Through the high-temperature solid-phase reaction of cheap iron powder with strontium carbonate and calcium carbonate, combined with oxidation, mineralization and water washing, the problem of high cost and poor magnetic properties of permanent magnet ferrite pre-sintered materials in the existing technology is solved. Low-cost, high-performance permanent ferrite materials are prepared, which are suitable for motor equipment.
Patent Information
- Application Number
- CN202410846132.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-27
AI Technical Summary
Existing permanent magnet ferrite pre-sintered materials have high preparation costs and poor magnetic properties, especially when iron oxide red is used as the main material, the production cost is high, and the purity requirements for ultra-pure magnet powder are high, Si and Al elements The low content results in low residual magnetism of strontium ferrite.
Cheap iron powder is used to react with strontium carbonate and calcium carbonate through high-temperature solid-state reaction to generate hexagonal structure permanent magnet pre-sintered material. After oxidation and mineralization treatment, combined with water washing and additive fine grinding treatment, the rectangularity ratio and uniformity are improved. density, and finally obtain excellent magnetic properties through wet pressing molding and sintering.
A permanent magnet ferrite material with low raw material cost, good magnet rectangularity ratio and density is achieved. The rectangularity ratio can reach more than 0.98 and has excellent magnetic properties, which is suitable for the requirements of high-performance permanent magnet ferrite materials.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of permanent magnetic ferrite materials, and in particular to a permanent magnetic ferrite material and a preparation method and application thereof. Background Art
[0003] At present, the preparation of permanent magnet ferrite pre-sintered materials generally includes the steps of raw material mixing, granulation, molding, pre-sintering and cooling. Through the above steps, permanent magnet ferrite pre-sintered materials with a certain density and mechanical strength can be prepared. These pre-sintered materials will then be further sintered and magnetized to finally form finished permanent magnet ferrite materials for the manufacture of various permanent magnet devices and products.
[0004] Traditional permanent ferrite pre-burned materials are basically made of red iron oxide as raw material. For example, CN 112174654A discloses a method for preparing high-performance permanent ferrite magnetic powder, which comprises the following steps: (1) ball milling: mixing the main material and additives and then ball milling to obtain a mixture slurry, wherein the main material comprises 75-85% red iron oxide and 15-25% barium carbonate by mass; the additives comprise calcium carbonate, silicon dioxide and clinker pre-burned powder; (2) drying: drying the mixture slurry to obtain permanent ferrite raw material; (3) pre-burning: pre-burning the permanent ferrite raw material to obtain a pre-burned material; (4) crushing: dry-crushing the pre-burned material to obtain the high-performance permanent ferrite magnetic powder. However, using red iron oxide as the main material has a high production cost.
[0005] CN 112071615A discloses a preparation method for improving the magnetic properties of strontium ferrite pre-sintered material, comprising the following steps: (1) mixing the ingredients; (2) making balls; (3) roasting; and (4) powdering. The high-performance strontium ferrite pre-sintered material of the invention uses ultrapure magnet powder as raw material, and also adds a small amount of rare earth element holmium (Ho) and conventional additives such as strontium carbonate, calcium carbonate and silicon dioxide. After fully mixing them, green balls are prepared. The green balls are first pre-oxidized at a relatively low temperature to oxidize Fe3O4 in the raw material to Fe2O3. After the pre-oxidation is completed, roasting is performed to finally obtain the ferrite pre-sintered material. However, this method has high requirements for the purity of ultrapure magnet powder, and requires low Si and Al content, and the remanence of the strontium ferrite prepared by the method is also relatively low.
[0006] Therefore, in view of the shortcomings of the prior art, it is necessary to provide a permanent magnet ferrite material with low raw material cost, good squareness ratio and density. Summary of the invention
[0007] The purpose of the present invention is to provide a permanent magnet ferrite material and its preparation method and application, using cheap iron concentrate as raw material, generating a hexagonal permanent magnet ferrite pre-sintered material through high-temperature solid phase reaction, and further sintering with additives to obtain a permanent magnet ferrite material with excellent rectangular ratio, density and magnetic properties.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing a permanent magnet ferrite material, the preparation method comprising the following steps:
[0010] (1) wet-milling iron ore concentrate, strontium carbonate and calcium carbonate to obtain a mixed slurry;
[0011] (2) the mixed slurry obtained in step (1) is sequentially subjected to drying, oxidation, mineralization treatment and first sintering to obtain a permanent magnet ferrite pre-sintered material;
[0012] (3) The pre-sintered permanent magnet ferrite obtained in step (2) is washed with water and then finely ground with additives to obtain a fine slurry;
[0013] (4) The fine slurry obtained in step (3) is subjected to wet pressing and a second sintering in sequence to obtain the permanent magnet ferrite material.
[0014] The invention provides a method for preparing a permanent magnet ferrite material. The method directly reacts cheap iron ore with strontium carbonate and calcium carbonate through high-temperature solid-phase reaction to generate a permanent magnet ferrite pre-sintered material with a hexagonal structure. The method comprises the following steps: firstly oxidizing ferrous oxide in the iron ore concentrate, and then mineralizing the impurity silicon and calcium carbonate therein at high temperature, thereby preventing the silicon, silicon dioxide and silicate in the impurities from reacting with elemental iron to generate ferrous oxide, thereby preventing the performance of the permanent magnet ferrite from being deteriorated. The obtained permanent magnet ferrite pre-sintered material is washed with water to remove soluble silicon salts, and then introducing additives to improve the squareness ratio and density of the permanent magnet ferrite material.
[0015] Preferably, the composition of the iron ore concentrate in step (1) is TFe≥69%, FeO≥30%, and SiO2≥0.4%.
[0016] The content of TFe in the iron ore concentrate is ≥ 69%, for example, it can be 69%, 70% or 71%, but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0017] The content of FeO in the iron ore concentrate is ≥30%, for example, it can be 30%, 31% or 32%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0018] The content of SiO2 in the iron ore concentrate is ≥ 0.4%, for example, it can be 0.4%, 0.5% or 0.6%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the molar ratio of the iron ore concentrate to strontium carbonate in step (1) is (6-6.2):1, for example, 6:1, 6.1:1 or 6.2:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the molar ratio of the iron ore concentrate to calcium carbonate in step (1) is (110-118):1, for example, it can be 110:1, 112:1, 115:1, 116:1 or 118:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the wet ball milling time in step (1) is 3.5-5 h, for example, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0022] Preferably, the average particle size of the powder in the mixed slurry in step (1) is 1-1.2 μm, for example, 1 μm, 1.05 μm, 1.1 μm, 1.15 μm or 1.2 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Preferably, the drying temperature in step (2) is 90-110°C, for example, 90°C, 95°C, 100°C, 105°C or 110°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] Preferably, the oxidation temperature in step (2) is 650-700°C, for example, 650°C, 660°C, 680°C, 690°C or 700°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] Preferably, the insulation time for the oxidation in step (2) is 1.8-2.2 h, for example, 1.8 h, 1.9 h, 2 h, 2.1 h or 2.2 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0026] Preferably, the temperature of the mineralization treatment in step (2) is 990-1010°C, for example, it can be 990°C, 995°C, 1000°C, 1005°C or 1010°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the holding time of the mineralization treatment in step (2) is 0.9-1.1 h, for example, 0.9 h, 0.95 h, 1 h, 1.05 h or 1.1 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] Preferably, the temperature of the first sintering in step (2) is 1280-1320°C, for example, 1280°C, 1290°C, 1300°C, 1310°C or 1320°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0029] Preferably, the holding time of the first sintering in step (2) is 1.8-2.2 h, for example, 1.8 h, 1.9 h, 2 h, 2.1 h or 2.2 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the step (3) further includes the step of vibrating and grinding the pre-sintered permanent magnet ferrite material before the water washing.
[0031] Preferably, the average particle size of the permanent magnet ferrite pre-sintered material after the vibration grinding treatment is 4-5 μm, for example, 4 μm, 4.5 μm or 5 μm, but not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0032] Preferably, the additive in step (3) includes red iron oxide.
[0033] Preferably, the average particle size of the red iron oxide is 1.9-2.1 μm, and the Fe2O3 in the red iron oxide is ≥99.2%.
[0034] The average particle size of the red iron oxide is 1.9-2.1 μm, for example, 1.9 μm, 1.95 μm, 2 μm, 2.05 μm or 2.1 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] The Fe2O3 in the red iron oxide is ≥99.2%, for example, it can be 99.2%, 99.3% or 99.4%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] In the present invention, since the purity of the iron concentrate is low, although the content of iron oxide increases after oxidation, the purity of SrO·6Fe2O3 obtained by pre-sintering is still lower than that of the pre-sintered material prepared with red iron oxide. Therefore, high-purity red iron oxide is added in the preparation process to increase the content of iron oxide. At the same time, the particle size of the red iron oxide is finer than that of the permanent magnet ferrite pre-sintered material after vibration grinding, which is conducive to achieving the maximum uniformity of the powder.
[0037] Preferably, the mass fraction of the red iron oxide is 0.3-0.6% of the mass fraction of the permanent magnet ferrite pre-sintered material after water washing, for example, it can be 0.3%, 0.4%, 0.5% or 0.6%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0038] Preferably, the additives in step (3) also include calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid.
[0039] Preferably, the total mass fraction of the calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid is 1.3-3.1% of the mass fraction of the permanent magnet ferrite pre-sintered material after washing, for example, it can be 1.3%, 1.95%, 2.2%, 2.5% or 3.1%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0040] Among the calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid, the calcium carbonate accounts for 0.6-1.3%, the silicon dioxide accounts for 0.2-0.6%, the strontium carbonate accounts for 0.2-0.6%, the calcium gluconate accounts for 0.2-0.4% and the boric acid accounts for 0.1-0.2%.
[0041] The calcium carbonate is 0.6-1.3%, for example, 0.6%, 1%, 1.2% or 1.3%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0042] The silicon dioxide is 0.2-0.6%, for example, 0.2%, 0.4%, 0.5% or 0.6%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0043] The strontium carbonate is 0.2-0.6%, for example, 0.2%, 0.3%, 0.4%, 0.5% or 0.6%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] The calcium gluconate is 0.2-0.4%, for example, 0.2%, 0.3% or 0.4%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0045] The boric acid is 0.1-0.2%, for example, 0.1%, 0.15% or 0.2%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0046] Preferably, the average particle size of the powder in the fine slurry obtained by the fine grinding treatment in step (3) is 0.85-0.95 μm, for example, it can be 0.85 μm, 0.88 μm, 0.9 μm, 0.92 μm or 0.95 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0047] Preferably, the wet pressing in step (4) is carried out in a press with a molding magnetic field of 6000 Gs.
[0048] Preferably, the temperature of the second sintering in step (4) is 1240-1260°C, for example, 1240°C, 1245°C, 1250°C, 1255°C or 1260°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] Preferably, the second sintering time in step (4) is 1-2 h, for example, 1 h, 1.2 h, 1.5 h, 1.8 h or 2 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0050] Preferably, as a preferred technical solution of the preparation method described in the present invention, the preparation method comprises the following steps:
[0051] (1) wet-milling iron ore concentrate, strontium carbonate and calcium carbonate for 3.5-5 hours to obtain a mixed slurry with an average particle size of 1-1.2 μm; the iron ore concentrate comprises TFe ≥ 69%, FeO ≥ 30%, and SiO2 ≥ 0.4%; the molar ratio of the iron ore concentrate to strontium carbonate is (6-6.2):1; the molar ratio of the iron ore concentrate to calcium carbonate is (110-118):1;
[0052] (2) The mixed slurry obtained in step (1) is sequentially dried at 90-110° C., oxidized at 650-700° C. for 1.8-2.2 h, mineralized at 990-1010° C. for 0.9-1.1 h, and first sintered at 1280-1320° C. for 1.8-2.2 h to obtain a permanent magnet ferrite pre-sintered material;
[0053] (3) vibrating and grinding the pre-sintered permanent magnet ferrite obtained in step (2) to an average particle size of 4-5 μm, washing with water, and then finely grinding with additives to obtain a fine slurry with an average particle size of 0.85-0.95 μm;
[0054] The additive includes red iron oxide; the average particle size of the red iron oxide is 1.9-2.1 μm, and the Fe2O3 in the red iron oxide is ≥99.2%; the mass fraction of the red iron oxide is 0.3-0.6% of the mass fraction of the permanent magnet ferrite pre-sintered material after washing; the additive also includes calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid; the total mass fraction of the calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid is 1.3-3.1% of the mass fraction of the permanent magnet ferrite pre-sintered material after washing;
[0055] (4) The fine slurry obtained in step (3) is wet pressed in a press with a forming magnetic field of 6000 Gs, and a second sintering is performed at 1240-1260° C. for 1-2 hours to obtain the permanent magnet ferrite material.
[0056] In a second aspect, the present invention provides a permanent magnet ferrite material, which is prepared by the preparation method described in the first aspect.
[0057] The permanent magnet ferrite material provided by the present invention has low raw material cost, good magnet rectangular ratio and density, the rectangular ratio can reach above 0.98, excellent magnetic properties, and can meet the requirements of being a high-performance permanent magnet ferrite material.
[0058] In a third aspect, the present invention provides an application of the permanent magnet ferrite material as described in the second aspect, wherein the permanent magnet ferrite material is used in motor equipment.
[0059] Compared with the prior art, the present invention has the following beneficial effects:
[0060] (1) The preparation method of the permanent magnet ferrite material provided by the present invention directly reacts cheap iron ore with strontium carbonate and calcium carbonate through high-temperature solid-phase reaction to generate a permanent magnet ferrite pre-sintered material with a hexagonal structure, wherein the ferrous oxide in the iron ore concentrate is first oxidized, and then the impurity silicon and calcium carbonate therein are subjected to a mineralization reaction at high temperature, thereby preventing the silicon, silicon dioxide and silicate in the impurities from reacting with elemental iron to generate ferrous oxide and thus deteriorating the performance of the permanent magnet ferrite; the obtained permanent magnet ferrite pre-sintered material is washed with water to remove soluble silicon salts, and then additives are introduced to improve the rectangular ratio and density of the permanent magnet ferrite material;
[0061] (2) The permanent magnet ferrite material provided by the present invention has low raw material cost, good magnet rectangular ratio and density, the rectangular ratio can reach 0.983, excellent magnetic properties, and can be used in motor equipment. DETAILED DESCRIPTION
[0062] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0063] Example 1
[0064] This embodiment provides a permanent magnet ferrite material, and the preparation method of the permanent magnet ferrite material comprises the following steps:
[0065] (1) wet-milling iron ore concentrate, strontium carbonate and calcium carbonate for 4.5 hours to obtain a mixed slurry with an average powder particle size of 1.1 μm; the iron ore concentrate comprises 69% TFe, 30% FeO and 0.5% SiO2; the molar ratio of the iron ore concentrate to strontium carbonate is 6.1:1; and the molar ratio of the iron ore concentrate to calcium carbonate is 115:1;
[0066] (2) The mixed slurry obtained in step (1) is sequentially dried at 100° C., oxidized at 680° C. for 2 h, mineralized at 1000° C. for 1 h, and first sintered at 1300° C. for 2 h to obtain a permanent magnet ferrite pre-sintered material;
[0067] (3) the pre-sintered permanent magnet ferrite obtained in step (2) is subjected to vibration grinding to an average particle size of 4.5 μm, washed with water, and then finely ground with red iron oxide, calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid to obtain a fine slurry with an average particle size of 0.9 μm;
[0068] The average particle size of the red iron oxide is 2 μm, and the content of Fe2O3 in the red iron oxide is 99.5%; the mass fraction of the red iron oxide is 0.4% of the mass fraction of the permanent magnet ferrite pre-sintered material after washing; the total mass fraction of the calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid is 2.2% of the mass fraction of the permanent magnet ferrite pre-sintered material after washing; based on the total mass percentage as 100wt%, the calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid are 1wt% of calcium carbonate, 0.5wt% of silicon dioxide, 0.3wt% of strontium carbonate, 0.2wt% of calcium gluconate and 0.2wt% of boric acid;
[0069] (4) The fine slurry obtained in step (3) is wet pressed in a press with a forming magnetic field of 6000 Gs, and a second sintering is performed at 1250° C. for 1.5 hours to obtain the permanent magnet ferrite material.
[0070] Example 2
[0071] This embodiment provides a permanent magnet ferrite material, and the preparation method of the permanent magnet ferrite material comprises the following steps:
[0072] (1) wet-milling iron ore concentrate, strontium carbonate and calcium carbonate for 3.5 hours to obtain a mixed slurry with an average particle size of 1.2 μm; the iron ore concentrate comprises 69% TFe, 30% FeO and 0.5% SiO2; the molar ratio of the iron ore concentrate to strontium carbonate is 6.2:1; and the molar ratio of the iron ore concentrate to calcium carbonate is 118:1;
[0073] (2) The mixed slurry obtained in step (1) is sequentially dried at 90° C., oxidized at 650° C. for 2.2 h, mineralized at 990° C. for 1.1 h, and first sintered at 1280° C. for 2.2 h to obtain a permanent magnet ferrite pre-sintered material;
[0074] (3) The pre-sintered permanent magnet ferrite obtained in step (2) is subjected to vibration grinding to an average particle size of 5 μm, washed with water, and then finely ground with red iron oxide, calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid to obtain a fine slurry with an average particle size of 0.95 μm;
[0075] The average particle size of the red iron oxide is 2.1 μm, and the content of Fe2O3 in the red iron oxide is 99.2%; the mass fraction of the red iron oxide is 0.3% of the mass fraction of the permanent magnet ferrite pre-sintered material after washing; the total mass fraction of the calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid is 2.5% of the mass fraction of the permanent magnet ferrite pre-sintered material after washing; based on the total mass percentage as 100wt%, among the calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid, calcium carbonate is 1.2wt%, silicon dioxide is 0.4wt%, strontium carbonate is 0.4wt%, calcium gluconate is 0.4wt%, and boric acid is 0.1wt%;
[0076] (4) The fine slurry obtained in step (3) is wet pressed in a press with a forming magnetic field of 6000 Gs, and a second sintering is performed at 1240° C. for 2 hours to obtain the permanent magnet ferrite material.
[0077] Example 3
[0078] This embodiment provides a permanent magnet ferrite material, and the preparation method of the permanent magnet ferrite material comprises the following steps:
[0079] (1) wet-milling iron ore concentrate, strontium carbonate and calcium carbonate for 5 hours to obtain a mixed slurry with an average particle size of 1 μm; the iron ore concentrate comprises 69% TFe, 30% FeO and 0.5% SiO2; the molar ratio of the iron ore concentrate to strontium carbonate is 6:1; the molar ratio of the iron ore concentrate to calcium carbonate is 110:1;
[0080] (2) The mixed slurry obtained in step (1) is sequentially dried at 110° C., oxidized at 700° C. for 1.8 h, mineralized at 1010° C. for 0.9 h, and first sintered at 1320° C. for 1.8 h to obtain a permanent magnet ferrite pre-sintered material;
[0081] (3) the pre-sintered permanent magnet ferrite obtained in step (2) is subjected to vibration grinding to an average particle size of 4 μm, washed with water, and then finely ground with red iron oxide, calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid to obtain a fine slurry with an average particle size of 0.85 μm;
[0082] The average particle size of the red iron oxide is 1.9 μm, and the content of Fe2O3 in the red iron oxide is 99.3%; the mass fraction of the red iron oxide is 0.6% of the mass fraction of the permanent magnet ferrite pre-sintered material after washing; the total mass fraction of the calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid is 1.95% of the mass fraction of the permanent magnet ferrite pre-sintered material after washing; based on the total mass percentage as 100wt%, the calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid, are 0.6wt% for calcium carbonate, 0.4wt% for silicon dioxide, 0.5wt% for strontium carbonate, 0.3wt% for calcium gluconate and 0.15wt% for boric acid;
[0083] (4) The fine slurry obtained in step (3) is wet pressed in a press with a forming magnetic field of 6000 Gs, and a second sintering is performed at 1260° C. for 1 hour to obtain the permanent magnet ferrite material.
[0084] Example 4
[0085] This embodiment provides a permanent magnet ferrite material, which is different from Embodiment 1 in that, except that the molar ratio of the iron ore concentrate to calcium carbonate in step (1) is adjusted to 120:1, the rest is the same as Embodiment 1.
[0086] Example 5
[0087] This embodiment provides a permanent magnet ferrite material, which is different from Embodiment 1 in that, except that the molar ratio of the iron ore concentrate to calcium carbonate in step (1) is adjusted to 108:1, the rest is the same as Embodiment 1.
[0088] Example 6
[0089] This embodiment provides a permanent magnet ferrite material, which is different from the embodiment 1 in that, except that the oxidation temperature in step (2) is adjusted to 600° C., the rest is the same as the embodiment 1.
[0090] Example 7
[0091] This embodiment provides a permanent magnet ferrite material, which is different from the embodiment 1 in that, except that the oxidation temperature in step (2) is adjusted to 750° C., the rest is the same as the embodiment 1.
[0092] Example 8
[0093] This embodiment provides a permanent magnet ferrite material, which is different from Embodiment 1 in that, except that the temperature of the mineralization treatment in step (2) is adjusted to 950° C., the rest is the same as Embodiment 1.
[0094] Example 9
[0095] This embodiment provides a permanent magnet ferrite material, which is different from Embodiment 1 in that, except for adjusting the temperature of the mineralization treatment in step (2) to 1050° C., the rest is the same as Embodiment 1.
[0096] Comparative Example 1
[0097] This comparative example provides a permanent magnet ferrite material, which differs from Example 1 in that calcium carbonate is not introduced in step (1), and the rest is the same as Example 1.
[0098] Comparative Example 2
[0099] This comparative example provides a permanent magnet ferrite material, which differs from Example 1 in that step (2) does not include an oxidation step, and the rest is the same as Example 1.
[0100] Comparative Example 3
[0101] This comparative example provides a permanent magnet ferrite material, which differs from Example 1 in that no additive is introduced in step (3), and the rest is the same as Example 1.
[0102] The permanent ferrite materials provided in Examples 1-9 and Comparative Examples 1-3 were subjected to magnetic performance tests using a TYU-2000H magnetic material automatic measuring device. The results are shown in Table 1.
[0103] Table 1
[0104]
[0105]
[0106] It can be seen from Table 1 that the permanent magnet ferrite material prepared by the preparation method provided by the present invention has excellent magnetic performance and good rectangular shape, and can meet the requirements of being a high-performance permanent magnet ferrite;
[0107] By comparing Example 1 with Examples 4 and 5, it can be seen that the molar ratio of iron ore concentrate to calcium carbonate exceeds the specified range, which will result in calcium ions failing to fully replace strontium ions, causing the magnet grains to coarsen, generating abnormal grains, and reducing the coercive force; by comparing Example 1 with Examples 6 and 7, it can be seen that the oxidation temperature is too low, the oxidation of ferrous oxide cannot be completely achieved, and the magnetic properties of the obtained permanent magnet ferrite material are reduced; if the temperature is too high, it will lead to insufficient oxidation, the appearance of ferrous phase, and the reduction of the Ms of the magnet, resulting in lower magnetic properties; by comparing Example 1 with Examples 8 and 9, it can be seen that the temperature of the mineralization treatment is too low, the impurity silicon in the iron ore concentrate cannot be completely mineralized with calcium carbonate, and the temperature of the mineralization treatment is too high, which will lead to the generation of non-magnetic phases and reduce the remanence;
[0108] By comparing Example 1 with Comparative Example 1, it can be seen that without adding calcium carbonate, the impurity silicon in the iron ore concentrate cannot be removed, which leads to the reaction of the impurity silicon with elemental iron to generate ferrous oxide, thereby deteriorating the performance of the permanent magnet ferrite material; by comparing Example 1 with Comparative Example 2, it can be seen that without oxidation treatment, the oxidation of ferrous oxide cannot be completely achieved, and the performance of the permanent magnet ferrite material obtained is significantly reduced; by comparing Example 1 with Comparative Example 3, it can be seen that without introducing additives, the purity of SrO·6Fe2O3 obtained by pre-calcination is low, and the magnetic properties of the permanent magnet ferrite material are reduced.
[0109] In summary, the preparation method of the permanent magnet ferrite material provided by the present invention directly reacts cheap iron ore with strontium carbonate and calcium carbonate through high-temperature solid-phase reaction to generate a permanent magnet ferrite pre-sintered material with a hexagonal structure, wherein the ferrous oxide in the iron ore concentrate is firstly oxidized, and then the impurity silicon and calcium carbonate therein are subjected to a mineralization reaction at high temperature, thereby preventing the silicon, silicon dioxide and silicate in the impurities from reacting with elemental iron to generate ferrous oxide and thus deteriorating the performance of the permanent magnet ferrite; the obtained permanent magnet ferrite pre-sintered material is washed with water to remove soluble silicon salts, and then additives are introduced to improve the rectangular ratio, density and magnetic properties of the permanent magnet ferrite material;
[0110] The permanent magnet ferrite material provided by the present invention has low raw material cost, good magnet rectangular ratio and density, the rectangular ratio can reach 0.983, excellent magnetic properties, and can be used in motor equipment.
[0111] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a permanent magnetic ferrite material, characterized in that: The preparation method comprises the following steps: (1) wet-milling iron ore concentrate, strontium carbonate and calcium carbonate to obtain a mixed slurry; (2) The mixed slurry obtained in step (1) is sequentially subjected to drying, oxidation, mineralization treatment and a first sintering to obtain a permanent magnet ferrite pre-sintered material; (3) The pre-sintered permanent magnet ferrite obtained in step (2) is washed with water and then finely ground with additives to obtain a fine slurry; (4) The fine slurry obtained in step (3) is sequentially subjected to wet pressing and a second sintering to obtain the permanent magnet ferrite material.
2. The preparation method according to claim 1, characterized in that: The iron ore concentrate of step (1) comprises TFe ≥ 69%, FeO ≥ 30%, and SiO2 ≥ 0.4%; Preferably, the molar ratio of the iron ore concentrate to strontium carbonate in step (1) is (6-6.2):1; Preferably, the molar ratio of the iron ore concentrate to calcium carbonate in step (1) is (110-118):1; Preferably, the wet ball milling time in step (1) is 3.5-5h; Preferably, the average particle size of the powder in the mixed slurry in step (1) is 1-1.2 μm.
3. The preparation method according to claim 1 or 2, characterized in that: The drying temperature in step (2) is 90-110° C. Preferably, the oxidation temperature in step (2) is 650-700°C; Preferably, the insulation time of the oxidation in step (2) is 1.8-2.2h.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The temperature of the mineralization treatment in step (2) is 990-1010°C; Preferably, the holding time of the mineralization treatment in step (2) is 0.9-1.1h; Preferably, the temperature of the first sintering in step (2) is 1280-1320°C; Preferably, the holding time of the first sintering in step (2) is 1.8-2.2 h.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The step (3) also includes the step of vibrating and grinding the pre-sintered permanent magnet ferrite material before the water washing; Preferably, the vibration grinding process is performed until the average particle size of the permanent magnet ferrite pre-sintered material is 4-5 μm.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The additive in step (3) includes red iron oxide; Preferably, the average particle size of the red iron oxide is 1.9-2.1 μm, and the Fe2O3 in the red iron oxide is ≥ 99.2%; Preferably, the mass fraction of the red iron oxide is 0.3-0.6% of the mass fraction of the permanent magnet ferrite pre-sintered material after water washing; Preferably, the additives in step (3) further include calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid; Preferably, the fine grinding treatment in step (3) is performed to obtain a fine slurry with an average particle size of 0.85-0.95 μm.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The wet pressing in step (4) is carried out in a press with a forming magnetic field of 6000 Gs; Preferably, the temperature of the second sintering in step (4) is 1240-1260° C.; Preferably, the second sintering time in step (4) is 1-2 hours.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) wet-milling iron ore concentrate, strontium carbonate and calcium carbonate for 3.5-5 hours to obtain a mixed slurry with an average particle size of 1-1.2 μm; the iron ore concentrate comprises TFe ≥ 69%, FeO ≥ 30%, and SiO2 ≥ 0.4%; the molar ratio of the iron ore concentrate to strontium carbonate is (6-6.2):1; the molar ratio of the iron ore concentrate to calcium carbonate is (110-118):1; (2) The mixed slurry obtained in step (1) is sequentially dried at 90-110° C., oxidized at 650-700° C. for 1.8-2.2 h, mineralized at 990-1010° C. for 0.9-1.1 h, and first sintered at 1280-1320° C. for 1.8-2.2 h to obtain a permanent magnet ferrite pre-sintered material; (3) vibrating and grinding the pre-sintered permanent magnet ferrite obtained in step (2) to an average particle size of 4-5 μm, washing with water, and then finely grinding with additives to obtain a fine slurry with an average particle size of 0.85-0.95 μm; The additive includes red iron oxide; the average particle size of the red iron oxide is 1.9-2.1 μm, and the Fe2O3 in the red iron oxide is ≥99.2%; the mass fraction of the red iron oxide is 0.3-0.6% of the mass fraction of the permanent magnet ferrite pre-sintered material after water washing; the additive also includes calcium carbonate, silicon dioxide, strontium carbonate, calcium gluconate and boric acid; (4) The fine slurry obtained in step (3) is wet pressed in a press with a forming magnetic field of 6000 Gs, and a second sintering is performed at 1240-1260° C. for 1-2 hours to obtain the permanent magnet ferrite material.
9. A permanent magnet ferrite material, characterized in that: The permanent magnetic ferrite material is prepared by the preparation method according to any one of claims 1 to 8.
10. An application of the permanent magnetic ferrite material as claimed in claim 9, characterized in that: The permanent ferrite material is used in electrical machinery equipment.
Citation Information
Patent Citations
Preparation method for non-rare-earth high-remanent-magnetism permanent-magnetism ferrite
CN104609843A
Method for producing ferrite pre-sintering material through steelmaking dry dedusting fine ash
CN104987055A
Preparation method of permanent-magnet ferrite material
CN107293398A
Preparation method of high-performance La-Co system strontium permanent magnetic ferrite material