Metalloporphyrin structure, synthesis method thereof and application of metalloporphyrin structure in electrocatalytic oxygen reduction

By introducing a metalloporphyrin structure with a lone pair of electron groups regulated by triphenylamine in the oxygen reduction reaction, and loading it on carbon nanotubes, carbon black and graphene oxide, a composite electrocatalyst is formed, which solves the problem of the high cost of precious metal catalysts. problem, achieving efficient oxygen reduction performance and an environmentally friendly production process.

CN118745186AActive Publication Date: 2024-10-08JIANGSU UNIV

Patent Information

Application Number
CN202410824535.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-08
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

In the existing technology, the electrocatalysts for the oxygen reduction reaction are mainly noble metal nanomaterials, which are expensive. Moreover, the performance of the existing metal porphyrin structures in the oxygen reduction reaction has problems such as large overpotential and low electron transfer number, making it difficult to completely replace them. Precious metal catalyst.

Method used

Triphenylamine is used to regulate the metalloporphyrin structure that introduces lone pair electron groups, and is loaded on carbon nanotubes, carbon black and graphene oxide to form a composite electrocatalyst. The electron density distribution and catalytic interface charge state are improved through structural modification. , improve oxygen reduction performance.

Benefits of technology

It achieves efficient oxygen reduction performance, reduces oxygen reduction potential, increases reaction current density, has low cost, simple synthesis method, green and environmentally friendly production process, and good repeatability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745186A_ABST
    Figure CN118745186A_ABST
Patent Text Reader

Abstract

The invention provides a metalloporphyrin structure, a synthesis method thereof and application of the metalloporphyrin structure in electrocatalytic oxygen reduction, and belongs to the technical field of electrocatalyst preparation. The preparation method comprises the following steps: introducing lone pair electron groups on the basis of triphenylamine regulation to obtain a metalloporphyrin structure, and then loading the metalloporphyrin structure on carbon nanotubes, carbon black and graphene oxide to obtain the metalloporphyrin composite electrocatalyst of metalloporphyrin in acidic and alkaline media. The metalloporphyrin composite electrocatalyst has the characteristics of being simple in synthesis and preparation method, relatively low in cost, high in repeatability, green and environment-friendly in production process and the like; the metalloporphyrin composite electrocatalyst has excellent ORR performance, can be used for electrocatalytic oxygen reduction, and has good practicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrocatalyst preparation, and in particular relates to a metalloporphyrin structure and a synthesis method thereof, and application in electrocatalytic oxygen reduction. Background Art

[0002] Energy devices such as fuel cells and zinc-air batteries can efficiently convert the chemical energy of fuels directly into electricity, and are currently a key development area in the energy sector. However, electrocatalysts for the oxygen reduction reaction (ORR), a crucial component of these technologies, are still primarily based on precious metal nanomaterials. In existing technologies, platinum accounts for 10-70% of the electrocatalyst's mass, and this high cost severely limits the widespread adoption of these battery technologies.

[0003] Metalloporphyrins are widely present in nature and are easy to derive, so they are considered to have the potential to replace noble metal electrocatalysts. Porphyrin macrocycles can be simply modified to change the electron density distribution on their molecules, thereby improving the interaction between porphyrin and the support, the charge state on the catalytic interface, the metal-oxygen bond energy, the oxygen-oxygen bond energy and other transition state properties in the oxygen reduction reaction, thereby making it possible to obtain efficient oxygen reduction electrocatalysts. In the prior art, aromatic rings containing heteroatoms are selected as substituents and combined with acetylene black to obtain multifunctional electrocatalysts. However, this method requires long-term polymerization under solvent thermal conditions, the heterochain length cannot be controlled, and the heteroatom steric hindrance is large, resulting in a low porphyrin yield. In addition, the prior art introduces triphenylamine groups into porphyrins to increase the probability of collision with protons in the solution, effectively promoting oxygen reduction. However, the single triphenylamine functional group has limited regulatory effects on porphyrins, and the related organic catalytic complexes still have problems such as large overpotential and low electron transfer number, making it impossible to fully replace noble metal catalysts. Therefore, it is necessary to develop new metalloporphyrin structures and use them for electrocatalytic oxygen reduction. Summary of the Invention

[0004] In response to some deficiencies in the prior art, the present invention provides a metalloporphyrin structure, a synthesis method thereof, and application thereof in electrocatalytic oxygen reduction. The present invention introduces a lone pair electron group on the basis of triphenylamine regulation to obtain a metalloporphyrin structure, and then loads the metalloporphyrin structure on carbon nanotubes, carbon black, and graphene oxide to obtain a metalloporphyrin composite electrocatalyst of the metalloporphyrin in acidic and alkaline media. The metalloporphyrin composite electrocatalyst has the characteristics of simple synthesis and preparation methods, low cost, high repeatability, and a green and environmentally friendly production process. The metalloporphyrin composite electrocatalyst has excellent ORR performance, can be used for electrocatalytic oxygen reduction, and has good practicality.

[0005] In order to achieve the above technical objectives, the present invention adopts the following technical means:

[0006] The present invention first provides a metalloporphyrin structure, wherein the metalloporphyrin structure is a metalloporphyrin structure containing a symmetrical lone electron group and substituted with triphenylamine at the para position;

[0007] Its structural formula is:

[0008]

[0009] In the structural formula, R1 includes groups containing lone pair electrons and their derivative groups;

[0010] R2 is Where n is 0 to 2;

[0011] M is cobalt, iron or nickel.

[0012] Preferably, the metalloporphyrin structure contains triphenylamine and its derivative groups and lone pair electron groups.

[0013] Preferably, the lone pair electron group includes any one of carboxylic acid, cyanoacetic acid, thiophene, pyridine, furan, pyrimidine, 2,1,3-benzothiadiazole or a derivative thereof.

[0014] Preferably, the metalloporphyrin structure includes the metalloporphyrin structures shown in structural formulas 1 to 6:

[0015]

[0016] The present invention also provides a method for synthesizing the above-mentioned metalloporphyrin structure, which comprises:

[0017] (1) Compound II, tetraformylmethylboric acid, tetrakis(triphenylphosphine)palladium, tetrahydrofuran, and potassium carbonate are mixed to obtain a mixed solution, and the mixed solution is subjected to a first condensation reaction under stirring conditions. After the reaction, a first intermediate A is obtained; the structural formula of the compound II is R2-Br;

[0018] Compound III, pyrrole and dilute hydrochloric acid are mixed to carry out a second condensation reaction, and a second intermediate B is obtained after the reaction is completed; the structural formula of the compound III is

[0019] (2) The first intermediate A, the second intermediate B and anhydrous dichloromethane are uniformly mixed, and then trifluoroacetic acid is added dropwise thereto for a first stirring reaction. After the reaction is completed, tetrachlorobenzoquinone is added for a second stirring reaction. After the reaction is completed, a small amount of triethylamine is added to finally obtain the third intermediate C;

[0020] (3) refluxing the third intermediate C in chloroform, adding a metal salt, continuing to reflux and stir, extracting, and purifying to obtain the metalloporphyrin structure; the metal salt includes a nickel salt, a cobalt salt, or an iron salt.

[0021] Preferably, in step (1), the ratio of compound II, tetraformylmethylboric acid, tetrakis(triphenylphosphine)palladium, and tetrahydrofuran is 1-3 mol: 1.5-5 mol: 0.1-2 mol: 5-15 mL; wherein the final concentration of potassium carbonate in the mixed solution is 0.1-0.5 M;

[0022] The conditions of the first condensation reaction are: stirring the reaction in a dark environment under N2 protection for 5 to 20 hours;

[0023] The structural formula of the first intermediate A is

[0024] Preferably, in step (1), the ratio of compound III, pyrrole and dilute hydrochloric acid is 1-2 mmol: 5-8 mmol: 15-25 mL; wherein the concentration of dilute hydrochloric acid is 0.1 M to 0.4 M;

[0025] The conditions of the second condensation reaction are: stirring the reaction in a dark environment under N2 protection for 5 to 30 hours;

[0026] The structural formula of the second intermediate B is

[0027] Preferably, in step (2), the usage ratio of the first intermediate A, the second intermediate B, anhydrous dichloromethane, trifluoroacetic acid, tetrachlorobenzoquinone and triethylamine is 0.5-2 mmol: 0.5-2 mmol: 50-300 mL: 1-10 mmol: 1-5 mmol: 1-5 mmol;

[0028] The conditions for the first stirring reaction are: reaction at room temperature for 1 to 5 hours;

[0029] The conditions for the second stirring reaction are: reaction at room temperature for 1 to 5 hours;

[0030] The structural formula of the third intermediate C is:

[0031]

[0032] Preferably, in step (3), the usage ratio of the third intermediate C, chloroform, and metal salt is 0.01-1 mmol: 1-50 mL: 0.1-10 mmol;

[0033] The reflux stirring time is 5 to 60 minutes;

[0034] The cobalt salt includes cobalt acetate or cobalt chloride; the iron salt includes ferric chloride or ferrous chloride; and the nickel salt includes nickel nitrate or nickel acetylacetonate.

[0035] The present invention also provides a metal porphyrin composite electrocatalyst, which is a composite of the metal porphyrin structure and a semiconductor; the loading amount of the metal porphyrin structure is 0.01 to 1 wt%, and the semiconductor includes any one of carbon black, carbon nanotubes or graphene oxide.

[0036] Preferably, when the metal porphyrin structure is composited with carbon black, the metal porphyrin composite electrocatalyst is an irregular approximately spherical polyhedron;

[0037] When the metalloporphyrin structure is composited with carbon nanotubes, the metalloporphyrin composite electrocatalyst is tubular;

[0038] When the metal porphyrin structure is composited with graphene oxide, the metal porphyrin composite electrocatalyst is in sheet form.

[0039] The present invention also provides a method for synthesizing the metalloporphyrin composite electrocatalyst, the method comprising:

[0040] mixing any one of carbon black, carbon nanotubes or graphene oxide with the metalloporphyrin, then adding dichloromethane as a solvent, ultrasonically mixing the mixture until uniform, and then drying the mixture to obtain a composite;

[0041] The complex is added into a mixed solution composed of diluted Nafion, and the mixture is uniformly mixed by ultrasonication to obtain a metal porphyrin composite electrocatalyst.

[0042] Preferably, the ratio of the semiconductor to the metalloporphyrin is 5-100 mg:1-5 mg;

[0043] The polymer content in the Nafion solution is 0.001-0.1 wt %.

[0044] The present invention also provides the use of the above-mentioned metalloporphyrin structure or metalloporphyrin composite electrocatalyst in electrocatalytic oxygen reduction. Compared with the prior art, the present invention has the following advantages:

[0045] The lone pair electrons / partial charges of elements or groups can effectively generate electrostatic forces or intermolecular forces on charged ions in the electrolyte solution, affecting the local ion concentration of the catalyst molecules and changing the charge state and reaction barrier of the ground state molecules or transition states. The present invention introduces lone pair electron groups based on the regulation of triphenylamine. On the one hand, they can effectively adsorb protons in the solution, generate and promote the proton-coupled electron transfer process at the catalytic interface, and are expected to increase the number of electron transfers and promote four-electron reduction. On the other hand, the lone pair electrons can regulate the metal electron cloud density of the porphyrin center and form a stronger π-π* stacking with the carbon support, which can effectively improve the electrocatalytic oxygen reduction activity, reduce the oxygen reduction potential and increase the reaction current density.

[0046] The metalloporphyrin structure of the present invention has different interfacial charge separation and migration capabilities, which are related to the electron-donating ability of the substituent. Compared with the metalloporphyrin structure in the prior art, the metalloporphyrin structure is a symmetrical metalloporphyrin structure containing lone-pair electron groups above and below and substituted with triphenylamine in the para position. This special structure can effectively improve the oxygen reduction performance of porphyrin and promote catalytic interfacial charge separation.

[0047] The present invention synthesizes a metalloporphyrin composite electrocatalyst based on the metalloporphyrin structure. This metalloporphyrin exposes more active sites on carbon black, carbon nanotubes, and graphene oxide, thereby improving the utilization rate of the porphyrin molecules. The metalloporphyrin composite electrocatalyst has a reduction potential and corresponding current density close to those of Pt / C, demonstrating that the synergistic effect of the lone pair electron group and the triphenylamine group can effectively improve oxygen reduction. This provides a possible solution for the engineering and efficient production of metalloporphyrins as electrocatalysts.

[0048] The metalloporphyrin in the metalloporphyrin composite electrocatalyst described herein is supported on a carbon material, without significant changes in the primary morphology of the supported material, nor does the morphology significantly affect the electrocatalytic performance. The metalloporphyrin structure and metalloporphyrin composite electrocatalyst described herein have the advantages of simple synthesis and preparation methods, low cost, high reproducibility, and an environmentally friendly production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 This is a flow chart for the preparation of metal porphyrin composite electrocatalysts.

[0050] Figure 2 Scanning electron microscope images of metalloporphyrin / carbon black composite electrocatalyst (a), metalloporphyrin / carbon nanotube composite electrocatalyst (b), and metalloporphyrin / graphene oxide composite electrocatalyst (c).

[0051] Figure 3 The cyclic voltammograms of different metal porphyrin composite electrocatalysts obtained under 0.1 M KOH.

[0052] Figure 4 Linear sweep voltammograms of different metal porphyrin composite electrocatalysts obtained in 0.1 M KOH. DETAILED DESCRIPTION

[0053] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereto.

[0054] Example 1: Synthesis of Metalloporphyrin Structure and Metalloporphyrin / Carbon Black Composite Electrocatalyst

[0055] Ⅰ. Synthesis of Metalloporphyrin Structure:

[0056] The process of synthesizing the metalloporphyrin structure in this embodiment is as follows:

[0057]

[0058] The specific synthesis steps are:

[0059] (1) Synthesis of the first intermediate A:

[0060] 2mmol 4-bromo-N, N-triphenylaniline, 2.2mmol 4-formylphenylboronic acid, 0.1mol tetrakis(triphenylphosphine)palladium, 10mL tetrahydrofuran and 10mL 0.4M potassium carbonate were added into a flask to obtain a mixed solution, which was stirred for 12 hours in the dark under a nitrogen atmosphere. Yellow first intermediate A was obtained by vacuum distillation and silica gel column chromatography purification (dichloromethane: petroleum ether=1:1).

[0061] The first intermediate A is 4'-(diphenylamino)-[1,1'-biphenyl]-4-carbaldehyde, with a yield of 91%.

[0062] (2) Synthesis of the second intermediate B:

[0063] In a 500 mL two-necked flask, 60 mmol (4.2 mL) of pyrrole was added, and 200 mL of newly prepared 0.18 M HCl was added. The mixture was stirred and mixed evenly under nitrogen protection. Then, 10 mmol (2.2 g) of 4-(5,5-dimethyl-1,3-diox-2-yl)benzaldehyde was added. The mixture was stirred at room temperature for 12 h to carry out the second condensation reaction. After the reaction, the reaction solution was extracted with dichloromethane, and the organic phase at the lower layer was collected.

[0064] Anhydrous sodium sulfate was added to the organic phase to remove water and dry it, and the mixture was filtered. Silica gel powder was added and the mixture was dried using a rotary evaporator to obtain a crude product. The crude product was purified using silica gel column chromatography (dichloromethane: petroleum ether = 1:1). After purification, the crude product was recrystallized to obtain a white solid, namely the second intermediate B. The second intermediate B is 2,2'-((4-(5,5-dimethyl-1,3-dioxan-2-yl)phenyl)methylene)bis(1l2-pyrrole).

[0065] (3) Synthesis of the third intermediate C:

[0066] 1 mmol (349.43 mg) of the first intermediate A and 1 mmol (334.32 mg) of the second intermediate B were added to 100 mL of anhydrous dichloromethane to obtain a mixture. The mixture was stirred for 5 minutes in a dark, nitrogen atmosphere to mix uniformly, and then 2.42 mmol (0.18 mL) of trifluoroacetic acid was slowly added to initiate the reaction. After stirring at room temperature for 1 hour, 1.5 mmol (393.3 mg) of tetrachloro-1,4-benzoquinone was added and stirred under the same conditions for another hour. After the reaction was completed, 2.42 mmol (0.337 mL) of triethylamine was added to neutralize the reaction to obtain a crude product.

[0067] The crude product was purified by silica gel column chromatography (dichloromethane: petroleum ether = 1:2) to obtain a solid, i.e., the third intermediate C, which is 4', 4"'-(10,20-bis(4-(5,5-dimethyl-1,3-diox-2-yl)phenyl)porphyrin-5,5-diyl)bis(N,N-diphenyl-[1,1'-biphenyl]-4-amine), with a yield of 14.4%.

[0068] (4) Synthesis of metalloporphyrin structure:

[0069] 0.05 mmol (66.483 mg) of the third intermediate C was dissolved in 15 mL of chloroform, and then 9 mL of trifluoroacetic acid and 1 mL of water were added thereto, the reaction was vigorously stirred, and then triethylamine was added to neutralize it to alkalinity, and then purified and dissolved in 4.5 mL of tetrahydrofuran and 4.5 mL of glacial acetic acid, followed by the addition of 1 mmol (77 mg) of ammonium acetate, refluxed for 6 hours, and extracted with 100 mL of water.

[0070] The extract was dissolved in chloroform and refluxed at 68° C. for 15 minutes. 0.25 mmol (40.55 mg) of ferric chloride in 9 mL of methanol was then added to a two-necked flask with a syringe. Under continuous reflux and stirring, the reaction was monitored by TLC. The organic phase was collected by extraction with dichloromethane and water. The organic phase was then dried over anhydrous sodium sulfate, an appropriate amount of silica gel powder was added, and the mixture was concentrated to a dry powder by vacuum distillation. The powder was then purified by silica gel column chromatography (dichloromethane: petroleum ether=1:2) to obtain a dark red solid, i.e., the metalloporphyrin structure.

[0071] The metalloporphyrin structure is (2E, 2'E)-3,3'-((10,20-bis(4'-(diphenylamino)-[1,1'-biphenyl]-4-yl)ironporphyrin-5,5-diyl)bis(4,1-phenylene))bis(2-cyanoacrylic acid): yield: 86%, recorded as porphyrin 1.

[0072] Ⅱ. Synthesis of Metalloporphyrin Composite Electrocatalysts:

[0073] In this step, the porphyrin 1 prepared in (I) is combined with carbon black to synthesize a metalloporphyrin composite electrocatalyst. The synthesis process is as follows: Figure 1 The specific synthesis steps are as follows:

[0074] 3 mg of porphyrin 1 and 10 mg of carbon black were placed in a 10 mL glass vial, and an appropriate amount of dichloromethane (DCM) was added. After ultrasonic treatment for 30 minutes, the mixture was dried to obtain a composite. 1 mg of the dried composite was placed in a mixed solution consisting of 100 μL of water, 100 μL of ethanol, and 8 μL of 5% Nafion and ultrasonicated for 30 minutes to obtain the metalloporphyrin composite electrocatalyst, designated as the porphyrin 1 / carbon black composite electrocatalyst.

[0075] Figure 2 (a) is a scanning electron microscope image of porphyrin 1 / carbon black composite electrocatalyst. It can be seen from the figure that

[0076] The porphyrin 1 / carbon black composite electrocatalyst is spherical. At the same time, when the iron porphyrin doping amount is relatively small, the morphology of the porphyrin 1 / carbon black composite electrocatalyst does not change significantly compared with the morphology of the semiconductor.

[0077] Example 2: Synthesis of Metalloporphyrin Structure and Metalloporphyrin / Carbon Nanotube Composite Electrocatalyst

[0078] Ⅰ. Synthesis of Metalloporphyrin Structure:

[0079] The process of synthesizing the metalloporphyrin structure in this embodiment is as follows:

[0080]

[0081] As shown in the process, the synthesis steps of the metalloporphyrin structure described in this embodiment are basically the same as the synthesis steps of porphyrin 1 described in Example 1, except that the formylphenylboronic acid in step (1) is replaced with (4'-formyl-[1,1'-biphenyl]-4-yl)boric acid, and the 4-(5,5-dimethyl-1,3-diox-2-yl)benzaldehyde in step (2) is replaced with 4-pyridinecarboxaldehyde. The resulting 4", 4""-(10,20-di(pyridin-4-yl)ironporphyrin-5,15-diyl)bis(N,N-diphenyl-[1,1':4',1"-triphenyl]-4-amine) is recorded as porphyrin 2.

[0082] Ⅱ. Synthesis of Metalloporphyrin Composite Electrocatalysts:

[0083] In this step, the porphyrin 2 prepared in (I) is combined with carbon nanotubes to synthesize a metalloporphyrin composite electrocatalyst. The specific synthesis steps are as follows:

[0084] 3 mg of porphyrin 2 and 10 mg of carbon nanotubes were placed in a 10 mL glass vial, and an appropriate amount of dichloromethane (DCM) was added. After ultrasonic treatment for 30 minutes, the mixture was dried to obtain a composite. 1 mg of the dried composite was placed in a mixed solution consisting of 100 μL of water, 100 μL of ethanol, and 8 μL of 5% Nafion and ultrasonicated for 30 minutes to obtain the metalloporphyrin composite electrocatalyst, designated as the porphyrin 2 / carbon nanotube composite electrocatalyst.

[0085] Figure 2 (b) is a scanning electron microscope image of the porphyrin 2 / carbon nanotube composite electrocatalyst. It can be seen from the figure that the porphyrin 2 / carbon nanotube composite electrocatalyst is mainly tubular. At the same time, when the iron porphyrin doping amount is relatively small, the morphology of the porphyrin 2 / carbon nanotube composite electrocatalyst does not change significantly compared with the morphology of the semiconductor.

[0086] Example 3: Synthesis of Metalloporphyrin Structure and Metalloporphyrin / Graphene Oxide Composite Electrocatalyst

[0087] Ⅰ. Synthesis of Metalloporphyrin Structure:

[0088] The process of synthesizing the metalloporphyrin structure in this embodiment is as follows:

[0089]

[0090] As shown in the process, the steps for synthesizing the metalloporphyrin structure described in this embodiment are basically the same as the steps for synthesizing porphyrin 1 described in Example 1, except that the 4-(5,5-dimethyl-1,3-diox-2-yl)benzaldehyde in step (2) is replaced with 2-thiophenecarboxaldehyde, and the ferric chloride in step (3) is replaced with cobalt acetate tetrahydrate. The resulting 4',4"'-(10,20-di(thiophen-2-yl)cobaltporphyrin-5,15-diyl)bis(N,N-diphenyl-[1,1'-biphenyl]-4-amine) is designated as porphyrin 3. The yield of the metalloporphyrin 3 is 60%.

[0091] Ⅱ. Synthesis of Metalloporphyrin Composite Electrocatalysts:

[0092] In this step, the porphyrin 3 prepared in (I) is combined with graphene oxide to synthesize a metalloporphyrin composite electrocatalyst. The specific synthesis steps are as follows:

[0093] 3 mg of porphyrin 2 and 10 mg of graphene oxide were placed in a 10 mL glass vial, and an appropriate amount of dichloromethane (DCM) was added. After ultrasonic treatment for 30 minutes, the mixture was dried to obtain a composite. 1 mg of the dried composite was placed in a mixed solution consisting of 100 μL of water, 100 μL of ethanol, and 8 μL of 5% Nafion and ultrasonicated for 30 minutes to obtain the metalloporphyrin composite electrocatalyst, designated as porphyrin 3 / graphene oxide composite electrocatalyst.

[0094] Figure 2 (c) is a scanning electron microscope image of the porphyrin 3 / graphene oxide composite electrocatalyst. It can be seen from the figure that the porphyrin 3 / graphene composite electrocatalyst is mainly in the form of flakes. When the amount of cobalt porphyrin doping is relatively small, the morphology of the porphyrin 3 / graphene composite electrocatalyst does not change significantly compared with the morphology of the graphene semiconductor.

[0095] Example 4: Electrocatalytic Oxygen Reduction Performance Test of Metalloporphyrin Composite Electrocatalyst

[0096] In this example, the electrocatalytic oxygen reduction performance of the metal porphyrin composite electrocatalyst prepared in Examples 1 to 3 was tested. The specific test process is as follows:

[0097] Cyclic voltammetry, linear sweep voltammetry, and rotating disk electrode tests were performed in 0.1 M potassium hydroxide solution to test the oxygen reduction activity potential and selectivity of three porphyrin-coated carbon nanotubes, carbon black, and graphene oxide composites. The test results are as follows: Figures 3-4 and shown in Table 1. All curves in O2-saturated electrolyte were obtained by subtracting the background current from the double-layer capacitance by recording the corresponding curves using N2-saturated solution under the same experimental conditions.

[0098] The test results are as follows Figures 3-4 and as shown in Table 1.

[0099] Figure 3 The cyclic voltammograms obtained for different metalloporphyrin composite electrocatalysts in 0.1M KOH show that the three composite materials exhibit distinct cathodic oxygen reduction peaks, indicating oxygen reduction and catalytic oxygen reduction performance. Porphyrin 3 / graphene oxide composite exhibits the highest oxygen reduction reaction activity, reaching a maximum positive peak potential at 0.90V. Porphyrin 2 / carbon nanotube composite is second most active, reaching a maximum positive peak potential at 0.86V. Porphyrin 1 / carbon black composite, which performs poorly among the three, also reaches a maximum positive peak potential at 0.83V. This demonstrates that all three composite materials possess excellent oxygen reduction reaction activity, approaching that of the existing commercial catalyst Pt / C (oxygen reduction CV peak potential of approximately 0.90V in 0.1M KOH).

[0100] Table 1. Electrocatalytic oxygen reduction performance of the composite electrocatalysts

[0101]

[0102] Figure 4The linear sweep voltammograms of different metalloporphyrin composite electrocatalysts obtained in 0.1 M KOH are shown. As can be seen from the figure, the limiting current density increases with increasing rotational speed, which is mainly attributed to the increased diffusion rate of oxygen in the electrolyte. Table 1 shows the oxygen reduction performance parameters of the composite catalysts. Among them, the porphyrin 3 / graphene oxide composite material has the most excellent oxygen reduction performance, with a limiting current density of -5.00 mA cm at a rotational speed of 900 rpm. -2 The onset potential and half-wave potential of the porphyrin 3 / graphene oxide composite were 0.98 V and 0.90 V, respectively, followed by the porphyrin 2 / carbon nanotube composite (0.97 V, 0.89 V), and then the porphyrin 1 / carbon black composite (0.95 V, 0.86 V). All three composite electrocatalysts were close to or slightly better than the existing commercial catalyst Pt / C (in 0.1 M KOH, at a rotation speed of 900, the limiting current density was approximately -4.90 mA cm -2 , the onset potential is about 0.98 V, and the half-wave potential is about 0.89 V), so the metal porphyrin composite electrocatalyst of the present invention has excellent oxygen reduction performance.

[0103] In summary, the present invention synthesizes a porphyrin composite electrocatalyst based on the metal porphyrin structure, and the metal porphyrin composite electrocatalyst has the characteristics of being strong and easy to derive; the present invention changes the molecular structure of the basic porphyrin by structural modification, thereby affecting the electron density distribution on the molecule, the interaction between the porphyrin and the carrier, the charge state on the catalytic interface, and the strength of the metal-oxygen and oxygen-oxygen bonds, thereby improving the electrocatalytic oxygen reduction performance; the metal porphyrin composite electrocatalyst of the present invention has the characteristics of simple synthesis and preparation methods, low cost, high repeatability, and green and environmentally friendly production process; the metal porphyrin composite electrocatalyst has excellent oxygen reduction performance and is a new platinum-free catalyst that can be actually used for oxygen reduction.

[0104] The embodiments described are preferred implementations of the present invention, but the present invention is not limited to the above implementations. Any obvious improvements, substitutions or modifications that can be made by those skilled in the art without departing from the essence of the present invention are within the scope of protection of the present invention.

Claims

1. A metalloporphyrin structure, characterized in that: The metalloporphyrin structure is a metalloporphyrin structure containing a symmetrical lone electron group which is para-substituted with triphenylamine; Its structural formula is: In the structural formula, R1 includes groups containing lone pair electrons and their derivative groups; R2 is Where n is 0 to 2; M is cobalt, iron or nickel.

2. The metalloporphyrin structure according to claim 1, characterized in that The metalloporphyrin structure contains triphenylamine and its derivative groups and lone pair electron groups; The lone pair electron group includes any one of carboxylic acid, cyanoacetic acid, thiophene, pyridine, furan, pyrimidine, 2,1,3-benzothiadiazole or a derivative group thereof.

3. The method for synthesizing the metalloporphyrin structure according to any one of claims 1 or 2, characterized in that: The synthesis method comprises: (1) Compound II, tetraformylmethylboric acid, tetrakis(triphenylphosphine)palladium, tetrahydrofuran, and potassium carbonate are mixed to obtain a mixed solution, and the mixed solution is subjected to a first condensation reaction under stirring conditions, and a first intermediate A is obtained after the reaction is completed; the structural formula of the compound II is R2-Br; Compound III, pyrrole and dilute hydrochloric acid are mixed to carry out a second condensation reaction, and a second intermediate B is obtained after the reaction is completed; the structural formula of the compound III is (2) The first intermediate A, the second intermediate B and anhydrous dichloromethane are uniformly mixed, and then trifluoroacetic acid is added dropwise thereto for a first stirring reaction. After the reaction is completed, tetrachlorobenzoquinone is added for a second stirring reaction. After the reaction is completed, a small amount of triethylamine is added to finally obtain a third intermediate C; (3) refluxing the third intermediate C in chloroform, adding a metal salt, continuing to reflux and stir, extracting, and purifying to obtain the metalloporphyrin structure; the metal salt includes a nickel salt, a cobalt salt, or an iron salt.

4. The synthesis method according to claim 3, characterized in that In step (1), the amount ratio of compound II, tetraformylmethylboric acid, tetrakis(triphenylphosphine)palladium and tetrahydrofuran is 1-3 mol: 1.5-5 mol: 0.1-2 mol: 5-15 mL; wherein the final concentration of potassium carbonate in the mixed solution is 0.1-0.5 M; The conditions of the first condensation reaction are: stirring the reaction in a dark environment under N2 protection for 5 to 20 hours; The structural formula of the first intermediate A is The dosage ratio of compound III, pyrrole and dilute hydrochloric acid is 1-2 mmol: 5-8 mmol: 15-25 mL; wherein the concentration of dilute hydrochloric acid is 0.1 M to 0.4 M; The conditions of the second condensation reaction are: stirring the reaction in a dark environment under N2 protection for 5 to 30 hours; The structural formula of the second intermediate B is 5. The synthesis method according to claim 3, characterized in that In step (2), the usage ratio of the first intermediate A, the second intermediate B, anhydrous dichloromethane, trifluoroacetic acid, tetrachlorobenzoquinone and triethylamine is 0.5-2 mmol: 0.5-2 mmol: 50-300 mL: 1-10 mmol: 1-5 mmol: 1-5 mmol; The conditions of the first stirring reaction are: reacting at room temperature for 1 to 5 hours; The conditions of the second stirring reaction are: reacting at room temperature for 1 to 5 hours; The structural formula of the third intermediate C is:

6. The synthesis method according to claim 3, characterized in that In step (3), the usage ratio of the third intermediate C, chloroform and metal salt is 0.01-1 mmol: 1-50 mL: 0.1-10 mmol; The reflux stirring time is 5 to 60 minutes; The cobalt salt includes cobalt acetate or cobalt chloride; the iron salt includes ferric chloride or ferrous chloride; the nickel salt includes nickel nitrate or nickel acetylacetonate.

7. A metal porphyrin composite electrocatalyst, characterized in that: The metal porphyrin composite electrocatalyst is a composite of the metal porphyrin structure of claim 1 or 2 and a semiconductor; the loading amount of the metal porphyrin structure is 0.01 to 1 wt%, and the semiconductor includes any one of carbon black, carbon nanotubes or graphene oxide.

8. The method for synthesizing the metal porphyrin composite electrocatalyst according to claim 7, characterized in that: The synthesis method comprises: Mixing any one of carbon black, carbon nanotubes or graphene oxide with metal porphyrin, then adding dichloromethane as a solvent, mixing evenly by ultrasonication and then drying to obtain a composite; The complex is added into a mixed solution composed of diluted Nafion, and the metal porphyrin composite electrocatalyst is obtained after ultrasonic mixing.

9. The synthesis method according to claim 8, characterized in that The usage ratio of the semiconductor to the metal porphyrin is 5-100 mg:1-5 mg; The polymer content in the Nafion solution is 0.001-0.1 wt %.

10. Use of the metalloporphyrin structure according to any one of claims 1 to 2 or the metalloporphyrin composite electrocatalyst according to claim 7 in electrocatalytic oxygen reduction.

Citation Information

Patent Citations

  • Double-color fluorescent probe as well as preparation method and application thereof

    CN112500420A

  • Triphenylamine cobalt porphyrin catalyst and preparation method and application thereof

    CN113416981A

Cited By

  • Proton coupling electron transfer method for resource removal of organic pollutants

    CN120423679A