taken out and ground in a mortar. The material of 500 mesh was sieved out with a sieve and then placed in an oven at 100° C. for 1 h to obtain pretreated bischofite. The average molar number of crystal water contained in each pretreated bischofite molecule was 3;
[0095] In step S1, 2000 g of treated bischofite is taken and quickly added into a rotating fluidized bed reactor.
[0096] Embodiment 11
[0097] The difference from Example 1 is that
[0098] Step S2, leak detection of the rotating fluidized reactor, close the inlet and outlet valves, evacuate to a vacuum degree of -0.1MPa, then introduce the pre-treated CO / N2 balance gas, and when the bed pressure reaches 0.1MPa, open the tail gas valve. Adjust the gas flow rate to 0.1L / min, control the bed pressure to 0.1MPa, the reactor speed to 1r / min, the bed inclination angle to 0°, and increase the temperature from room temperature to 50°C at a heating rate of 5°C / min. The reaction time is 8h to carry out catalytic dehydration reaction to obtain reaction products and tail gas. The tail gas is returned to the front process and recycled after pretreatment;
[0099] Step S3, cooling the reaction product to room temperature under the protection of an inert gas flow of N2 at 0.1 L / min, tilting the rotary fluidized reactor until the material is completely poured out, and obtaining a low-water magnesium chloride product.
[0100] Example 12
[0101] The difference from Example 1 is that
[0102] Raw gas pretreatment: methane / H2 balance gas (the volume ratio of methane to H2 is 10:1) is dehydrated using spherical calcium chloride and deoxygenated using 401 deoxidizer to obtain pretreated methane / H2 balance gas;
[0103] Step S2, leak detection of the rotating fluidized reactor, close the inlet and outlet valves, evacuate to a vacuum degree of -0.5MPa, then introduce pre-treated methane / H2 balance gas, and when the bed pressure reaches 0.1MPa, open the tail gas valve. Adjust the gas flow rate to 1L / min, control the bed pressure to 0.1MPa, the reactor speed to 2r / min, the inclination angle of the bed to 0°, and increase the temperature from room temperature to 130°C at a heating rate of 5°C / min. The reaction time is 8h to carry out catalytic dehydration reaction to obtain reaction products and tail gas, and the tail gas is returned to the front process and recycled after pretreatment;
[0104] Step S3, cooling the reaction product to room temperature under the protection of an inert gas flow of N2 at 0.2 L / min, tilting the rotary fluidized reactor until the material is completely poured out, and obtaining a low-water magnesium chloride product.
[0105] Example 13
[0106] The difference from Example 1 is that
[0107] Raw gas pretreatment: methane / H2 balance gas (the volume ratio of methane to H2 is 10:1) is dehydrated using spherical calcium chloride and deoxygenated using 401 deoxidizer to obtain pretreated methane / H2 balance gas;
[0108] Step S2, leak detection of the rotating fluidized reactor, close the inlet and outlet valves, evacuate to a vacuum degree of -0.5MPa, then introduce pretreated methane / H2 balance gas, and when the bed pressure reaches 0.5MPa, open the tail gas valve. Adjust the gas flow rate to 10L / min, control the bed pressure to 0.5MPa, the reactor speed to 100r / min, the bed inclination angle to 45°, and increase the temperature from room temperature to 130°C at a heating rate of 5°C / min. The reaction time is 8h to carry out catalytic dehydration reaction to obtain reaction products and tail gas. The tail gas is returned to the front process and recycled after pretreatment;
[0109] Step S3, cooling the reaction product to room temperature under the protection of an inert gas flow of N2 at 8 L / min, tilting the rotary fluidized reactor until the material is completely poured out, and obtaining a low-water magnesium chloride product.
[0110] Embodiment 14
[0111] The difference from Example 1 is that
[0112] Step S2, leak detection of the rotating fluidized reactor, close the inlet and outlet valves, evacuate to a vacuum degree of 0MPa, then introduce the pre-treated CO / N2 balance gas, and open the tail gas valve when the bed pressure reaches 1MPa. Adjust the gas flow rate to 20L / min, control the bed pressure to 1MPa, the reactor speed to 200r / min, the bed inclination angle to 20°, and increase the temperature from room temperature to 300°C at a heating rate of 5°C / min. The reaction time is 8h to carry out catalytic dehydration reaction to obtain reaction products and tail gas. The tail gas is returned to the front process and recycled after pretreatment;
[0113] Step S3, cooling the reaction product to room temperature under the protection of an inert gas flow of N2 at a flow rate of 10 L / min, tilting the rotary fluidized reactor until the material is completely poured out, and obtaining a low-water magnesium chloride product.
[0114] Embodiment 15
[0115] The difference from Example 1 is that
[0116] Raw gas pretreatment: dehydrate the CO / N2 balance gas (the volume ratio of CO and N2 is 0.1:1) using spherical calcium chloride and deoxidize the gas using 401 deoxidizer to obtain pretreated CO / N2 balance gas;
[0117] Step S2, leak detection of the rotating fluidized reactor, closing the inlet and outlet valves, evacuating to a vacuum degree of -0.1MPa, then introducing the pre-treated CO / N2 balance gas, and opening the tail gas valve when the bed pressure reaches 0.1MPa. Adjust the gas flow rate to 1L / min, control the bed pressure to 0.1MPa, the reactor speed to 5r / min, the inclination angle of the bed to 0°, and increase the temperature from room temperature to 80°C at a heating rate of 1°C / min. The reaction time is 30h to carry out catalytic dehydration reaction to obtain reaction products and tail gas, and the tail gas is returned to the front process and recycled after pretreatment.
[0118] Example 16
[0119] The difference from Example 1 is that
[0120] Raw gas pretreatment: dehydrate the CO / N2 balance gas (the volume ratio of CO and N2 is 19:1) using spherical calcium chloride and deoxidize the gas using 401 deoxidizer to obtain pretreated CO / N2 balance gas;
[0121] Step S2, leak detection of the rotating fluidized reactor, closing the inlet and outlet valves, evacuating to a vacuum degree of -0.1MPa, then introducing the pre-treated CO / N2 balance gas, and opening the tail gas valve when the bed pressure reaches 0.1MPa. Adjust the gas flow rate to 1L / min, control the bed pressure to 0.1MPa, the reactor speed to 5r / min, the inclination angle of the bed to 0°, and increase the temperature from room temperature to 300°C at a heating rate of 50°C / min. The reaction time is 3h to carry out catalytic dehydration reaction to obtain reaction products and tail gas, and the tail gas is returned to the front process and recycled after pretreatment.
[0122] Comparative Example 1
[0123] The difference from Example 1 is that a conventional fixed bed reactor is used.
[0124] Comparative Example 2
[0125] The difference from Example 2 is that a conventional fixed bed reactor is used.
[0126] The magnesium chloride products prepared in the above examples and comparative examples were measured, and the results are shown in Table 1.
[0127] Crystallization water content: The Karl Fischer method is used for accurate measurement. To reduce experimental errors, Karl Fischer water meters from different laboratories can be used to perform multiple measurements under the same temperature and humidity conditions and take the average value.
[0128] Basic magnesium chloride content: iodine titration is used for accurate calculation. To reduce experimental errors, multiple titration experiments can be performed and the average value can be taken.
[0129] Table 1
[0130]
[0131]
[0132] As can be seen from the above, compared with the comparative example, each embodiment of the present invention is based on catalytic coupled dehydration as the basic principle, and combines the fluidized reactor for process optimization. By using a rotating fluidized reactor and controlling the reactor process parameters, the solid material in the reactor can be fully contacted with the raw gas and maintained in an expanded state, and the mass transfer and heat transfer effect is good, avoiding the agglomeration phenomenon caused by the dehydration shrinkage of the material during the amplification reaction, and ensuring the uniformity of the product. At the same time, specific reaction parameters enable the catalytic dehydration reaction to be fully and efficiently carried out, with lower energy consumption, more convenient operation, and milder reaction conditions, a larger yield and higher quality of low-water magnesium chloride are obtained, which provides a basis for realizing industrial-grade production amplification, and has broad application prospects.
[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for dehydrating bischofite, characterized in that: The following steps are involved: Step S1, feeding bischofite into a rotating fluidized reactor; Step S2, evacuating the rotary fluidized phase reactor, and then introducing the raw gas to perform a catalytic dehydration reaction to obtain a reaction product and tail gas; Step S3, cooling the reaction product to obtain low-hydrated magnesium chloride, wherein the average molar number of crystal water contained in each molecule of the low-hydrated magnesium chloride is ≤2; Wherein, the raw gas includes carbon monoxide and / or methane; the rotation speed of the rotating fluidized bed reactor is 1-200r / min, the bed pressure is 0.1-1MPa, the bed is inclined upward from the material inlet to the material outlet, and the inclination angle is 0-60°; the reaction temperature of the catalytic dehydration reaction is 50-300°C.
2. The dehydration method according to claim 1, characterized in that: In the step S2, the gas flow rate of the raw gas is 0.1 to 20 L / min, preferably 1 to 10 L / min.
3. The dehydration method according to claim 1 or 2, characterized in that: In the step S2, an auxiliary gas is introduced while the raw gas is introduced, and the auxiliary gas includes one or more of hydrogen, nitrogen and carbon dioxide; Preferably, the volume ratio of the raw gas to the auxiliary gas is (0.1-19):
1.
4. The dehydration method according to any one of claims 1 to 3, characterized in that: In step S2, the vacuum degree of the rotating fluidized bed reactor is -0.1 to 0 MPa; and / or The rotating speed of the rotating fluidized state reactor is 2 to 100 r / min; and / or The bed pressure of the rotating fluidized bed reactor is 0.1-0.5 MPa; and / or The bed layer of the rotating fluidized bed reactor is inclined upward from the material inlet to the material outlet, and the inclination angle is 0-45 degrees.
5. The dehydration method according to any one of claims 1 to 4, characterized in that: In the step S2, the reaction temperature of the catalytic dehydration reaction is 80-300°C, the reaction time is 3-30h, and the heating rate is 1-50°C / min.
6. The dehydration method according to any one of claims 1 to 5, characterized in that: In the step S1, the amount of bischofite charged into the rotary fluidized bed reactor is 0.1 to 2000 g, preferably 1 to 1000 g.
7. The dehydration method according to any one of claims 1 to 6, characterized in that: The step S1 further comprises a step of subjecting the bischofite to a first pretreatment, wherein the first pretreatment comprises: subjecting the bischofite to a first drying, a grinding, a particle size screening and a second drying in sequence to obtain a pretreated bischofite, wherein the average molar number of crystal water contained in each molecule of the pretreated bischofite is 3 to 5; Preferably, the temperature of the first drying is 50-120°C and the time is 1-8 hours; and / or the screening mesh number of the particle size screening is 20-500 mesh; and / or the temperature of the second drying is 50-120°C and the time is 1-8 hours; More preferably, the temperature of the first drying is 60-100°C; and / or the screening mesh number of the particle size screening is 30-300 mesh; and / or the temperature of the second drying is 60-100°C.
8. The dehydration method according to any one of claims 1 to 7, characterized in that: The step S2 further comprises the step of subjecting the raw gas to a second pretreatment, wherein the second pretreatment comprises: subjecting the raw gas to gas dehydration and gas deoxygenation in sequence; Preferably, one or more of spherical calcium chloride, spherical molecular sieve and color-changing silica gel are used to dehydrate the gas; and / or one or more of 401 deoxidizer, PSN deoxidizer and PSE deoxidizer are used to deoxidize the gas; More preferably, the dehydration method further comprises the step of returning the tail gas to the second pretreatment.
9. The dehydration method according to any one of claims 1 to 8, characterized in that: In the step S3, the reaction product is cooled under an inert gas atmosphere, wherein the inert gas comprises N2 and / or Ar; Preferably, the flow rate of the inert gas is 0.1 to 10 L / min, more preferably 0.2 to 8 L / min.
10. The dehydration method according to any one of claims 1 to 9, characterized in that: In the low-water magnesium chloride, the weight percentage of basic magnesium chloride impurities is ≤5%; preferably, the average molar number of crystal water contained in each low-water magnesium chloride molecule is ≤1, and the weight percentage of basic magnesium chloride impurities is ≤3%.