Catalyst for formaldehyde production and preparation method thereof
By using the complexation of organic acids and molybdenum salts or iron salts in the preparation of iron-molybdenum catalysts, a uniform system is formed, and the catalyst is prepared by evaporation crystallization and dehydration and drying, the problems of complex preparation process and wastewater pollution are solved, and the performance of the catalyst is improved and formaldehyde selectivity.
Patent Information
- Application Number
- CN202411141391.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
At present, there are problems such as complex conditions and cumbersome control in the preparation process of iron and molybdenum catalysts, loss of iron and molybdenum components and serious wastewater pollution during the preparation process. At the same time, the by-products in the application stage are relatively large and the selectivity of formaldehyde needs to be improved.
The soluble molybdenum salt and iron salt are dissolved in deionized water respectively, and organic acid is added to form a mixed solution. The catalyst is prepared by stirring, evaporation and crystallization, dehydration and drying, crushing and calcining to form a uniform catalyst precursor, simplifying the preparation process and reducing wastewater pollute.
The catalyst is simple and easy to prepare, the phase composition and pore structure of the catalyst surface is improved, the raw material conversion and selectivity of formaldehyde production is enhanced, and the loss of iron and molybdenum components and wastewater pollution are reduced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a catalyst for formaldehyde production and a preparation method thereof. Background Art
[0002] As an important organic chemical raw material and chemical intermediate, formaldehyde is widely used in many fields such as chemical industry, materials, and medicine. According to a global market survey, the output of CH2O in 2020 was 45.6 metric tons, and it is expected to grow further at an annual rate of 4.65% during the period 2021-2028, reaching a market value of US$37.7 billion by 2028. At the same time, my country has become the world's largest formaldehyde producer and consumer, with formaldehyde production capacity accounting for 55% of the global total production capacity and consumption accounting for 53%. Among the existing formaldehyde production processes in China, the main one is methanol oxidation process. According to the type of catalyst used, it is divided into "silver method" and "iron-molybdenum method". Compared with the "silver method", the "iron-molybdenum method" has the advantages of lower reaction temperature, lower methanol consumption, longer catalyst service life, and can produce high-concentration formaldehyde solution. Therefore, most of the newly built and expanded formaldehyde units in recent years have adopted the iron-molybdenum production process.
[0003] Although iron-molybdenum catalysts have a high single-pass conversion rate, the formaldehyde selectivity in industry is usually only around 94%. The main byproduct of methanol oxidation to formaldehyde is dimethyl ether in the low-temperature stage, and the main byproduct is carbon monoxide formed by excessive oxidation in the high-temperature stage. In industry, by recycling tail gas, on the one hand, the tail gas energy can be fully recycled, and on the other hand, the carbon monoxide content in the reaction atmosphere can be increased to achieve the purpose of suppressing the side reaction. It can be seen that from the perspective of iron-molybdenum catalysts in industry, its selectivity needs to be further improved.
[0004] In addition, the iron-molybdenum catalysts currently used for formaldehyde production are mostly prepared by co-precipitation. For example, Chinese patents CN 106693981 B, CN 115845865 A, CN 107952445 A, U.S. patents US 4829042A, US3978136A, etc. all use co-precipitation to prepare catalysts. Although better activity can be obtained, there are still problems such as complex condition control, cumbersome preparation process, and generation of a large amount of wastewater, which restricts the further development of iron-molybdenum catalysts.
[0005] In order to solve the problem of a large amount of waste water and waste gas generated during the preparation of iron-molybdenum catalysts, Chinese patent application CN110893344A discloses: using metallic iron, organic acid and molybdic acid as raw materials, first metallic iron reacts with organic acid to generate corresponding organic acid iron and hydrogen, then molybdic acid reacts with organic acid iron to generate iron molybdate precipitation and corresponding organic acid, the obtained iron molybdate precipitation is mixed with molybdenum acid solution again and precipitated, filtered, washed, calcined to obtain an iron-molybdenum catalyst with a certain molybdenum-iron ratio. In this method, since molybdenum acid is only slightly soluble in water, only a suspended dispersion can be formed when a high concentration of molybdenum acid mixed solution is prepared in water, thereby affecting the uniformity of the prepared iron molybdate and the catalyst structure. Relative to conventional precipitation methods, although the method reported in this patent reduces the treatment of soluble inorganic salt waste liquids such as ammonium salts and nitrates in production waste liquid, there are a large number of organic acids, slightly soluble molybdic acid and iron molybdate waste water problems in the filtered waste water at the same time.
[0006] In summary, the current iron-molybdenum catalysts not only have problems such as complex condition control, cumbersome process, loss of iron-molybdenum components, and serious wastewater pollution in the preparation stage, but also face the problem of excessive by-products and the need to further improve formaldehyde selectivity in the application stage. Summary of the invention
[0007] One of the purposes of the present invention is to provide a method for preparing a catalyst for formaldehyde production to solve the above problems.
[0008] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is as follows: a method for preparing a catalyst for formaldehyde production, the steps of which are: firstly dissolving a soluble molybdenum salt and an iron salt in deionized water to prepare a molybdenum salt solution and an iron salt solution respectively, then dissolving an organic acid in one of the solutions to obtain a mixed solution, and under stirring conditions, gradually adding the other solution to the mixed solution, stirring evenly, and then evaporating and crystallizing the mixed solution, dehydrating and drying, crushing, molding and calcining to obtain the catalyst.
[0009] As a preferred technical solution, the soluble molybdenum salt is selected from at least one of ammonium octamolybdate, ammonium heptamolybdate, ammonium tetramolybdate, ammonium dimolybdate and molybdenum nitrate.
[0010] As a preferred technical solution, the iron salt is selected from at least one of ferric nitrate, ferrous nitrate, ferric chloride, ferrous chloride, ferrous sulfate and ferrous sulfate.
[0011] As a preferred technical solution, the organic acid is selected from at least one of formic acid, acetic acid, propionic acid, citric acid, tartaric acid, malic acid, ethylenediaminetetraacetic acid, oxalic acid, lactic acid, gluconic acid, glycine, and p-toluenesulfonic acid.
[0012] As a preferred technical solution, the ratio of the organic acid: (molybdenum atom + iron atom) is 0.01 to 10:1 in terms of molar ratio.
[0013] As a preferred technical solution, the ratio of molybdenum atoms contained in the soluble molybdenum salt to iron atoms contained in the soluble iron salt is 1-5:1.
[0014] As a preferred technical solution, the evaporation crystallization and dehydration drying temperatures are between 30 and 150°C, and the calcination temperature is between 300 and 600°C.
[0015] A second object of the present invention is to provide a catalyst prepared by the above method.
[0016] The third object of the present invention is to provide an application of the above-mentioned catalyst, wherein the raw material of the catalyst that can be used for formaldehyde production can be one of methanol, dimethyl ether, methylal, etc.
[0017] Compared with the prior art, the advantages of the present invention are: (1) The present application first utilizes the complexation of organic acid and molybdenum salt or iron salt to form a relatively uniform system when they are mixed with each other, and then obtains the catalyst precursor by evaporation, crystallization, dehydration and drying. The method of the present invention has a simple preparation process, reduces the influence of many unfavorable factors in the coprecipitation method, makes the controllable preparation of the catalyst simple and easy to achieve, and solves the problems of iron and molybdenum component loss and wastewater pollution. (2) The catalyst prepared by the method adopted in the present application has a more suitable catalyst surface phase composition, electronic environment and pore structure, and has a higher raw material conversion rate and formaldehyde selectivity when used in formaldehyde production. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0019] The following is a detailed description of a catalyst for formaldehyde production and a preparation method thereof provided in an embodiment of the present invention. Example
[0020] First, 14.12g of ammonium heptamolybdate and 13.69g of ferric nitrate were added into 150ml and 50ml of deionized water respectively to dissolve to obtain an ammonium heptamolybdate solution and a ferric nitrate solution; 1.28g of oxalic acid was weighed and dissolved in the ammonium heptamolybdate solution to obtain a mixed solution; the rotation speed was controlled at 100r / min and the reaction temperature was 50°C, and the ferric nitrate solution was added into the mixed solution at a rate of 20ml / min, and stirred for 10min to obtain a clarified mixed solution; the clarified mixed solution was then placed in an oven at 90°C for evaporation, crystallization and drying to obtain a catalyst precursor, which was then crushed, calcined at 600°C for 4 hours, and then pressed into shape to obtain a catalyst.
[0021] Examples 2 to 10 have the same preparation methods and steps as Example 1, and the changed materials, addition amounts and process parameters are listed in Table 1.
[0022] Comparative Example 1: First, 14.12 g of ammonium heptamolybdate and 8.22 g of ferric nitrate were added into 150 ml and 50 ml of deionized water respectively to dissolve to obtain an ammonium heptamolybdate solution and a ferric nitrate solution; then, the rotation speed was controlled at 100 r / min and the reaction temperature was 50°C, the pH value of the ammonium heptamolybdate solution was adjusted to 2 with nitric acid, and then the ferric nitrate solution was added into the solution at a rate of 20 ml / min, and the mixture was stirred for 30 min and aged for 2 hours. The precipitate was filtered and dried to obtain a catalyst precursor, which was then crushed and calcined at 500°C for 4 hours and then pressed into tablets to obtain a co-precipitation catalyst.
[0023] The catalytic activity of the catalysts obtained in the above-mentioned embodiments and comparative examples was evaluated. The catalyst activity evaluation was carried out in a fixed bed reactor using methanol as a probe molecule. The raw material methanol vapor was mixed with air to form a reaction gas. The molar content of methanol in the reaction gas was 10%, and the reaction gas space velocity was 12000h -1 , the reaction temperature is 280°C, the reaction pressure is normal pressure, and the evaluation results of the above catalyst are shown in Table 1 below.
[0024] Table 1 Catalyst performance of various examples and comparative examples
[0025] Table 1 lists the differences in the preparation process of each embodiment and comparative example and the performance comparison of the catalyst. It can be seen from the table that, compared with the comparative example 1 without adding organic acid, the embodiments with added organic acid generally have higher methanol conversion rate and formaldehyde selectivity. In Examples 1 to 3, as the proportion of oxalic acid increases, the catalyst conversion rate gradually decreases and the selectivity gradually increases. When the ratio of organic acid to metal element is 1.0, there is a higher formaldehyde yield; Examples 2 and 4 compare the selection of water-soluble molybdenum salt and iron salt raw materials, preferably iron nitrate and ammonium heptamolybdate; Examples 2, 5, and 6 compare the molar ratio of molybdenum to iron elements, and it can be seen that the catalyst performance is better when the molybdenum to iron ratio is 2.5; Examples 5, 7, and 8 use different organic acid additives, and tartaric acid has better catalytic performance, especially the catalyst selectivity is significantly improved; Examples 8 to 10 further compare the effect of calcination temperature on catalytic performance, and it can be seen that 500°C is more conducive to the improvement of formaldehyde yield.
[0026] The method of the present application for preparing the catalyst can form a uniform and transparent system when the materials are mixed due to the complexing and dispersing effect of the organic acid, and even no precipitation is generated. Therefore, the stirring speed, stirring time, reaction temperature and other conditions during the mixing reaction have a very wide adaptability and can be adjusted within a wide range, and are not limited to the process parameters mentioned in the above embodiments, which makes the production simple and easy to control. In addition, the method does not produce precipitation, does not require the use of filtration separation, does not lose iron and molybdenum components and does not produce wastewater, which is convenient for catalyst composition control and clean production.
[0027] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a catalyst for formaldehyde production, characterized in that: The steps are as follows: firstly, soluble molybdenum salt and iron salt are respectively dissolved in deionized water to prepare molybdenum salt solution and iron salt solution, then organic acid is dissolved in one of the solutions to obtain a mixed solution, the other solution is gradually added to the mixed solution under stirring conditions, and after stirring evenly, the mixed solution is evaporated and crystallized, dehydrated and dried, crushed, formed and calcined to obtain the catalyst.
2. The method according to claim 1, characterized in that The soluble molybdenum salt is selected from at least one of ammonium octamolybdate, ammonium heptamolybdate, ammonium tetramolybdate, ammonium dimolybdate and molybdenum nitrate.
3. The method according to claim 1, characterized in that The iron salt is selected from at least one of ferric nitrate, ferrous nitrate, ferric chloride, ferrous chloride, ferrous sulfate and ferrous sulfate.
4. The method according to claim 1, characterized in that The organic acid is selected from at least one of formic acid, acetic acid, propionic acid, citric acid, tartaric acid, malic acid, ethylenediaminetetraacetic acid, oxalic acid, lactic acid, gluconic acid, glycine, and p-toluenesulfonic acid.
5. The method according to claim 1, characterized in that In terms of molar ratio, the ratio of the organic acid to (molybdenum atom+iron atom) is 0.01 to 10:
1.
6. The method according to claim 1, characterized in that The ratio of the molybdenum atoms contained in the soluble molybdenum salt to the iron atoms contained in the soluble iron salt is 1-5:
1.
7. The method according to claim 1, characterized in that The evaporation crystallization and dehydration drying temperatures are between 30 and 150°C, and the calcination temperature is between 300 and 600°C.
8. The catalyst prepared by the method according to any one of claims 1 to 7.
9. Use of the catalyst prepared by the method according to any one of claims 1 to 7, characterized in that: The catalyst is used for preparing formaldehyde by oxidation with methanol, dimethyl ether and methylal as raw materials.
Citation Information
Cited By
Preparation method of shape-controllable iron-molybdenum formaldehyde catalyst
CN120618476A
Preparation method of iron-molybdenum formaldehyde catalyst with controllable morphology
CN120618476B
Iron-molybdenum catalyst for preparing formaldehyde through methanol oxidation and preparation method of iron-molybdenum catalyst
CN122377482A