Method for starting up cathode plate with zinc in zinc electrodeposition process
By adjusting the maintenance and starting steps of wet zinc smelting, the problems of cathode zinc adhesive plate and acid permeability are solved, ensuring the normal operation and production efficiency of the automatic zinc stripper.
Patent Information
- Application Number
- CN202411151387.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
During wet zinc smelting, artificial zinc stripping can easily lead to cathode zinc sticking and acid permeability, affecting production efficiency and product quality. Automatic zinc stripping machine has high requirements for cathode plate thickness and adhesiveness, and when there is insufficient processing personnel Difficult to deal with it in time, resulting in lag in production progress.
By adjusting the maintenance and starting steps, it includes separating and stacking thin cathode plates before shutdown, canceling the addition of tartar, increasing the current strength, and real-time patrol and adjusting the current strength during the startup process, controlling the electrolyte index and tank temperature. Ensure the correct installation of the cathode plate and the circulation state of the electrolyte.
It effectively reduces the risk of cathode zinc adhesive plate and acid permeability, ensures the normal operation of the automatic zinc stripper production line, and improves production efficiency and product quality.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of zinc electrowinning process production, and in particular relates to a method for starting a zinc-bearing cathode plate in a zinc electrowinning process. Background Art
[0002] The hydrometallurgical zinc industry uses an insoluble lead-silver alloy plate as the anode and a pure aluminum plate as the cathode. Under the action of direct current, the zinc ions in the electrolyte are adsorbed on the cathode plate. After a 24-hour or 48-hour precipitation cycle, the zinc skin on the cathode plate is peeled off to obtain the intermediate product cathode zinc. The cathode zinc is melted in an induction furnace to obtain a high-purity zinc ingot product.
[0003] Most of the zinc stripping methods for electrolytic zinc smelting enterprises are manual zinc stripping, and some enterprises use automatic zinc stripping machines for mechanical zinc stripping. After technical transformation, our factory has increased the effective zinc deposition area of cathode zinc in the electrolytic workshop from the original 1.13m2 to 1.32m2. The electrolytic production capacity has been expanded by increasing the effective zinc deposition area of the plate, but it still belongs to the production scope of small plates and has always used manual zinc stripping. During the "three transformations" transformation process, two sets of automatic zinc stripping machine production lines were introduced to replace manual zinc stripping.
[0004] The maintenance and startup method when the workshop adopts manual zinc stripping is as follows: ① Strip the cathode zinc remaining on the cathode plate, level and brush the cathode plate. ② Replenish the electrolyte, circulate it in a large cycle, and fully mix the electrolyte. ③ Add strontium carbonate to participate in the circulation 8 hours before starting the machine, and stop the electrolyte circulation when the cathode plate is about to be installed. ④ Add tartar emetic to each electrolytic cell. After the addition is completed, the electrolyte circulates for 5-6 minutes. ⑤ After the electrolyte stops circulating, load the cathode plates (24 or 48 sheets) according to the planned production current intensity. After the loading is completed, contact the main DC power supply. ⑥ When the current density rises to 100A / m2, start the electrolyte circulation again and continue to increase the current intensity to the planned current intensity.
[0005] Because the electrolyte contains high zinc, low acid and high impurities when the machine is started, it is easy to cause cathode zinc precipitation, acid permeation and plate sticking in actual production, but it has little effect on manual zinc stripping.
[0006] After our factory put into use the automatic zinc stripping machine production line, the number of zinc stripping operators decreased. Once a large-scale cathode zinc sticking to the plate and acid penetration occurs, the lack of on-site handling personnel will inevitably cause the production progress of the day to lag behind, and continuously affect the production output in the following days. At the same time, the automatic zinc stripping machine has high requirements for the thickness and adhesion of the cathode plate. It must ensure the thickness of the cathode zinc and ensure that the cathode zinc and the cathode plate do not stick to the plate. According to the previous maintenance and startup of the electrolytic deposition process in our factory, the electrolytic deposition maintenance and startup method of the automatic zinc stripping machine production line is innovated to avoid the occurrence of acid penetration and sticking of the cathode plate during maintenance and startup. Summary of the invention
[0007] The technical problem to be solved by the present invention is to address the problem raised in the background technology.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is:
[0009] A method for starting up a zinc electrodeposition process cathode plate with zinc, comprising the following specific steps:
[0010] S1. On the day of the planned maintenance shutdown, the loading tank operation of the 3rd and 4th columns shall be completed in the morning. After the loading tank operation is completed, there shall be an interval of more than 1 hour. After the DC power is shut down in the afternoon, the personnel shall be organized to pull out the heavy cathode plates of the 1st and 2nd columns and the thinner cathode plates of the 3rd and 4th columns from the electrolytic cells and stack them separately. During the maintenance period, the personnel shall be organized to strip the zinc of the heavy cathode plates of the 1st and 2nd columns and to level and brush the cathode plates;
[0011] S2. Before starting up, the electrolyte shall be replenished, circulated, and strontium carbonate shall be added according to the conventional method. The various element indicators of the electrolyte after replenishment shall meet the standards. When preparing the cathode plates, the cathode plates with cathode zinc films in columns 3 and 4 shall be evenly distributed to 4 columns for preparation;
[0012] S3. Cancel the step of adding tartar emetic, and after the electrolyte circulation stops, start installing the cathode plate;
[0013] S4. After the plate installation is completed, contact the main reduction to increase the current intensity to 3KA, and check the conductivity of the cathode plate in the installed slot. Then notify the main reduction to increase the current intensity to 15KA within 1 hour, and do the following: first, inspect the cathode zinc precipitation on the slot surface at any time within 4 hours of startup, and adjust the current intensity in time if re-dissolution occurs; second, control the low liquid level operation of the circulating pool electrolyte.
[0014] The stacking condition in step S1 is that the bottom of the thinner cathode plates should be off the ground when stacked to prevent the ground acid from dissolving the precipitated cathode zinc.
[0015] The element indicators in step S2 are: zinc content ≤ 80 g / L, acid content ≥ 130 g / L, copper content ≤ 0.2 mg / L, antimony content ≤ 0.01 mg / L, and cobalt content ≤ 0.2 mg / L.
[0016] The standard for installing cathode plates in step S3 is 24 plates per slot, and two adjacent cathode plates are installed with an interval.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] This method is used during the startup process to reduce the risk of cathode zinc sticking to the plate and acid penetration when the electrolytic process is started up for maintenance, ensuring the normal operation of the automatic zinc stripping machine production line. DETAILED DESCRIPTION
[0019] The present invention will be described in detail below in conjunction with specific embodiments. The exemplary embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0020] Example 1
[0021] The method for starting up a cathode plate with zinc in a zinc electrowinning process of the present invention comprises the following specific steps:
[0022] S1. On the day of the planned maintenance shutdown, the loading tank operation of the 3rd and 4th columns shall be completed in the morning. After the loading tank operation is completed, there shall be an interval of more than 1 hour. After the DC power is shut down in the afternoon, the personnel shall be organized to pull out the heavy cathode plates of the 1st and 2nd columns and the thinner cathode plates of the 3rd and 4th columns from the electrolytic cells and stack them separately. During the maintenance period, the personnel shall be organized to strip the zinc of the heavy cathode plates of the 1st and 2nd columns and to level and brush the cathode plates;
[0023] S2. Before starting up, the electrolyte shall be replenished, circulated, and strontium carbonate shall be added according to the conventional method. The various element indicators of the electrolyte after replenishment shall meet the standards. When preparing the cathode plates, the cathode plates with cathode zinc films in columns 3 and 4 shall be evenly distributed to 4 columns for preparation;
[0024] S3. Cancel the step of adding tartar emetic, and after the electrolyte circulation stops, start installing the cathode plate;
[0025] S4. After the plate is installed, contact the main reduction to increase the current intensity to 3KA, and check the conductivity of the cathode plate in the slot. Then notify the main reduction to increase the current intensity to 15KA within 1 hour. In addition, first, inspect the cathode zinc precipitation on the slot surface at any time within 4 hours of starting the machine, and adjust the current intensity in time if there is a re-dissolution phenomenon. Second, control the low liquid level of the circulating pool electrolyte to reduce the acid content of the electrolyte to about 55g / L as soon as possible; third, control the slot temperature at 35℃ for production.
[0026] The stacking condition in step S1 is that the bottom of the thinner cathode plates should be off the ground when stacked to prevent the ground acid from dissolving the precipitated cathode zinc.
[0027] The element indicators in step S2 are: zinc content ≤ 80 g / L, acid content ≥ 130 g / L, copper content ≤ 0.2 mg / L, antimony content ≤ 0.01 mg / L, and cobalt content ≤ 0.2 mg / L.
[0028] The standard for installing cathode plates in step S3 is 24 plates per slot, and two adjacent cathode plates are installed with an interval.
[0029] This method is used during the startup process to reduce the risk of cathode zinc sticking to the plate and acid penetration when the electrolytic process is started up for maintenance, ensuring the normal operation of the automatic zinc stripping machine production line.
[0030] The technical solutions provided by the embodiments of the present invention are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the embodiments of the present invention. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present invention.
Claims
1. A method for starting up a cathode plate strip zinc in a zinc electrowinning process, characterized in that: The specific steps include: S1. On the day of the planned maintenance shutdown, the loading tank operation of the 3rd and 4th columns shall be completed in the morning. After the loading tank operation is completed, there shall be an interval of more than 1 hour. After the DC power is shut down in the afternoon, the personnel shall be organized to pull out the heavy cathode plates of the 1st and 2nd columns and the thinner cathode plates of the 3rd and 4th columns from the electrolytic cells and stack them separately. During the maintenance period, the personnel shall be organized to strip the zinc of the heavy cathode plates of the 1st and 2nd columns and to level and brush the cathode plates; S2. Before starting up, the electrolyte shall be replenished, circulated, and strontium carbonate shall be added according to the conventional method. The various element indicators of the electrolyte after replenishment shall meet the standards. When preparing the cathode plates, the cathode plates with cathode zinc films in columns 3 and 4 shall be evenly distributed to 4 columns for preparation; S3. Cancel the step of adding tartar emetic, and after the electrolyte circulation stops, start installing the cathode plate; S4. After the plate installation is completed, contact the main reduction to increase the current intensity to 3KA, and check the conductivity of the cathode plate in the installed slot. Then notify the main reduction to increase the current intensity to 15KA within 1 hour, and do the following: first, inspect the cathode zinc precipitation on the slot surface at any time within 4 hours of startup, and adjust the current intensity in time if re-dissolution occurs; second, control the low liquid level operation of the circulating pool electrolyte.
2. A method for starting up a cathode plate strip zinc in a zinc electrodeposition process according to claim 1, characterized in that: The stacking condition in step S1 is that the bottom of the thinner cathode plates should be off the ground when stacked to prevent the ground acid from dissolving the precipitated cathode zinc.
3. A method for starting up a cathode plate with zinc in a zinc electrodeposition process according to claim 2, characterized in that: The element indicators in step S2 are: zinc content ≤ 80 g / L, acid content ≥ 130 g / L, copper content ≤ 0.2 mg / L, antimony content ≤ 0.01 mg / L, and cobalt content ≤ 0.2 mg / L.
4. A method for starting up a cathode plate strip zinc in a zinc electrodeposition process according to claim 3, characterized in that: The standard for installing cathode plates in step S3 is 24 plates per slot, and two adjacent cathode plates are installed with an interval.