Zinc-based tin sulfide and preparation method and application thereof

Zinc-based tin sulfide Cs10Zn4Sn4S17 was successfully prepared through solvothermal synthesis, which solved the problems of high reaction temperature and complex operation in the existing technology, achieved low-temperature synthesis and high yield, and provided new applications for optical semiconductor materials.

CN118744997AInactive Publication Date: 2024-10-08宿州学院
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410784055.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, when synthesizing zinc-containing tin sulfide, a high-temperature solid-phase method or a medium-temperature flux method is often used. The reaction temperature is high, the operation is complex, and the flux is toxic. There is a lack of a mild and simple synthesis method.

Method used

Adopting solvothermal synthesis method, by adding Zn powder, Sn powder, S powder and Cs2CO3 into a thick-walled glass tube, adding 1,3-propanediamine and deionized water, reacting at 160-200℃, cooling and washing to obtain free Color block zinc-based tin sulfide Cs10Zn4Sn4S17.

Benefits of technology

The reaction temperature is lower, the conditions are mild, the operation is simple, the yield is as high as 70-75%, and it provides new application prospects for optical semiconductor materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744997A_ABST
    Figure CN118744997A_ABST
Patent Text Reader

Abstract

The invention discloses zinc-based tin sulfide as well as a preparation method and application thereof. The chemical formula of the zinc-based tin sulfide is Cs10Zn4Sn4S17, the zinc-based tin sulfide is composed of [Zn4Sn4S17] 10 <-> anion clusters and equilibrium cations Cs < + >, the zinc-based tin sulfide is crystallized in a cubic system and belongs to a # imgabs0 # space group, and the cell parameters are as follows: # imgabs1 # alpha = beta = gamma = 90 degrees, Z = 1, and # imgabs2 # Dc = 3.816 g / cm < 3 >; the material is prepared by a solvothermal method. The preparation method provided by the invention has the advantages of lower synthesis temperature, mild reaction conditions, higher yield and the like, and has important guiding significance for synthesizing more zinc-based tin sulfides. The optical band gap of the obtained zinc-based tin sulfide is 3.26 eV, and the zinc-based tin sulfide can be used for preparing optical semiconductor devices such as photoelectric conversion materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a multinary metal sulfide, in particular to a zinc-based tin sulfide and a preparation method and application thereof, belonging to the field of semiconductor materials. Background Art

[0002] The rich composition and diverse structures of polysulfides give them excellent physical and chemical properties in the fields of ion conduction, photocatalysis, photoelectric response, nonlinear optics, etc. Therefore, this type of compound has broad application prospects in the preparation of fast ion conductors, photocatalytic materials, optical semiconductor materials and nonlinear optical materials. The preparation of polysulfides has become a research hotspot in the field of inorganic synthesis.

[0003] In recent years, some zinc-containing tin sulfides have been synthesized, which greatly enriched the structural chemistry and material chemistry of this type of compounds. However, the current synthesis of zinc-containing tin sulfides is basically based on high-temperature solid-phase method and medium-temperature flux method. The high-temperature solid-phase method requires a very high reaction temperature and complicated experimental operation. The medium-temperature flux method requires a lower temperature than the high-temperature solid-phase method, but many fluxes have varying degrees of toxicity. In contrast, the low-temperature solvothermal method has the advantages of low reaction temperature, relatively mild reaction conditions, simple operation, and easy adjustment of the ratio of reaction raw materials. Therefore, exploring the use of solvothermal synthesis of zinc-containing tin sulfides is of great significance for the synthesis of more compounds of this type with rich structures and diverse properties. Summary of the invention

[0004] One of the purposes of the present invention is to provide a novel chalcogenide, zinc-based tin sulfide.

[0005] The second object of the present invention is to provide a method for preparing the above zinc-based tin sulfide, which has a low reaction temperature, relatively mild reaction conditions and relatively simple operation.

[0006] The third object of the present invention is to provide the application of the above zinc-based tin sulfide as an optical semiconductor material.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] In the first aspect, the present invention provides a zinc-based tin sulfide, whose chemical formula is Cs 10 Zn4Sn4S 17 , by [Zn4Sn4S 17 ] 10- Anion cluster and counter cation Cs + Composition, crystallizes in the cubic system, belongs to The space group and unit cell parameters are α=β=γ=90°, Z=1, Dc =3.816g / cm 3 .

[0009] In a second aspect, the present invention provides a method for preparing the above-mentioned zinc-based tin sulfide, comprising the following steps:

[0010] (1) According to the chemical formula Cs 10 Zn4Sn4S 17 Weigh Zn powder, Sn powder, S powder, and Cs2CO3 in the molar ratio of each element and put them into a thick-walled glass tube in sequence;

[0011] (2) adding 1,3-propylenediamine and deionized water into a thick-walled glass tube in sequence;

[0012] (3) sealing the tube, after the sealed thick-walled glass tube cools to room temperature, placing it in a reaction kettle, sealing the reaction kettle and placing it in an oven at 160-200° C. for reaction for 6-9 days, and then cooling it to room temperature;

[0013] (4) Wash the mixture in the thick-walled glass tube to obtain colorless block crystals, namely zinc-based tin sulfide Cs 10 Zn4Sn4S 17 .

[0014] Preferably, the amount of 1,3-propylenediamine and deionized water added in step (2) is 8-30% of the volume of the glass tube.

[0015] More preferably, the amount of 1,3-propylenediamine added in step (2) is 7-8 times that of deionized water.

[0016] Preferably, in step (3), the reaction temperature is 160° C. and the reaction time is 7 days.

[0017] Preferably, in step (4), anhydrous ethanol and deionized water are used to wash the mixture.

[0018] In a third aspect, the present invention also provides the use of the above zinc-based tin sulfide as an optical semiconductor material in the preparation of optical semiconductor devices.

[0019] The optical band gap of the zinc-based tin sulfide is 3.26 eV, and the photocurrent under simulated sunlight is about 0.20 μA / cm 2 .

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The zinc-based tin sulfide provided by the present invention is a new type of sulfide containing two metals. In its structure, both Zn and Sn adopt a four-coordination mode to form ZnS4 tetrahedron and SnS4 tetrahedron respectively. Four pairs of ZnS4 tetrahedrons and four pairs of SnS4 tetrahedrons are connected by common vertices to form [Zn4Sn4S 17 ] 10- Anionic clusters.

[0022] 2. The present invention adopts the solvent thermal synthesis method. Compared with the prior art, this method has the advantages of lower reaction temperature, relatively mild reaction conditions, simpler operation, easy adjustment of the ratio of reaction raw materials, higher yield, etc., and can synthesize Cs 10 Zn4Sn4S 17 The yield is about 70-75%.

[0023] 3. The present invention also provides the use of the above zinc-based tin sulfide as an optical semiconductor. The optical band gap of the above zinc-based tin sulfide is 3.26 eV, and the photocurrent under simulated sunlight is about 0.20 μA / cm 2 , which has application prospects in semiconductor materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Cs prepared by the present invention 10 Zn4Sn4S 17 The crystal morphology of

[0025] Figure 2 Cs 10 Zn4Sn4S 17 A unit cell structure diagram of , containing four atoms: Cs, Zn, Sn, and S;

[0026] Figure 3 [Zn4Sn4S 17 ] 10- Structural diagram of anion cluster;

[0027] Figure 4 Cs prepared by the present invention 10 Zn4Sn4S 17 Simulated and experimental X-ray powder diffraction patterns of;

[0028] Figure 5 Cs prepared in the present invention 10 Zn4Sn4S 17 UV-Vis diffuse reflectance spectrum;

[0029] Figure 6 Cs prepared in the present invention 10 Zn4Sn4S 17 Photoelectric response performance diagram. DETAILED DESCRIPTION

[0030] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0031] Example 1

[0032] A method for synthesizing zinc-based tin sulfide comprises the following steps:

[0033] Weigh Zn powder (0.020 g), Sn powder (0.020 g), S powder (0.060 g), and Cs2CO3 (0.045 g) and place them in a thick-walled glass tube (volume about 10 mL) in sequence;

[0034] To a thick-walled glass tube, 1,3-propylenediamine (1.500 g) and deionized water (0.200 g) were added in sequence;

[0035] The tube was sealed on an alcohol burner. After the sealed thick-walled glass tube cooled to room temperature, it was placed in a stainless steel reactor. The reactor was sealed and placed in an oven at 160°C for reaction for 7 days before being cooled to room temperature.

[0036] The mixture in the thick-walled glass tube was repeatedly washed with anhydrous ethanol and deionized water to obtain colorless block crystals with a yield of about 75%. The morphology of the crystals is as follows Figure 1 shown.

[0037] Example 2

[0038] A method for synthesizing zinc-based tin sulfide comprises the following steps:

[0039] Weigh Zn powder (0.025 g), Sn powder (0.030 g), S powder (0.095 g), and Cs2CO3 (0.075 g) and place them in a thick-walled glass tube (volume about 10 mL) in sequence;

[0040] To a thick-walled glass tube, 1,3-propylenediamine (0.800 g) and deionized water (0.100 g) were added in sequence;

[0041] The tube was sealed on an alcohol burner. After the sealed thick-walled glass tube cooled to room temperature, it was placed in a stainless steel reactor. The reactor was sealed and placed in an oven at 180°C for reaction for 9 days before being cooled to room temperature.

[0042] The mixture in the thick-walled glass tube was repeatedly washed with anhydrous ethanol and deionized water to obtain colorless block crystals with a yield of about 70%. Figure 1 similar.

[0043] Example 3

[0044] A method for synthesizing zinc-based tin sulfide comprises the following steps:

[0045] Weigh Zn powder (0.020 g), Sn powder (0.020 g), S powder (0.060 g), and Cs2CO3 (0.045 g) and place them in a thick-walled glass tube (volume about 10 mL) in sequence;

[0046] To a thick-walled glass tube, 1,3-propylenediamine (0.800 g) and deionized water (0.100 g) were added in sequence;

[0047] The tube was sealed on an alcohol burner. After the sealed thick-walled glass tube cooled to room temperature, it was placed in a stainless steel reactor. The reactor was sealed and placed in an oven at 200°C for reaction for 7 days before being cooled to room temperature.

[0048] The mixture in the thick-walled glass tube was repeatedly washed with anhydrous ethanol and deionized water to obtain colorless block crystals with a yield of about 70%. Figure 1 similar.

[0049] Performance Testing:

[0050] (1) Single crystal X-ray diffraction

[0051] Select single crystals of appropriate size under a microscope and perform single crystal X-ray diffraction at room temperature. 10 Zn4Sn4S 17 Crystallizes in the cubic system, belonging to The space group and unit cell parameters are

[0052] α=β=γ=90°, Z=1, D c =3.816g / cm 3 The crystal structure obtained by analysis is as follows Figure 2 and Figure 3 The zinc-based tin sulfide provided by the present invention is a new type of sulfide containing two metals. In its structure, both Zn and Sn adopt a four-coordination mode to form ZnS4 tetrahedron and SnS4 tetrahedron respectively. Four pairs of ZnS4 tetrahedrons and four pairs of SnS4 tetrahedrons are connected by common vertices to form [Zn4Sn4S 17 ] 10- Anionic clusters.

[0053] (2) Powder X-ray diffraction analysis

[0054] Powder X-ray diffraction experiments were performed using a Smart-Lab 9KW diffractometer. The simulated and experimental X-ray powder diffraction patterns of the compounds are shown in Figure 4 The main diffraction peaks of the compounds obtained experimentally are consistent with the simulation results, indicating that the synthesized samples are all pure phases.

[0055] (3) UV-Vis diffuse reflectance analysis

[0056] The UV-visible diffuse reflectance spectrum was measured by Hitachi U3900 spectrometer. Figure 5 As shown, the optical band gap of the compound can be estimated to be 3.26 eV, indicating that the compound is a semiconductor.

[0057] (4) Photoelectric response performance test

[0058] The photoelectric response performance test was carried out on a CHI660E electrochemical workstation using a 500W xenon lamp equipped with an ultraviolet filter (λ = 420nm) as the light source. Figure 6 As shown, under visible light illumination, the compound immediately generates a photocurrent of about 0.20 μA / cm 2 , and shows good regeneration, indicating that it has high efficiency of photogenerated electron migration and separation efficiency of photogenerated electron-photogenerated hole pairs. These characteristics indicate that the compound is a very promising semiconductor material.

[0059] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A zinc-based tin sulfide, It is characterized in that Its chemical formula is Cs 10 Zn 4 Sn 4 S 17 , by [Zn 4 Sn 4 S 17 ] 10- Anion cluster and counter cation Cs + Composition, crystallizes in the cubic system, belongs to The space group and unit cell parameters are α=β=γ=90°, Z=1, D c =3.816g / cm 3 .

2. A method for preparing the zinc-based tin sulfide according to claim 1, It is characterized in that The following steps are involved: (1) According to the chemical formula Cs 10 Zn 4 Sn 4 S 17 The molar ratio of each element in the Zn powder, Sn powder, S powder, Cs 2 CO 3 , put them into thick-walled glass tubes in turn; (2) adding 1,3-propylenediamine and deionized water into a thick-walled glass tube in sequence; (3) sealing the tube, after the sealed thick-walled glass tube cools to room temperature, placing it in a reaction kettle, sealing the reaction kettle and placing it in an oven at 160-200° C. for reaction for 6-9 days, and then cooling it to room temperature; (4) Wash the mixture in the thick-walled glass tube to obtain colorless block crystals, namely zinc-based tin sulfide Cs 10 Zn 4 Sn 4 S 17 .

3. The method for preparing zinc-based tin sulfide according to claim 2, It is characterized in that The amount of 1,3-propylenediamine and deionized water added in step (2) is 8-30% of the volume of the glass tube.

4. The method for preparing zinc-based tin sulfide according to claim 3, It is characterized in that The amount of 1,3-propylenediamine added in step (2) is 7-8 times that of deionized water.

5. The method for preparing zinc-based tin sulfide according to claim 2, It is characterized in that In step (3), the reaction temperature is 160° C. and the reaction time is 7 days.

6. The method for preparing zinc-based tin sulfide according to claim 2, It is characterized in that In step (4), anhydrous ethanol and deionized water are used to wash the mixture.