Method for preparing lambda-Ti3O5 functional material

By using laser heating and specific metal oxide stabilizers in a low oxygen partial pressure environment, λ-Ti3O5 is directly prepared, which solves the problem of difficulty in obtaining a stable phase of λ-Ti3O5 at room temperature in the existing technology, simplifies the process and improves improve preparation efficiency.

CN118745113AActive Publication Date: 2024-10-08SHANGHAI UNIV

Patent Information

Application Number
CN202410753752.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-08
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

It is difficult to easily obtain the stable phase of λ-Ti3O5 at room temperature with the existing technology, and it often requires the introduction of reducing agents and complicated preparation processes.

Method used

By adding specific metal oxides as stabilizers and using lasers as heat sources to directly prepare λ-Ti3O5 in a low oxygen partial pressure environment, the use of reducing agents and complex preparation processes are avoided.

Benefits of technology

It is possible to directly obtain the stable phase of λ-Ti3O5 at room temperature, simplifying the preparation process and improving preparation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745113A_ABST
    Figure CN118745113A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a lambda-Ti3O5 functional material, which comprises the following steps: (1) taking TiO2 powder and oxide of metal M as raw materials, metering the ratio of the raw materials according to the molar ratio of metal element atom M / Ti of x: (3-x), and x is more than or equal to 0.09 and less than or equal to 0.40; (2) fully grinding the raw materials metered in the step (1) to obtain mixed powder, and carrying out compression molding on the mixed powder in a mold to obtain a molded block; (3) in the atmosphere of inert gas, laser heating reaction is carried out on the formed block obtained in the step (2) at the high laser power density, the temperature of the laser heating reaction ranges from 1800 DEG C to 2300 DEG C, and a sintered block A is obtained; (4) slowly reducing the laser power density and enabling the laser to continuously act on the sintered block A obtained in the step (3) to obtain a sintered block B; and (5) after the sintered block B is naturally cooled, the lambda-Ti3O5 functional material is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional materials, and in particular relates to a method for preparing λ-Ti3O5 functional material. Technical Background

[0002] Ti3O5 is a type of titanium suboxide with multiple crystal forms. At room temperature, Ti3O5 exists stably in the β phase, while λ-Ti3O5 is a high-temperature metastable phase. Due to its structural and property characteristics, λ-Ti3O5 has broad application prospects in many fields and is a highly promising functional material. For example, due to the wide-spectrum solar absorption and high light absorption rate of λ-Ti3O5, it is considered to be a potential photothermal material that can be used in the field of seawater desalination. In addition, the reversible phase change process between λ-Ti3O5 and β-Ti3O5 under the induction of external temperature and pressure also makes it a phase change heat storage material for waste heat recovery. However, the λ phase of Ti3O5 is a high-temperature metastable phase and is difficult to obtain at room temperature. At present, the method of obtaining a room temperature stable λ phase is to prepare it into nanoparticles. For example, Chinese patent CN 104973622 B first obtains TiO2 nanoparticles by raw material pretreatment, and then obtains λ-Ti3O5 by carbon reduction; Chinese patent CN 111003727 A directly uses commercial nano-TiO2 as raw material to prepare λ-Ti3O5 by hydrogen reduction. Chinese patent CN 116375079 A uses laser as a heat source and proposes a method for directly preparing Ti3O5 without a reducing agent under a low oxygen partial pressure environment, but only the β phase can be obtained and the λ phase cannot be obtained. Therefore, the methods currently used all require the introduction of a reducing agent. Not only is the preparation process complicated and the conditions are harsh, but it is also necessary to control the reaction temperature, time and amount of reducing agent, etc., making it difficult to easily obtain λ-Ti3O5 at room temperature. Summary of the invention

[0003] In response to the above problems, this patent proposes a method of adding specific metal oxides as stabilizers and using laser as a heat source to directly prepare λ-Ti3O5 functional materials under reducing agent-free conditions.

[0004] The technical solution adopted by the present invention is as follows:

[0005] In a first aspect, the present invention provides a method for preparing a λ-Ti3O5 functional material, comprising the following steps:

[0006] (1) The raw materials are TiO2 powder and oxide of metal M, and the raw material ratios are measured according to the metal element atomic M / Ti molar ratio of x:(3-x), where 0.09≤x≤0.40;

[0007] (2) fully grinding the raw materials measured in step (1) to obtain a mixed powder, and pressing the mixed powder into a mold to obtain a molded block;

[0008] (3) after adjusting the oxygen partial pressure in the cavity, subjecting the formed block obtained in step (2) to a laser heating reaction at a high laser power density, wherein the temperature of the laser heating reaction is 1800 to 2300° C., to obtain a sintered block A;

[0009] (4) then slowly reducing the laser power density and allowing the laser to continue acting on the sintered block A obtained in step (3) to obtain a sintered block B;

[0010] (5) After the sintered block B is naturally cooled, the λ-Ti3O5 functional material is obtained;

[0011] Optionally, in step (3), the oxygen partial pressure is lower than 10 -3 Pa.

[0012] Optionally, in step (3), the laser heating reaction time is 1 to 10 minutes, preferably 2 to 8 minutes;

[0013] Optionally, in step (3), the high laser power density is 1.0 to 10.0 kW / cm 2 , preferably 3.0~8.0kW / cm 2 .

[0014] Optionally, in step (4), the rate of slowly reducing the laser power density is 0.1 to 2 kW / cm 2 , preferably 0.5~1.2kW / cm 2 .

[0015] Optionally, the specific step of adjusting the oxygen partial pressure is: after the gas in the reaction chamber for accommodating the formed block is extracted, the total pressure of the chamber is controlled at 10 -2 ~10 -4 Pa adjusts the oxygen partial pressure in the cavity or extracts the gas and then fills in an inert gas to adjust the oxygen partial pressure in the cavity. Specifically, the formed block obtained in step (2) is placed in a crucible and then transferred to the reaction cavity. Specifically, the inert gas includes inert gases such as nitrogen, argon, and helium.

[0016] The process steps include:

[0017] Preferably, in step (1):

[0018] The oxides of TiO2 and metal M are powders with a purity higher than 99.9%.

[0019] The oxide of the metal M may be at least one of MgO, Al2O3, Sc2O3, V2O3, Cr2O3, MnO, and FeO.

[0020] Preferably, in step (2):

[0021] The compression molding pressure is 5 to 20 MPa, preferably 8 to 15 MPa, and the holding time is 5 to 10 minutes.

[0022] The second aspect of the present invention provides a λ-Ti3O5 functional material prepared by the preparation method described in the first aspect of the present invention.

[0023] The beneficial effects of the present invention are:

[0024] The present invention adopts the strategy of adding metal oxides to directly prepare λ-Ti3O5 functional materials by using laser as a heat source without a reducing agent, and can obtain a λ-Ti3O5 stable phase at room temperature; the method of the present invention can directly use ordinary TiO2 powder as a raw material without preparing TiO2 powder into nanoparticles; the method of the present invention does not need to prepare λ-Ti3O5 into nanoparticles, and can directly obtain λ-Ti3O5 at room temperature; the laser is used as a heat source for direct reduction preparation in a low oxygen partial pressure environment, the process is simple, and the preparation efficiency is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is the X-ray diffraction pattern of the sample prepared in Example 1

[0026] Figure 2 is the X-ray diffraction pattern of the sample prepared in Example 2

[0027] Figure 3 is the X-ray diffraction pattern of the sample prepared in Example 3

[0028] Figure 4 is the X-ray diffraction pattern of the sample prepared in Example 4

[0029] Figure 5 is the X-ray diffraction pattern of the sample prepared in Example 5

[0030] Figure 6 is the X-ray diffraction pattern of the sample prepared in Example 6

[0031] Figure 7 is the X-ray diffraction pattern of the sample prepared in Example 7

[0032] Figure 8 This is the X-ray diffraction pattern of the sample prepared in Comparative Example 1 DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with the examples. It should be understood that the examples are only used to further illustrate and explain the invention and are not used to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0034] In this specification, unless otherwise specified, percentages refer to mass percentages.

[0035] Example 1

[0036] (1) Weigh a certain proportion of TiO2 and MgO powder, where the molar ratio of metal element atoms (Mg / Ti) is x:(3-x).

[0037] (2) The raw materials measured in step (1) are fully ground and pressed into shape in a mold at 8 MPa and maintained at the pressure for 5 minutes to obtain a block raw material.

[0038] (3) Place the sample obtained in step (2) in a crucible and transfer it to the reaction chamber, and adjust the oxygen partial pressure to 10 -8 Pa.

[0039] (4) After reaching the required oxygen partial pressure, the 2 The laser power density acted on the sample for 1 min, and the acting temperature was controlled at 2200°C.

[0040] (5) After high laser power density 0.2kW / cm 2 The power density is slowly reduced at a rate that continues to act on the sample.

[0041] (6) After the sample has cooled naturally, take out the prepared sample.

[0042] When x=0.1, the λ phase accounts for 96.59%; when x=0.09, the λ phase accounts for 95.53%.

[0043] Example 2

[0044] (1) Weigh a certain proportion of TiO2 and Al2O3 powder, where the molar ratio of metal element atoms (Al / Ti) is x:(3-x).

[0045] (2) The raw materials measured in step (1) are fully ground and pressed into shape in a mold at 10 MPa and maintained at the pressure for 5 minutes to obtain a block raw material.

[0046] (3) Place the sample obtained in step (2) in a crucible and transfer it to the reaction chamber, and adjust the oxygen partial pressure to 10 -7 Pa.

[0047] (4) After reaching the required oxygen partial pressure, 8.0 kW / cm 2 The laser power density acted on the sample for 3 minutes, and the action temperature was controlled at 2100℃.

[0048] (5) After high laser power density 0.5kW / cm 2 The power density is slowly reduced at a rate that continues to act on the sample.

[0049] (6) After the sample has cooled naturally, take out the prepared sample.

[0050] When x=0.12, the λ phase accounts for 92.14%; when x=0.11, the λ phase accounts for 90.37%; when x=0.1, the λ phase accounts for 87.43%.

[0051] Example 3

[0052] (1) Weigh a certain proportion of TiO2 and Sc2O3 powder, where the molar ratio of metal element atoms (Sc / Ti) is x:(3-x).

[0053] (2) The raw materials measured in step (1) are fully ground and pressed into shape in a mold at 8 MPa and maintained at the pressure for 5 minutes to obtain a block raw material.

[0054] (3) Place the sample obtained in step (2) in a crucible and transfer it to the reaction chamber, and adjust the oxygen partial pressure to 10 -7 Pa.

[0055] (4) After reaching the required oxygen partial pressure, the 2 The laser power density acted on the sample for 5 minutes, and the acting temperature was controlled at 2200℃.

[0056] (5) After high laser power density 0.2kW / cm 2 The power density is slowly reduced at a rate that continues to act on the sample.

[0057] (6) After the sample has cooled naturally, take out the prepared sample.

[0058] When x=0.1, the λ phase accounts for 96.79%; when x=0.09, the λ phase accounts for 92.30%.

[0059] Example 4

[0060] (1) Weigh a certain proportion of TiO2 and V2O3 powder, where the molar ratio of metal element atoms (V / Ti) is x:(3-x).

[0061] (2) The raw materials measured in step (1) are fully ground and pressed into shape in a mold at 10 MPa and maintained at the pressure for 10 min to obtain a bulk raw material.

[0062] (3) Place the sample obtained in step (2) in a crucible and transfer it to the reaction chamber, and adjust the oxygen partial pressure to 10 -7 Pa.

[0063] (4) After reaching the required oxygen partial pressure, the 2 The laser power density acted on the sample for 2 minutes, and the acting temperature was controlled at 1800℃.

[0064] (5) After high laser power density 0.6kW / cm 2 The power density is slowly reduced at a rate that continues to act on the sample.

[0065] (6) After the sample has cooled naturally, take out the prepared sample.

[0066] When x=0.3, the λ phase accounts for 96.06%; when x=0.25, the λ phase accounts for 94.45%.

[0067] Example 5

[0068] (1) Weigh a certain proportion of TiO2 and Cr2O3 powder, where the molar ratio of metal element atoms (Cr / Ti) is x:(3-x).

[0069] (2) The raw materials measured in step (1) are fully ground and pressed into shape in a mold at 15 MPa and maintained at the pressure for 5 minutes to obtain a block raw material.

[0070] (3) Place the sample obtained in step (2) in a crucible and transfer it to the reaction chamber, and adjust the oxygen partial pressure to 10 -8 Pa.

[0071] (4) After reaching the required oxygen partial pressure, the 2 The laser power density acted on the sample for 8 minutes, and the acting temperature was controlled at 1800℃.

[0072] (5) After high laser power density 0.9kW / cm 2 The power density is slowly reduced at a rate that continues to act on the sample.

[0073] (6) After the sample has cooled naturally, take out the prepared sample.

[0074] When x=0.4, the λ phase accounts for 93.58%; when x=0.35, the λ phase accounts for 91.52%.

[0075] Example 6

[0076] (1) Weigh a certain proportion of TiO2 and MnO powder, and the molar ratio of metal element atoms (Mn / Ti) is x:(3-x).

[0077] (2) The raw materials measured in step (1) are fully ground and pressed into shape in a mold at 10 MPa and maintained at the pressure for 5 minutes to obtain a block raw material.

[0078] (3) Place the sample obtained in step (2) in a crucible and transfer it to the reaction chamber, and adjust the oxygen partial pressure to 10 -9 Pa.

[0079] (4) After reaching the required oxygen partial pressure, the 2 The laser power density acted on the sample for 5 minutes, and the acting temperature was controlled at 2200℃.

[0080] (5) After high laser power density 0.6kW / cm 2 The power density is slowly reduced at a rate that continues to act on the sample.

[0081] (6) After the sample has cooled naturally, take out the prepared sample.

[0082] When x=0.2, the λ phase accounts for 94.63%; when x=0.15, the λ phase accounts for 90.27%; when x=0.1, the λ phase accounts for 80.64%.

[0083] Example 7

[0084] (1) Weigh a certain proportion of TiO2 and FeO powder, and the molar ratio of metal element atoms (Fe / Ti) is x:(3-x).

[0085] (2) The raw materials measured in step (1) are fully ground and pressed into shape in a mold at 15 MPa and maintained at the pressure for 10 minutes to obtain a block raw material.

[0086] (3) Place the sample obtained in step (2) in a crucible and transfer it to the reaction chamber, and adjust the oxygen partial pressure to 10 -7 Pa.

[0087] (4) After reaching the required oxygen partial pressure, the 2 The laser power density acted on the sample for 6 minutes, and the acting temperature was controlled at 1900℃.

[0088] (5) After high laser power density 0.2kW / cm 2 The power density is slowly reduced at a rate that continues to act on the sample.

[0089] (6) After the sample has cooled naturally, take out the prepared sample.

[0090] When x=0.225, the λ phase accounts for 97.16%; when x=0.2, the λ phase accounts for 96.81%.

[0091] Comparative Example 1

[0092] (1) Weigh a certain proportion of TiO2 and Al2O3 powder, where the molar ratio of metal element atoms (Al / Ti) is x:(3-x).

[0093] (2) The raw materials measured in step (1) are fully ground and pressed into shape in a mold at 10 MPa and maintained at the pressure for 5 minutes to obtain a block raw material.

[0094] (3) Place the sample obtained in step (2) in a crucible and transfer it to the reaction chamber, and adjust the oxygen partial pressure to 10 -7 Pa.

[0095] (4) After reaching the required oxygen partial pressure, 8.0 kW / cm 2 The laser power density acted on the sample for 3 minutes, and the action temperature was controlled at 2100℃.

[0096] (5) After the high laser power density was applied, the sample was taken out after natural cooling. Since the power reduction step was not implemented, Ti2O3 impurity phase appeared in the product.

Claims

1. A method for preparing λ-Ti 3 O 5 Functional materials approach, The following steps are involved: (1) The raw material is TiO 2 The powder and the oxide of metal M are measured according to the molar ratio of metal element atoms M / Ti being x:(3-x), where 0.09≤x≤0.40; (2) fully grinding the raw materials measured in step (1) to obtain a mixed powder, and pressing the mixed powder in a mold to obtain a molded block; (3) after adjusting the oxygen partial pressure in the cavity, subjecting the formed block obtained in step (2) to a laser heating reaction at a high laser power density, wherein the temperature of the laser heating reaction is 1800 to 2300° C., to obtain a sintered block A; (4) then slowly reducing the laser power density and allowing the laser to continue acting on the sintered block A obtained in step (3) to obtain a sintered block B; (5) After the sintered block B is naturally cooled, the λ-Ti 3 O 5 Functional materials.

2. The method according to claim 1, It is characterized in that In step (3), the oxygen partial pressure is lower than 10 -3 Pa.

3. The method according to claim 1, It is characterized in that In step (3), the laser heating reaction time is 1 to 10 minutes.

4. The method according to claim 1, It is characterized in that In step (3), the high laser power density is 1.0 to 10.0 kW / cm 2 .

5. The method according to claim 1, It is characterized in that In step (4), the rate of slowly reducing the laser power density is 0.1 to 2 kW / cm 2 .

6. The method according to claim 2, It is characterized in that The specific steps of adjusting the oxygen partial pressure are as follows: after the gas in the reaction chamber for accommodating the formed block is extracted, the total pressure of the chamber is controlled at 10 -2 ~10 -4 Pa adjusts the oxygen partial pressure in the cavity or extracts the gas and then fills it with inert gas to adjust the oxygen partial pressure in the cavity.

7. The method according to claim 1, It is characterized in that The oxide of the metal M is MgO, Al 2 O 3 ,Sc 2 O 3 ,V 2 O 3 ,Cr 2 O 3 , at least one of MnO, FeO.

8. The method according to claim 1, It is characterized in that In step (1), the TiO 2 The oxide of metal M is a powder with a purity higher than 99.9%.

9. The method according to claim 1, It is characterized in that In step (2), the compression molding pressure is 5 to 20 MPa, and the holding time is 5 to 10 min.

10. A λ-Ti 3 O 5 The functional material is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of light-induced phase transition storage powdery material lamda-Ti3O5

    CN104973622A

  • Method for preparing ceramics capable of repeatedly storing heat

    CN105481344A

  • Preparation and defocusing forming method of low-cost ceramic powder for selective laser melting

    CN111689764A

  • METHOD FOR PRODUCING λ TITANIUM SUBOXIDE

    JP2020015657A

  • Metal-substituted titanium oxide, and method for producing metal-substituted titanium oxide sintered body

    US20190161359A1

Cited By

  • Preparation method of lambda-Ti3O5 nano antifouling agent with photothermal-photodynamic antibacterial performance