Application of nanofluid admixture in concrete
By mixing graphene nanofluid admixture with cement and water in concrete, the problems of poor flexural and compressive strength and high cost of existing nanomaterials in concrete are solved, and the effects of strength improvement and cost reduction are achieved. , suitable for large-scale applications.
Patent Information
- Application Number
- CN202411011205.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-08
AI Technical Summary
The application of existing nanomaterials in concrete has problems such as poor flexural and compressive strength, high cost, and difficulty in scale-up.
Modified concrete is prepared by mixing graphene nanofluid admixture with cement and water, and peeling off graphene nanosheets through high-speed stirring. The nanofluid dosage is 0.41 to 0.45% to improve the mechanical properties of the concrete.
It significantly improves the flexural and compressive strength of concrete, reduces costs, and is easy to apply on a large scale.
Smart Images

Figure CN118745089A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical materials, and in particular relates to application of a nanofluid admixture in concrete. Background Art
[0002] In recent years, with the advent of graphene, the use of graphene to modify cement-based composites has become a research hotspot in the field of civil engineering cementitious materials. Most research results show that adding appropriate amounts of graphene to cement-based composites can significantly enhance their mechanical properties, durability and multifunctionality. However, the current preparation cost of graphene is relatively high, which seriously restricts its application in the engineering field. For the civil engineering industry, if the cost is high, even if the new material shows excellent performance, it is difficult to achieve large-scale preparation and can only be limited to highly specialized applications. The use of cheap and readily available raw materials and relatively simple processes to produce low-cost graphene products will be conducive to the promotion and application of graphene in cement-based composites. In this regard, continuing to study the application of a new type of nanofluid admixture containing graphene in concrete to enhance the mechanical properties, durability and multifunctionality of concrete is still one of the main themes that researchers are currently working on. Summary of the invention
[0003] The purpose of the present invention is to provide an application of a nanofluid admixture in concrete, which solves the problems of technical bottlenecks in the application of existing nanomaterials in concrete, poor flexural and compressive strength, high cost and difficulty in scale.
[0004] In order to achieve the above object, the technical solution of the present invention is achieved as follows:
[0005] The invention discloses an application of a nanofluid admixture in concrete.
[0006] In some embodiments, the nanofluid admixture, cement and water are mixed to prepare modified concrete.
[0007] In some embodiments, the mass fraction of the nanofluid admixture to cement in the modified concrete is 0.41-0.45%.
[0008] Compared with the prior art, the nanofluid admixture in the present invention can improve the flexural and compressive strength of concrete, and in addition, it has low cost and is easy to apply on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] FIG1 is a diagram of a nanofluid modified concrete mechanical strength test device according to an embodiment of the present invention; wherein:
[0010] Figure 1A Schematic diagram of flexural strength loading in mechanical strength test of nanofluid modified concrete;
[0011] Figure 1B Schematic diagram of compressive strength loading in mechanical strength test of nanofluid modified concrete;
[0012] FIG2 is a graph showing drying shrinkage of nanofluid modified concrete according to an embodiment of the present invention; wherein:
[0013] Figure 2A Constant temperature and humidity device used in the drying shrinkage test of nanofluid modified concrete;
[0014] Figure 2B Schematic diagram of drying shrinkage test of concrete with different nanofluid dosages;
[0015] FIG3 shows the flexural and compressive strength of concrete at different nanofluid dosages in an embodiment of the present invention, wherein:
[0016] Figure 3A Schematic diagram of the flexural strength of concrete with different nanofluid content;
[0017] Figure 3B Schematic diagram of the compressive strength of concrete with different nanofluid dosages.
[0018] Figure 4 1 is a comparison diagram of drying shrinkage of concrete at different nanofluid dosages in an embodiment of the present invention. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0020] The following is a method for preparing graphene nanofluid admixtures:
[0021] In the embodiment of the present invention, PVA is polyvinyl alcohol, CMC is carboxymethyl cellulose, and the graphene nanofluid admixture is GNAs.
[0022] Example 1
[0023] The graphene nanofluid admixture provided in this embodiment 1 is obtained by the following steps:
[0024] S1. Dissolve polyvinyl alcohol powder in water and heat and stir at 70°C for 12 hours to form a uniform 1 g / L polyvinyl alcohol solution;
[0025] S2. Mix the polyvinyl alcohol solution obtained in S1 with 5 g of graphite powder and place them in a blender for high-speed stirring to obtain a graphene nanofluid admixture; exfoliate the graphite by high-speed stirring, and generate shear force by means of the high-speed rotation of the blender, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder.
[0026] Example 2
[0027] The graphene nanofluid admixture provided in this embodiment 2 is obtained by the following steps:
[0028] S1. Dissolve carboxymethyl cellulose powder in water and heat and stir at 800°C for 24 hours to form a uniform 30 g / L polyvinyl alcohol solution;
[0029] S2. Mix the polyvinyl alcohol solution obtained in S1 with 5 g of graphite powder and place them in a blender for high-speed stirring to obtain a graphene nanofluid admixture; exfoliate the graphite by high-speed stirring, and generate shear force by means of the high-speed rotation of the blender, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder.
[0030] Example 3
[0031] The graphene nanofluid admixture provided in this embodiment 3 is obtained by the following steps:
[0032] S1. Dissolve hydroxyethyl cellulose in water and heat and stir at 80°C for 36 hours to form a uniform 50 g / L polyvinyl alcohol solution;
[0033] S2. Mix the polyvinyl alcohol solution obtained in S1 with 5 g of graphite powder and place them in a blender for high-speed stirring to obtain a graphene nanofluid admixture; exfoliate the graphite by high-speed stirring, and generate shear force by means of the high-speed rotation of the blender, thereby achieving effective exfoliation of graphene nanosheets from the original graphite powder.
[0034] The following is an example of applying the above graphene nanofluid admixture to concrete.
[0035] The nanofluid admixture obtained in Example 1, cement and water are mixed to prepare modified concrete, and the specific method is as follows:
[0036] The cement particles were mixed with the nanofluid prepared in Example 1 and water at a water-cement ratio of 0.41. Subsequently, the fine aggregate and the coarse aggregate were successively poured into the cement slurry and stirred to obtain a concrete specimen. The proportion of the nanofluid modified concrete is shown in Table 1, and the specific preparation process is shown in Figure 1.
[0037] Table 1 Mix ratio of each component in modified concrete (kg / m 3 )
[0038]
[0039] In order to verify the specific performance of nanofluid modified concrete with specimen numbers GC-0, GC-1, GC-2, GC-3, GC-4, and GC-5, the following tests were carried out respectively:
[0040] (1) Flexural and compressive strength test
[0041] According to the Standard for Test Methods of Mechanical Properties of Ordinary Concrete (GB / T 50081-2002), flexural tests were carried out, where the size of the flexural specimens was 100mm×100mm×400mm. The flexural strength test of the specimens was carried out after 7d and 28d of curing. After the bending test was completed, half of the specimens were selected for compression test, where the bearing area of the compression specimens was 100mm×100mm. The instruments used to test the flexural strength and compressive strength of concrete specimens are shown in Figure 1(A) and Figure 1(B), respectively.
[0042] Three parallel specimens are measured for each test, and the test results are taken as the arithmetic mean. The calculation results should be accurate to 0.01MPa. If the discreteness of a group of test data exceeds the requirements of the specification, another specimen should be prepared and its compressive strength should be re-measured.
[0043] Results: Mechanical properties are the most important factor to be considered in practical applications of cement-based composites. Most studies have found that graphene can effectively improve the compressive and flexural strength of cement composites. The enhancement mechanism is mainly attributed to the following aspects: (1) Nanofilling effect, by filling and dividing coarse pores into finer pores, the reduction of porosity is conducive to the improvement of mechanical properties; (2) The high specific surface area of graphene enhances the nucleation effect, promotes the cement hydration reaction, generates more hydration products, increases the adsorption between cement particles, and thus enhances the density of the matrix structure; (3) Graphene is evenly dispersed in the cement matrix, which can exert a bridging effect to inhibit the formation and expansion of microcracks.
[0044] Figure 3 shows the test results of the flexural and compressive strength of concrete at different nanofluid dosages. It is not difficult to find from Figure 3 that for the specimens cured for 7 days, the nanofluid has no obvious effect on the flexural and compressive strength of concrete. This may be because the PVA surfactant in the nanofluid will reduce the exothermic rate of the hydration reaction and delay cement hydration in the early stage; but with the increase of the curing age, the nanofluid-concrete specimens with a dosage of 0.08wt% under 28d curing showed the highest flexural and compressive strength, which increased by 9.95 and 5.44% respectively compared with the blank group specimens.
[0045] (2) Shrinkage test
[0046] Drying shrinkage refers to the volume deformation caused by the migration of moisture from the concrete to the external environment after the curing is completed. The drying shrinkage test refers to the "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete" (GB / T50082-2009), and the test method adopts the contact method. The instruments used to test the concrete drying shrinkage test are shown in Figure 2. Figure 2A and Figure 2B shown.
[0047] The specimen size is 100mm×100mm×515mm. The preparation and curing of the specimen are the same as those of the mechanical properties test. After demoulding, the measuring head is fixed on the sample, and then it is placed in a standard curing room for 3 days. After taking it out, it is immediately placed in a drying room with a temperature of (20±2)℃ and a relative humidity of (60±5)% or more. The micrometer is fixed on a standing bracket, and the bracket should not be affected by external vibration. After the micrometer is installed, place the sample on the bracket for the first reading. Record the corresponding shrinkage data at 1-56 days. Use formula (1) to calculate the shrinkage rate of the concrete specimen.
[0048]
[0049] Where L b Indicates the measuring gauge length of the concrete test block, L o Indicates the initial reading of the concrete specimen length, L t It indicates the length reading of the concrete specimen measured at a certain age. The test device for drying shrinkage is shown in Figure 3.
[0050] Result analysis: Figure 4 The effect of different nanofluid dosages on the drying shrinkage of concrete is shown. It can be seen that the appropriate amount of nanofluid can inhibit the drying shrinkage of concrete; when the nanofluid dosage is 0.02wt%, it has the best inhibition effect, and the inhibition rate relative to the blank group is 18.56%; but when the dosage of nanofluid continues to increase, the addition of nanofluid will increase the drying shrinkage of cement paste, even exceeding the blank group. This phenomenon may be that when the nanofluid content continues to increase (0.08wt%-0.10wt%), the agglomeration of graphene will increase the drying shrinkage rate of the internal cement paste.
[0051] In addition, on the one hand, the nucleation effect of nanofluid promotes cement hydration, increases the volume of cement paste, and thus increases shrinkage; on the other hand, nanofluid can promote the formation of a denser microstructure, prevent the expansion of microcracks, and thus reduce shrinkage. When the nanofluid content is low, the positive effect is dominant, and when the nanofluid content continues to increase, the negative effect is dominant.
[0052] In summary, by applying the graphene nanofluid described in the embodiments of the present invention to concrete, the flexural and compressive strengths of concrete can be effectively improved. In addition, the cost is low and it is easy to apply on a large scale.
[0053] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. Application of a nanofluid admixture in concrete.
2. The use according to claim 1, characterized in that: The specific method of the application is: mixing the nanofluid admixture, cement and water to prepare modified concrete.
3. The use according to claim 2, characterized in that: The mass fraction of the nanofluid admixture in the modified concrete to cement is 0.41-0.45%.
Citation Information
Patent Citations
Nano / micro-carbon material composite modified concrete and preparation method thereof
CN114853397A
Low-temperature-rise, high-impermeability and low-carbon concrete nano-fluid admixture as well as preparation method and application thereof