Method for synthesizing periclase-forsterite refractory material at low temperature

Through the low-temperature synthesis method, raw materials such as high-silicon magnesite, magnesium oxide raw materials and talc ore are used, combined with silica sol, to solve the problem of harsh production conditions of high-temperature synthesis technology, and realize low-cost and efficient periclase-forsterite refractory materials Preparation, improves thermal shock resistance and service life.

CN118745116AInactive Publication Date: 2024-10-08LIAONING INST OF SCI & TECH

Patent Information

Application Number
CN202411119335.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The high-temperature synthesis technology of periclase-forsterite refractory materials in the prior art has harsh production conditions, resulting in high production costs and high preparation temperatures, making it difficult to effectively reduce the thermal expansion rate and improve thermal shock resistance.

Method used

Using a low-temperature synthesis method, through raw materials such as high-silicon magnesite, magnesia raw materials, talc ore and silica sol, through steps such as heating, grinding and calcination, the temperature is controlled at 1100-1300°C to reduce the preparation temperature and improve the thermal shock resistance of the material. sex.

Benefits of technology

The low-temperature synthesis of periclase-forsterite refractory materials has been achieved, which reduces production costs, improves thermal shock resistance, extends the service life of the material, and improves the bonding strength of composite aggregates through nano-scale silica particles. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for synthesizing a periclase-forsterite refractory material at low temperature, which comprises the following steps: preparing the following raw materials in parts by weight: 8-20 parts of high-silicon magnesite, 15-30 parts of magnesium oxide raw material, 8-15 parts of talc ore and 3-8 parts of additional silica sol; the method comprises the following steps: heating high-silicon magnesite to 600-900 DEG C, preserving heat for 4-6 hours to prepare high-silicon magnesite clinker, and crushing and sieving the clinker to obtain high-silicon magnesite clinker fine powder; the high-silicon magnesite is used as a main raw material, low-grade mineral resources are fully utilized, the production cost is reduced, the production benefit is improved, in addition, in the processing process, thermal stress generated by thermal expansion and shrinkage of the refractory material is absorbed and released, slag permeation and structural stripping of the refractory material are avoided, and the quality of the refractory material is improved. And the service life of the refractory material is prolonged. The silica sol, which is one of the raw materials, has relatively small granularity and superplasticity, is beneficial to reducing the preparation temperature of the periclase-forsterite refractory material, and has the effects of saving energy and reducing consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of periclase-forsterite refractory materials, in particular to a method for synthesizing periclase-forsterite refractory materials at low temperature. Background Art

[0002] Magnesia refractory is a refractory material made of magnesite, seawater magnesia and dolomite, with periclase as the main crystal phase and magnesium oxide content of more than 80%. It belongs to alkaline refractory. Magnesia refractory has high refractoriness and good resistance to alkaline slag and iron slag. It is an important high-grade refractory material, mainly used in open-hearth furnaces, electric furnaces, oxidation converters, non-ferrous metal smelting furnaces, cement kilns and calcining kilns for alkaline refractory materials.

[0003] The main chemical component of periclase is MgO, and the mineral composition is periclase equiaxed crystal system, with a density of 3.56-3.65 g / cm 3 , Mohs hardness is 5.5, melting point is 2800℃, it volatilizes significantly at 1800~2400℃, and is the main component of magnesia refractory materials. Forsterite is an island-shaped silicate mineral with a mineral composition of 2MgO-SiO2, theoretical chemical composition: MgO 57.3%, SiO242.7%, and the crystal structure belongs to the orthorhombic system. The overall performance of forsterite is consistent with that of periclase, and its thermal expansion coefficient is close to and lower than that of periclase. The thermal shock resistance of periclase-forsterite refractory materials is significantly improved compared with pure phase magnesia refractory materials, and has good application prospects. There are few natural high-purity forsterite, which is generally synthesized artificially. The synthesis methods include solid phase method, high-energy ball milling method, etc. The synthesis temperature is high and the production conditions are demanding. The preparation technology of periclase-forsterite refractory materials needs to be further improved. Therefore, a method for low-temperature synthesis of periclase-forsterite refractory materials is urgently needed to be developed. Summary of the invention

[0004] The object of the present invention is to provide a method for low-temperature synthesis of periclase-forsterite refractory materials to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for low-temperature synthesis of periclase-forsterite refractory material, the production method of which comprises the following steps: S1. In parts by weight, the following raw materials need to be prepared: 8-20 parts of high-silicon magnesite, 15-30 parts of magnesium oxide raw material, 8-15 parts of talc, and 3-8 parts of silica sol; S2, heating the high-silicon magnesite to 600-900°C, keeping the temperature for 4-6 hours, preparing high-silicon magnesite clinker, and crushing and sieving the clinker to obtain high-silicon magnesite clinker fine powder; S3, pouring the obtained high silicon magnesite clinker fine powder and magnesium oxide raw material into a drum, and grinding and mixing to obtain a mixture a; S4, crushing and sieving the talc ore to obtain fine powder, pouring the fine powder into a mixing drum, and then adding an appropriate amount of additives and silica sol to mix to obtain a mixture b; S5. Transfer the mixture a and the mixture b into a high-temperature kiln, raise the temperature to 1100-1300°C for calcination, keep the temperature and then cool with the furnace to obtain the periclase-forsterite refractory material.

[0006] Preferably, the magnesium oxide raw material is prepared from one or two of magnesium hydroxide, light-burned magnesia and magnesite.

[0007] Preferably, the additive is one or two of boric acid, borate, and metal halide.

[0008] Preferably, in step S3, the mass of the magnesium oxide raw material poured in is 20% of the fine powder of high-silicon magnesite clinker, and the mixing time is 30 minutes.

[0009] Preferably, the high-silicon magnesite is crushed and then calcined at 800° C. for 1 hour and cooled along with the furnace.

[0010] Preferably, the talc ore is crushed and sieved to obtain talc powder, which is poured into a mixing drum and mixed for 15 minutes.

[0011] Preferably, the cooling time in the high-temperature kiln is more than 2 hours, and the temperature is controlled below 50°C.

[0012] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses high-silicon magnesite as the main raw material, fully utilizes low-grade mineral resources, reduces production costs, and improves production efficiency. In addition, this method not only absorbs and releases the thermal stress generated by the thermal expansion and contraction of the refractory material during the processing, but also reduces its thermal expansion rate on a certain basis, improves the thermal shock resistance of the refractory material, avoids slag penetration and structural peeling of the refractory material, and extends the service life of the refractory material.

[0013] 2. Silica sol is a dispersion of nano-sized silica particles in water or solvent, which is conducive to the formation of nano-sized forsterite and can improve the bonding strength between different phases in the composite aggregate. Nano-materials show excellent superplasticity due to their high diffusion coefficient. Superplasticity refers to the fact that when inorganic materials with fine grain size are subjected to a slowly increasing load at a high temperature, their permanent deformation capacity will be greatly improved, exceeding the conventional deformation limit. Smaller particle size and superplasticity are conducive to reducing the preparation temperature of periclase-forsterite refractory materials, which has the effect of energy saving and consumption reduction. DETAILED DESCRIPTION

[0014] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0015] To achieve the above object, the present invention provides the following technical solution: a method for low-temperature synthesis of periclase-forsterite refractory material, the production method of which comprises the following steps: S1. In parts by weight, the following raw materials need to be prepared: 8-20 parts of high-silicon magnesite, 15-30 parts of magnesium oxide raw material, 8-15 parts of talc, and 3-8 parts of silica sol; S2, heating the high-silicon magnesite to 600-900°C, keeping the temperature for 4-6 hours, preparing high-silicon magnesite clinker, and crushing and sieving the clinker to obtain high-silicon magnesite clinker fine powder; S3, pouring the obtained high silicon magnesite clinker fine powder and magnesium oxide raw material into a drum, and grinding and mixing to obtain a mixture a; S4, crushing and sieving the talc ore to obtain fine powder, pouring the fine powder into a mixing drum, and then adding an appropriate amount of additives and silica sol to mix to obtain a mixture b; S5. Transfer the mixture a and the mixture b into a high-temperature kiln, raise the temperature to 1100-1300°C for calcination, keep the temperature and then cool with the furnace to obtain the periclase-forsterite refractory material. Embodiment 1:

[0016] A method for low-temperature synthesis of periclase-forsterite refractory material, the production method of which comprises the following steps: S1. In parts by weight, the following raw materials need to be prepared: 8 parts of high-silicon magnesite, 15 parts of magnesium oxide raw material, 8 parts of talc, and 3 parts of silica sol; S2, heating the high-silicon magnesite to 800°C and keeping the temperature for 4 hours to prepare high-silicon magnesite clinker, and crushing and sieving the clinker to obtain high-silicon magnesite clinker fine powder; S3, pouring the obtained high silicon magnesite clinker fine powder and magnesium oxide raw material into a drum, and grinding and mixing them for 30 minutes to obtain a mixture a; S4, crushing and sieving the talc ore to obtain fine powder, pouring the fine powder into a mixing drum, adding an appropriate amount of additives and silica sol, and mixing for 15 minutes to obtain a mixture b; S5. Transfer the mixture a and the mixture b into a high-temperature kiln, raise the temperature to 1100°C for calcination, keep the temperature for 2 hours and then cool with the furnace to obtain the periclase-forsterite refractory material. Embodiment 2:

[0017] A method for low-temperature synthesis of periclase-forsterite refractory material, the production method of which comprises the following steps: S1. In parts by weight, the following raw materials need to be prepared: 15 parts of high-silicon magnesite, 20 parts of magnesium oxide raw material, 12 parts of talc, and 5 parts of silica sol; S2, heating the high-silicon magnesite to 1000° C. and keeping the temperature for 5 hours to prepare high-silicon magnesite clinker, and crushing and sieving the clinker to obtain high-silicon magnesite clinker fine powder; S3, pouring the obtained high silicon magnesite clinker fine powder and magnesium oxide raw material into a drum, and grinding and mixing them for 40 minutes to obtain a mixture a; S4, crushing and sieving the talc ore to obtain fine powder, pouring the fine powder into a mixing drum, adding an appropriate amount of additives and silica sol, and mixing for 20 minutes to obtain a mixture b; S5. Transfer the mixture a and the mixture b into a high-temperature kiln, raise the temperature to 1200°C for calcination, keep the temperature for 2.5 hours and then cool with the furnace to obtain the periclase-forsterite refractory material. Embodiment three:

[0018] A method for low-temperature synthesis of periclase-forsterite refractory material, the production method of which comprises the following steps: S1. In parts by weight, the following raw materials need to be prepared: 20 parts of high-silicon magnesite, 30 parts of magnesium oxide raw material, 15 parts of talc, and 8 parts of silica sol; S2, heating the high-silicon magnesite to 900°C and keeping the temperature for 6 hours to prepare high-silicon magnesite clinker, and crushing and sieving the clinker to obtain high-silicon magnesite clinker fine powder; S3, pouring the obtained high silicon magnesite clinker fine powder and magnesium oxide raw material into a drum, and grinding and mixing them for 50 minutes to obtain a mixture a; S4, crushing and sieving the talc ore to obtain fine powder, pouring the fine powder into a mixing drum, adding an appropriate amount of additives and silica sol, and mixing for 25 minutes to obtain a mixture b; S5. Transfer the mixture a and the mixture b into a high-temperature kiln, raise the temperature to 1300°C for calcination, keep the temperature for 3 hours, and then cool with the furnace to obtain the periclase-forsterite refractory material.

[0019] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for low-temperature synthesis of periclase-forsterite refractory materials, Features: The production method comprises the following steps: S1. In parts by weight, the following raw materials need to be prepared: 8-20 parts of high-silicon magnesite, 15-30 parts of magnesium oxide raw material, 8-15 parts of talc, and 3-8 parts of silica sol; S2, heating the high-silicon magnesite to 600-900°C, keeping the temperature for 4-6 hours, preparing high-silicon magnesite clinker, and crushing and sieving the clinker to obtain high-silicon magnesite clinker fine powder; S3, pouring the obtained high silicon magnesite clinker fine powder and magnesium oxide raw material into a drum, and grinding and mixing to obtain a mixture a; S4, crushing and sieving the talc ore to obtain fine powder, pouring the fine powder into a mixing drum, and then adding an appropriate amount of additives and silica sol to mix to obtain a mixture b; S5. Transfer the mixture a and the mixture b into a high-temperature kiln, raise the temperature to 1100-1300°C for calcination, keep the temperature and then cool with the furnace to obtain the periclase-forsterite refractory material.

2. A method for low-temperature synthesis of periclase-forsterite refractory materials according to claim 1, Features: The magnesium oxide raw material is prepared from one or two of magnesium hydroxide, light-burned magnesia and magnesite.

3. A method for low-temperature synthesis of periclase-forsterite refractory materials according to claim 1, Features: The additive is one or two of boric acid, borate and metal halide.

4. A method for low-temperature synthesis of periclase-forsterite refractory materials according to claim 1, Features: In step S3, the mass of the magnesium oxide raw material poured in is 20% of the high-silicon magnesite clinker fine powder, and the mixing time is 30 minutes.

5. A method for low-temperature synthesis of periclase-forsterite refractory material according to claim 1, Features: The high silicon magnesite is crushed, calcined at 800° C. for 1 hour and cooled along with the furnace.

6. A method for low-temperature synthesis of periclase-forsterite refractory material according to claim 1, Features: The talc ore is crushed and sieved to obtain talc powder, which is poured into a mixing drum and mixed for 15 minutes.

7. A method for low-temperature synthesis of periclase-forsterite refractory material according to claim 1, Features: The cooling time in the high temperature kiln is more than 2 hours, and the temperature is controlled below 50°C.

Citation Information

Patent Citations

  • Refractory repairing material, method for preparing the same and composition comprising the same

    CN101434491A

  • Nano-aperture porous periclase-forsterite ceramic material and preparation method thereof

    CN107445594A

  • Periclase, forsterite and spinel construction material

    DE19548589A1

Cited By

  • Periclase and forsterite composite material as well as preparation method and application thereof