Method for preparing surface imprinted polymer microspheres through horseradish peroxidase-mediated surface initiation and application of surface imprinted polymer microspheres

Through the enzyme-mediated surface-initiated polymerization method, HRP is used to generate free radicals on the surface of nanospheres and combine with the polypeptide cross-linking agent, which solves the problems of insufficient pre-assembly and agglomeration under high monomer concentration in the existing technology, and improves the surface Specific selection ability and adsorption efficiency of imprinted polymers.

CN118745237AActive Publication Date: 2024-10-08CANGZHOU INSTITUTE OF TIANGONG UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410716538.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-08
Estimated Expiration
2044-06-04

AI Technical Summary

Technical Problem

Existing surface-imprinted polymer preparation methods are difficult to achieve sufficient preassembly and avoid aggregation at high monomer concentrations, resulting in poor specific selection ability for macromolecular templates and long adsorption times.

Method used

An enzyme-mediated surface-initiated polymerization method is used to generate free radicals on the surface of nanospheres through horseradish peroxidase (HRP). HRP is fixed on the surface of the microspheres to catalyze the reaction. A polypeptide cross-linking agent is used to enhance the pH of the imprinting layer. Responsiveness enables polymerization at high concentrations.

Benefits of technology

Under high-concentration conditions, sufficient preassembly of monomers and template molecules is achieved, agglomeration is avoided, the specific recognition ability and adsorption efficiency of surface-imprinted polymers are significantly improved, and the polymerization time is shortened.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745237A_ABST
    Figure CN118745237A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing surface imprinted microspheres through horseradish peroxidase-mediated surface initiation and application of the surface imprinted microspheres. Comprising the following steps: preparing and modifying nano microspheres; the preparation method comprises the following steps: mixing and dissolving a main monomer, a functional monomer, a polypeptide cross-linking agent and template protein in a water-soluble solvent to obtain a prepolymerization solution; adding horse radish peroxidase modified nanoparticles and an initiator into the mixed solution to initiate free radical polymerization; and eluting the template protein to obtain the polypeptide cross-linked surface imprinted microspheres. The nano-imprinted microspheres disclosed by the invention are prepared by an enzyme-mediated free radical polymerization method, the problem of poor imprinting effect in traditional free radical polymerization can be solved by realizing full pre-assembly of a monomer and a template under high concentration, and meanwhile, the agglomeration phenomenon possibly occurring under a high-concentration reaction condition is avoided. Due to the introduction of the polypeptide cross-linking agent, the imprinted microspheres have high specific selection and recognition capability on target protein, and the time for adsorbing template protein can be greatly shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biological separation engineering, and particularly relates to a method for preparing surface-imprinted polymer microspheres by surface initiation mediated by horseradish peroxidase and application thereof. Background Art

[0002] Surface imprinting is one of the mature methods for preparing molecularly imprinted polymers. Surface imprinted nanospheres have a larger specific surface area than traditional bulk imprinted polymers. The imprinted sites are located in the thin imprinted layer on the surface of the microspheres. The accessibility of the imprinted sites is higher and the mass transfer rate is faster. After the template is removed, the three-dimensional imprinted cavity that is complementary to the template molecule has a higher affinity for the template molecule.

[0003] At present, surface imprinted microspheres have been widely used in the field of protein separation and purification. For the preparation of surface imprinted polymers, researchers usually use a variety of polymerization methods such as traditional free radical polymerization, precipitation polymerization, emulsion polymerization, and surface induced atom transfer radical polymerization, but these polymerization methods still have many problems. These polymerization methods usually involve complex polymerization conditions, and the polymerization process is difficult to control. Traditional free radical polymerization reactions usually need to be carried out under conditions of highly diluted monomers. The concentrations of monomers and template molecules are low, and it is difficult to fully complete pre-assembly, resulting in low imprinting site-specific selectivity. At the same time, the traditional polymerization method is to generate free radicals in the solution, and the polymerization starts in the solution. When the concentration of the polymerized monomer is too high, although the effect of pre-assembly of monomers and template molecules can be enhanced, aggregation may occur at high monomer concentrations. For biomacromolecules, because they have a large molecular weight and a flexible three-dimensional structure, the imprinting process is more difficult. The surface imprinted polymers prepared by the above methods usually have poor imprinting effects on biomacromolecules. The surface imprinted polymers prepared by these methods are limited in their application in the separation and purification of proteins. For example, Dong et al. disclosed a nanoimprinted microsphere with bovine serum albumin (BSA) as the template molecule, using N,N-methylenebisacrylamide as a crosslinker, and using ammonium persulfate (APS) and N,N,N',N'-tetramethylethylenediamine (TEMED) to initiate free radical polymerization. The polymerization process of this method is multi-step, complex and difficult to control, the reaction time is as long as 24h, the adsorption equilibrium time is 120min, the imprinting capacity is 119.88mg / g, and the specificity for the template protein is also poor, with an imprinting factor of only 2.25 (DONG X, MAY, et al. Preparation of pH and temperature dual-sensitive molecularly imprinted polymers based on chitosan and N-isopropylacrylamide for recognition of bovine serum albumin [J]. Polymer International, 2019, 68 (5): 955-963.). Qian et al. prepared a nanoimprinted microsphere by oxidative self-polymerization of dopamine using Fe3O4@IL microspheres with imidazole groups and BSA. The imprinted layer of the nano-imprinted microspheres prepared by this method is relatively thick, the self-polymerization process is uncontrollable, the uniformity of the imprinted sites is poor, and the mass transfer resistance is large. The polymerization reaction of the imprinted microparticles lasts for 7 hours, the adsorption capacity is only 50.6 mg / mL, the imprinting factor is only 3.33, and the specific selectivity is low.(QIAN L, SUN J, et al. Immobilization of BSA on ionic liquid functionalized magnetic Fe3O4 nanoparticles for use in surface imprinting strategy [J]. Talanta, 2017, 168: 174-182). Wang et al. prepared a BSA nano-imprinted microsphere (Fe3O4@MnO2@BSA-MIPs) by superimposing MnO2 on the Fe3O4 hollow core and using chitosan as monomers through free radical polymerization. Although the nano-imprinted microspheres prepared by this polymerization method have a larger specific surface area, the pre-assembly of the monomer and the template is insufficient, the imprinting sites are few and the uniformity of the imprinting sites cannot be guaranteed, the integrity and utilization of the imprinting sites are not high, and therefore the specific selection ability is poor. The polymerization reaction time of this method is as long as 24 hours, and the preparation process is also complex and uncontrollable. The imprinting factor of the nano-imprinted particles is only 3.3. (WANG Y,MAY,et al.MnO2 corolla-like magneticmolecularly imprinted microspheres with enhanced adsorption capacity and specificity recognition to bovine serum albumin[J]. Chemical Engineering Journal, 2021,405:126655.). Summary of the invention

[0004] The purpose of the present invention is to improve the limitation that the existing preparation method of surface imprinted polymer can only initiate polymerization at a relatively dilute monomer concentration, because this limitation causes the surface imprinted polymer to have the problem of insufficient pre-assembly of functional monomers and template molecules, which further leads to the difficulty of the surface imprinted polymer's ability to specifically select macromolecular templates. By adopting an enzyme-mediated in-situ initiated polymerization method to generate free radicals on the surface of nano-microspheres, and using nano-microspheres as the reaction core, on the one hand, the problem of insufficient pre-assembly of template molecules and functional monomers in traditional free radical polymerization methods can be solved, and on the other hand, the problem of possible agglomeration in traditional polymerization methods under high monomer concentration conditions can be solved. Therefore, the method proposed by the present invention can achieve sufficient pre-assembly and avoid the occurrence of agglomeration at a higher monomer concentration, and further improves the problem of low specific recognition ability of surface imprinted polymers for template molecules and long adsorption time.

[0005] Enzyme-mediated free radical polymerization is becoming increasingly popular in the preparation of surface microgels due to its simple and mild initiation method. This method mainly initiates free radical polymerization through initiation systems such as glucose oxidase and β-D-glucose or acetylacetone (ACAC)-horseradish peroxidase (HRP)-hydrogen peroxide (H2O2). We enhance the binding ability to the template molecule by selecting functional monomers that can produce covalent or non-covalent interactions with the template molecule. At the same time, we use peptide cross-linkers to give the imprinted layer a reversible conformational transition that responds to pH, so that the imprinted site has the characteristic of accurately restoring the three-dimensional structure complementary to the template molecule, thereby enhancing the specificity of the imprinted site to the template molecule. We can combine these conditions with enzyme-mediated free radical polymerization methods to carry out polymerization reactions under high concentration conditions, thereby improving the problems of poor imprinting effect caused by insufficient pre-assembly of monomers and template molecules and the possibility of agglomeration at high polymerization concentrations in traditional free radical polymerization methods. Here, we use this method to prepare surface imprinted polymers, initiate polymerization under high concentration reaction conditions, enhance the pre-assembly effect of monomers and template molecules, and avoid agglomeration and gelation.

[0006] The present invention proposes an HRP-mediated surface initiation strategy for preparing surface imprinted polymer microspheres and applications thereof, wherein the peroxidase immobilized on the surface of the nano-microspheres is used as an active site to catalyze the reaction of H2O2 and acetylacetone to produce free radicals to gently initiate polymerization, thereby forming a stable imprinted gel layer.

[0007] The specific technical solutions are as follows:

[0008] A method for preparing surface-imprinted polymer microspheres by horseradish peroxidase-mediated surface initiation; comprising the following steps:

[0009] 1) horseradish peroxidase (HRP) is subjected to an amidation reaction with activated carboxyl-functionalized nanospheres to immobilize HRP on the surface of the microspheres as active sites, thereby obtaining HRP-modified nanoimprinted microspheres;

[0010] 2) dispersing the HRP-modified nanospheres obtained in step 1) in a phosphate buffer solution under ultrasound to obtain a dispersion of HRP nanoimprinted microspheres;

[0011] 3) adding the main monomer N-isopropyl acrylamide, the functional monomers acrylamide, methacrylic acid and dimethylaminoethyl methacrylate, the polypeptide cross-linking agent and the template protein bovine serum albumin (BSA) to the dispersion of the HRP nanoimprinted microspheres in step 2); after being completely dissolved, stirring and mixing evenly, and standing to complete the full pre-assembly process, to obtain a pre-polymerized mixed solution;

[0012] 4) passing N2 into the prepolymerized mixed solution obtained in step 3) to remove O2 in the system;

[0013] 5) Under mechanical stirring and N2 atmosphere, the pH of the solution after excluding the system O2 in step 4) is adjusted, so that when the polypeptide cross-linking agent is in a helix conformation condition, acetylacetone and hydrogen peroxide are added thereto to initiate a free radical polymerization reaction under HRP catalysis; after the reaction, the microspheres in the solution are magnetically separated, and then the microspheres are washed twice with ultrapure water to obtain surface-imprinted microspheres with templates.

[0014] 6) The surface imprinted nano-microspheres obtained in step 5) are placed in a phosphate buffer solution to elute the template, and then nano-imprinted microspheres (BSA-PC-Fe3O4@MIP) with imprinted cavities are obtained.

[0015] The method for preparing surface imprinted polymer microspheres by horseradish peroxidase-mediated surface initiation; based on the volume of the phosphate buffer solution used in step 2), the concentration of the main monomer N-isopropylacrylamide added in step 3) in the phosphate buffer solution is 5-50 mg / mL, the concentration of the functional monomer acrylamide (AAM) is 0.1-1.1 mg / mL, the concentration of methacrylic acid (MAA) is 0.001-0.011M, and the concentration of dimethylaminoethyl methacrylate (DMAEMA) is 0.001-0.011M.

[0016] The method for preparing surface imprinted polymer microspheres by horseradish peroxidase-mediated surface initiation; the crosslinker used in step 3) is a polyglutamic acid polypeptide crosslinker with double bonds at both ends of the chain segment, with a degree of polymerization ranging from 18 to 25, and a pH-responsive helix-coil conformational transition. (DONG Q, YANG M, WANG Y, et al. Peptide-crosslinked molecularly imprinted polymers for efficient separation of immunoglobulin G from human serum[J].

[0017] Biomaterials Science,2023,11(4):1398-1407)

[0018] The total amount is the sum of the amounts of the monomers and functional monomers used in step 3), and the amount of the polypeptide cross-linking agent added in step 3) is 1-5% of the total amount.

[0019] In step 5), the pH of the solution is adjusted to 4.5-5.0. The polypeptide cross-linking agent is in a helix conformation in this pH range, and the polypeptide cross-linking agent will not precipitate from the solution in this pH range.

[0020] In step 5), the HRP-mediated free radical polymerization has a reaction temperature of 20° C. to 35° C. and a reaction time of 2.5 to 6 h;

[0021] In step 6), the template is eluted in a solution similar to the human body fluid environment, and a phosphate buffer solution with a pH of 7.4 containing 154 mM NaCl is selected as the elution medium. At this time, the polypeptide cross-linking agent is in a coil conformation.

[0022] The nano-imprinted microspheres of the present invention are used as adsorption materials in high-specificity recognition and selection, rapid separation and purification of BSA.

[0023] The nanoimprinted microspheres of the present invention can complete the pre-assembly of monomers and template molecules at a higher concentration under an enzyme-mediated surface initiation system, thereby obtaining nanoimprinted microspheres with more effective imprinted sites. At the designed concentration in the experiment, no aggregation occurs during the polymerization process. The polypeptide cross-linking agent exists in helix and coil conformations at different pH values. The nanoimprinted microspheres have highly specific selection and recognition capabilities for target proteins in the helix conformation.

[0024] The method for preparing Fe3O4 nano-imprinted microspheres by free radical polymerization mediated by HRP can be used for the preparation of nano-imprinted polymers of different matrix materials, such as Fe3O4, SiO2, silver nano-microspheres, nickel nano-microspheres, etc. By modifying HRP on the surface of Fe3O4 nano-microspheres as an active core, a short-acting free radical is generated by using an initiation system of H2O2 and ACAC to quickly initiate free radical polymerization. Through this polymerization method, we can select a higher monomer concentration, achieve full pre-assembly of monomers and template molecules, and improve the integrity of the imprinted site and the specificity for the template molecule. At the same time, by using HRP as the active core to initiate polymerization in situ, the agglomeration phenomenon that may occur in the traditional free radical polymerization method is avoided. In addition, the reaction conditions of this method are simple and the process is easy to control. The use of a polypeptide cross-linking agent enables the imprinted layer to have a pH-responsive helix to coil conformational transition, and the imprinted cavity can accurately restore to a three-dimensional structure complementary to the template protein. The above advantages can significantly improve the imprinting performance of the nano-imprinted microspheres, and improve the imprinting performance of the nano-imprinted microspheres and the specific selection ability for the template protein. The results of protein adsorption studies show that the newly synthesized polypeptide cross-linked nanoimprinted microspheres have an imprinting capacity of 140 mg / g for bovine serum albumin and an imprinting factor of 10.4. The nanoimprinted microspheres can reach adsorption equilibrium within 30 minutes. Compared with the results of other literature, the nanoimprinted microspheres prepared by this method have greatly improved specific selectivity, polymerization reaction time, and time to reach adsorption equilibrium. In addition, this method is not limited to using bovine serum albumin as a template molecule, but can also be used to improve the specific selectivity of a variety of template molecules, such as bovine hemoglobin, cytochrome C, human serum albumin, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 : Transmission electron microscopy image of polypeptide cross-linked Fe3O4 surface imprinted microspheres prepared by HRP-mediated free radical polymerization using BSA as template protein, corresponding to Example 2;

[0026] Figure 2 :Effect of monomer concentration on the polydispersity of nanoparticles during the preparation of polypeptide cross-linked Fe3O4 surface imprinted microspheres;

[0027] Figure 3 :The hydrodynamic diameter of peptide-crosslinked Fe3O4 surface imprinted microspheres BSA-PC-Fe3O4@MIP changes with the concentration of reaction monomers and reaction time;

[0028] Figure 4 : Adsorption kinetics and isothermal adsorption diagrams of polypeptide cross-linked Fe3O4 surface imprinted microspheres BSA-PC-Fe3O4@MIP and non-imprinted microspheres BSA-PC-Fe3O4@NIP to template proteins, corresponding to Example 18;

[0029] Figure 5 : Selective adsorption results of peptide-cross-linked Fe3O4 nanoimprinted microspheres BSA-PC-Fe3O4@MIP and corresponding BSA-PC-Fe3O4@NIP on template protein and non-template protein;

[0030] Figure 6 :The results of SDS-PAGE analysis of BSA extracted from fetal bovine serum, wherein the first lane is BSA standard sample, the second lane is untreated fetal bovine serum, the third lane is fetal bovine serum treated with imprinted microspheres, and the fourth lane is a sample of the eluate after the fetal bovine serum was treated with imprinted microspheres and eluted with phosphate buffer solution. DETAILED DESCRIPTION

[0031] In the present invention, there can be a variety of nano-microspheres suitable for the polymerization method, such as gold, silver, nickel, silicon dioxide, Fe3O4 and other nano-microspheres. Fe3O4 nano-microspheres are selected as the matrix in this paper because they have excellent magnetic response properties. The hydrodynamic diameter of the nano-microspheres is between 50 and 300 nm, and the optimal range is between 100 and 200 nm. There are no specific restrictions on the modification methods of amino and carboxyl groups and the compounds used. There is no specific restriction on the method used for carboxyl activation. The modification of the enzyme uses peroxidase, and HRP is selected in this paper.

[0032] In the present invention, the main monomer, the functional monomer, the template protein and the polypeptide cross-linking agent are dissolved in a phosphate buffer solution to obtain a prepolymer solution. The main monomer and the functional monomer used in the polymerization reaction are commonly used monomers in the field of surface protein imprinting polymers, and there is no special limitation. The template protein is selected from common proteins, such as bovine serum albumin, human serum albumin, bovine hemoglobin, etc., and bovine serum albumin is selected in this article.

[0033] In the present invention, the substrate initiated by HRP is common oxygen or a combination of H2O2 and ACAC, preferably H2O2 and ACAC. Preparation of HRP-modified Fe3O4 nanoparticles:

[0034] 1) Fe3O4 nanospheres were prepared by solvothermal method, and then the washed Fe3O4 nanospheres were ultrasonically dispersed in a mixed solution of 400 mL ethanol, 12 mL ultrapure water and 12 mL ammonia water. After ultrasonication for 15 min, 0.1 mL of tetraethyl orthosilicate was added, and the mixture was mechanically stirred at 30°C for 2 h. Then, 12 mL of APTES was added to the mixed solution under ultrasonication, and the mixture was stirred and reacted at 45°C for 24 h.

[0035] 2) The amino-modified nanospheres obtained in step 1 were washed three times with a mixed solution of ethanol and ultrapure water, respectively. After washing three times with ultrapure water, they were dispersed in 400 mL of tetrahydrofuran solution by ultrasonication for 15 min, and then 43 g of succinic anhydride was added, and the reaction was mechanically stirred for 18 h.

[0036] 3) After washing the carboxyl-modified nanospheres obtained in step 2 three times with ultrapure water, they were ultrasonically dispersed in 100 mL of a phosphate buffer solution with a pH of 5.8, 1.2 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide were added, and the mixture was mechanically stirred at room temperature for 2 h to activate the carboxyl groups.

[0037] 4) The carboxyl-activated nanoparticles obtained in step 3 were washed three times with ultrapure water, and then resuspended in a phosphate buffer solution with a pH of 5.5 containing 1.5 mg / mL horseradish peroxidase, and reacted with mechanical stirring for 4 hours. The obtained HRP-modified nanoparticles were washed twice with ultrapure water.

[0038] The functionalization of the nanosphere surface was completed by amino modification using ethyl orthosilicate and 3-aminopropyltriethoxysilane (APTES); carboxyl modification was completed by succinic anhydride; carboxyl activation was completed by using 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide, the activator concentration was 10 mg / mL, and the activation time was more than 2 hours; enzyme modification was performed using horseradish peroxidase, the concentration of horseradish peroxidase in the solution was 1.5 mg / mL, and the reaction time was more than 4 hours (Microgel coating of magnetic nanoparticles via bienzyme-mediated free-radical polymerization for colorimetric detection of glucose[J].Nanoscale,2015,7(40):16578-16582)

[0039] Example 1

[0040] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0041] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0042] 3) Add 40 mg of bovine serum albumin to the dispersion obtained in step 2 and stir for 5 minutes to mix evenly. Then add 5.7 mg of acrylamide (0.1 mg / mL), 5.1 μL of methacrylic acid (0.001 M) and 10.1 μL of dimethylaminoethyl methacrylate (0.001 M) to the solution. Then add 0.25 g of the main monomer N-isopropylacrylamide (5 mg / mL) and stir for 10 minutes to fully dissolve, and change the polymerization reaction concentration by controlling its concentration. Subsequently, 83 mg of a polypeptide cross-linker with a degree of polymerization of 22 is dissolved in the solution to obtain a pre-polymerized mixed solution.

[0043] 4) Pass N2 into the mixed solution of step 3 to remove O2.

[0044] 5) After ensuring that O2 is removed in step 4, the pH of the mixed solution is adjusted to 5.0. Mechanically stir for 15 minutes under N2 atmosphere. Then, 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide are added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. The reaction is mechanically stirred for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres obtained are magnetically separated and washed three times with ultrapure water.

[0045] 6) The surface imprinted microspheres in step 5 were eluted with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was determined using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant. The obtained surface imprinted microspheres were named BSA-PC-Fe3O4@MIP. Non-imprinted microspheres BSA-PC-Fe3O4@NIP were prepared without adding template protein.

[0046] Imprinting Effect Studies:

[0047] Prepare bovine serum albumin solutions of different concentrations with 20mM pH 5.0 phosphate buffer solution. Add BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP at 25°C. After reaching adsorption equilibrium, use a UV spectrophotometer to detect the concentration of bovine serum albumin in the supernatant and calculate the adsorption amount. The adsorption amount is calculated using conventional calculation methods in the art, see J. Guo, et al. ANAL METHODS-UK, 7 (2015) 10018-10025. Draw an adsorption isotherm (equilibrium protein concentration-adsorption amount curve), and use the Langmuir model for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max It is 26.5 mg / g and the imprinting factor is 2.1.

[0048] Example 2

[0049] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0050] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0051] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 minutes to mix evenly, then add 42 mg (0.84 mg / mL) of acrylamide, 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 minutes to fully dissolve. Subsequently, 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 is dissolved in the above solution to obtain a prepolymerized mixed solution. At this point, the system cross-linking degree is 1%.

[0052] 4) Pass N2 into the mixed solution of step 3 to remove O2.

[0053] 5) Under N2 atmosphere, the pH of the mixed solution from step 4 with O2 removed was adjusted to 5.0, and then 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. The reaction was mechanically stirred for 4 h under N2 atmosphere and 25°C. The surface imprinted microspheres were magnetically separated and washed three times with ultrapure water.

[0054] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0055] Imprinting Effect Research:

[0056] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max The imprinting factor is 118 mg / g and 8.25. Figure 1 As shown in FIG. 1 , it can be observed through transmission electron microscopy that the surface of the prepared imprinted microspheres has an obvious imprinted layer, indicating that the method used in the present invention successfully initiates and synthesizes the imprinted polymer layer at a high monomer concentration of 40 mg / mL. Figure 2 As shown in the figure, even at a high NIPAM monomer concentration of 40 mg / mL, the polydispersity index of the imprinted microspheres is always below 0.1, indicating that the surface imprinted microspheres prepared using the enzyme-mediated surface initiation strategy have good monodispersity and will not agglomerate under high concentration reaction conditions. This method uses in situ initiation to make the polymerization more orderly, fully avoiding the agglomeration phenomenon that may occur in traditional free radical polymerization methods at high monomer concentrations. In addition, the adsorption capacity Q max It can be seen from the IF that it has a significantly higher specific selection ability, indicating that under the condition of high monomer concentration, the monomer and template molecules have achieved sufficient pre-assembly and the specificity of the imprinting site has been significantly improved. Figure 3 As shown, during the preparation of BSA-PC-Fe3O4@MIP, the hydrodynamic diameter has a mutation at 2 h and reaches growth equilibrium at 2.5 h, indicating that the reaction is completed in 2.5 h. Therefore, the polymerization method has a fast reaction speed. The polymerization can be completed in only 4 h, which can effectively shorten the time to obtain imprinted microspheres.

[0057] Example 3

[0058] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0059] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0060] 3) Add 40 mg of bovine serum albumin to the dispersion of step 2, stir for 5 min to mix evenly, then add 53 mg of acrylamide (1.06 mg / mL), 45 μL of methacrylic acid (0.1 M) and 89 μL of dimethylaminoethyl methacrylate (0.1 M) to the solution, then add 2.5 g of the main monomer N-isopropylacrylamide (50 mg / mL), stir for 10 min to fully dissolve. Subsequently, 838 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 is dissolved in the above solution to obtain a prepolymer solution.

[0061] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0062] 5) The pH of the prepolymer solution from step 4, which had been purged of O2, was adjusted to 5.0. Under N2 atmosphere, 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. The reaction was mechanically stirred for 4 h under N2 atmosphere and 25°C. The surface-imprinted microspheres were magnetically separated and washed three times with ultrapure water.

[0063] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0064] Imprinting Effect Research:

[0065] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max It is 109 mg / g and the imprinting factor is 8.01.

[0066] Example 4

[0067] The effect of the degree of polymerization of the peptide cross-linker on the imprinting effect at the optimal reaction monomer concentration (40 mg / mL).

[0068] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0069] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0070] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg (0.84 mg / mL) of acrylamide, 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, 804 mg of a polypeptide cross-linking agent with a degree of polymerization of 18 is dissolved in the above solution to obtain a prepolymer solution.

[0071] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0072] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Under N2 atmosphere, the reaction temperature was changed to 20°C and mechanically stirred for 4 hours. The surface imprinted microspheres were washed three times with ultrapure water.

[0073] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0074] Imprinting Effect Research:

[0075] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 20°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max It is 91 mg / g and the imprinting factor is 7.01.

[0076] Example 5

[0077] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0078] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0079] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg (0.84 mg / mL) of acrylamide, 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, 579 mg of a polypeptide cross-linking agent with a degree of polymerization of 25 is dissolved in the above solution to obtain a prepolymer solution.

[0080] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0081] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Under N2 atmosphere, the reaction temperature was changed to 20°C and mechanically stirred for 4 hours. The surface imprinted microspheres were washed three times with ultrapure water.

[0082] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0083] Imprinting Effect Research:

[0084] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 20°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max The imprinting factor is 7.53 and the molecular weight is 98 mg / g. Compared with the study in Example 2, the best imprinting effect was obtained by using a polypeptide cross-linking agent with a polymerization degree of 22, and the polypeptide cross-linking agent with this polymerization degree was used in subsequent studies.

[0085] Example 6

[0086] The effect of reaction temperature on the imprinting effect at the optimal reaction monomer concentration (40 mg / mL).

[0087] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0088] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0089] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg (0.84 mg / mL) of acrylamide, 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0090] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0091] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Under N2 atmosphere, the reaction temperature was changed to 20°C and mechanically stirred for 4 hours. The surface imprinted microspheres were washed three times with ultrapure water.

[0092] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0093] Imprinting Effect Research:

[0094] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 20°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max It is 80 mg / g and the imprinting factor is 6.67.

[0095] Example 7

[0096] The effect of reaction temperature on the imprinting effect at the optimal reaction monomer concentration (40 mg / mL).

[0097] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0098] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0099] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg (0.84 mg / mL) of acrylamide, 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0100] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0101] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Under N2 atmosphere, the reaction temperature was changed to 35°C and mechanically stirred for 4 hours. The surface imprinted microspheres were washed three times with ultrapure water.

[0102] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0103] Imprinting Effect Research:

[0104] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 35°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. maxThe imprinting factor is 5.41 and the reaction temperature is 25℃, which has the best imprinting effect and specific selection ability.

[0105] Example 8

[0106] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0107] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0108] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg (0.84 mg / mL) of acrylamide, 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0109] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0110] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Under N2 atmosphere and 25°C, the reaction time was changed to 2.5 h. The surface imprinted microspheres were washed three times with ultrapure water.

[0111] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0112] Imprinting Effect Research:

[0113] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. maxThe concentration of 100 mg / g and the imprinting factor are 8.

[0114] Example 9

[0115] The effect of reaction time on the imprinting effect under the conditions of optimal reaction monomer concentration (40 mg / mL) and reaction temperature 25°C.

[0116] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0117] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0118] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg (0.84 mg / mL) of acrylamide, 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0119] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0120] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Under N2 atmosphere and 25°C, the reaction time was changed to 6 h. The surface imprinted microspheres were washed three times with ultrapure water.

[0121] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0122] Imprinting Effect Research:

[0123] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max The imprinting factor is 7.86. The effect of reaction time on the imprinting effect shows that the best imprinting effect is achieved when the reaction time is 4 hours, and the difference in imprinting effect is small when the reaction time is more than 2.5 hours. Figure 3 As shown in the figure, the reaction is basically completed after 2.5 hours, so the imprinting effect is not much different.

[0124] Example 10

[0125] The effect of the pH of the reaction solution on the imprinting effect under the conditions of the optimal reaction monomer concentration (40 mg / mL), reaction temperature 25°C and reaction time 4 h.

[0126] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0127] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0128] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg (0.84 mg / mL) of acrylamide, 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0129] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0130] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 4.5, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. The reaction was mechanically stirred for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0131] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0132] Imprinting Effect Research:

[0133] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max It is 95 mg / g and the imprinting factor is 7.

[0134] Embodiment 11

[0135] The effect of the pH of the reaction solution on the imprinting effect under the conditions of the optimal reaction monomer concentration (40 mg / mL), reaction temperature 25°C and reaction time 4 h.

[0136] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0137] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0138] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg (0.84 mg / mL) of acrylamide, 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0139] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0140] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 4.8, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0141] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0142] Imprinting Effect Research:

[0143] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max The imprinting factor is 7.51 and the pH value of the reaction solution is 101 mg / g. The effect of the pH value of the reaction solution on the imprinting effect shows that the best imprinting effect is obtained when the pH value of the reaction solution is 5.0.

[0144] Example 12

[0145] Effect of the concentration of functional monomer acrylamide on the imprinting effect.

[0146] Effect of reaction solution pH on imprinting effect under the conditions of optimal NIPAM monomer concentration (40 mg / mL), reaction temperature 25°C and reaction time 4 h.

[0147] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0148] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0149] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 5.7 mg of acrylamide (0.1 mg / mL), 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0150] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0151] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0152] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0153] Imprinting Effect Research:

[0154] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max It is 97 mg / g and the imprinting factor is 7.1.

[0155] Example 13

[0156] Effect of the concentration of functional monomer acrylamide on the imprinting effect.

[0157] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0158] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0159] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 55 mg of acrylamide (1.1 mg / mL), 35 μL of methacrylic acid (0.008 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0160] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0161] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0162] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0163] Imprinting Effect Research:

[0164] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max The concentration of acrylamide monomer was 90 mg / g, and the imprinting factor was 6.73. The effect of acrylamide on the imprinting effect showed that the best imprinting effect was obtained when the concentration of acrylamide monomer was 0.84 mg / mL.

[0165] Embodiment 14

[0166] Effect of the concentration of functional monomer methacrylic acid on the imprinting effect.

[0167] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0168] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0169] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg of acrylamide (0.84 mg / mL), 5.1 μL of methacrylic acid (0.001 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0170] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0171] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0172] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0173] Imprinting Effect Research:

[0174] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max It is 96 mg / g and the imprinting factor is 7.1.

[0175] Embodiment 15

[0176] Effect of the concentration of functional monomer methacrylic acid on the imprinting effect.

[0177] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0178] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0179] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg of acrylamide (0.84 mg / mL), 45 μL of methacrylic acid (0.011 M) and 69 μL of dimethylaminoethyl methacrylate (0.008 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0180] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0181] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0182] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0183] Imprinting Effect Research:

[0184] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max The imprinting factor is 6.8 and the concentration of methacrylic acid is 92 mg / g. The effect of methacrylic acid on the imprinting effect shows that the best imprinting effect is obtained when the concentration of methacrylic acid monomer is 0.008 M.

[0185] Example 16

[0186] Effect of functional monomer dimethylaminoethyl methacrylate on imprinting effect.

[0187] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0188] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0189] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg of acrylamide (0.84 mg / mL), 35 μL of methacrylic acid (0.008 M) and 18 μL of dimethylaminoethyl methacrylate (0.001 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0190] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0191] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0192] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0193] Imprinting Effect Research:

[0194] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max It is 85 mg / g and the imprinting factor is 7.08.

[0195] Embodiment 17

[0196] Effect of functional monomer dimethylaminoethyl methacrylate on imprinting effect.

[0197] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0198] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0199] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg of acrylamide (0.84 mg / mL), 35 μL of methacrylic acid (0.008 M) and 89 μL of dimethylaminoethyl methacrylate (0.011 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, dissolve 658 mg of a polypeptide cross-linking agent with a degree of polymerization of 22 in the above solution to obtain a prepolymer solution.

[0200] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0201] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0202] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0203] Imprinting Effect Research:

[0204] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max The concentration of dimethylaminoethyl methacrylate monomer was 105 mg / g, and the imprinting factor was 7.8. The effect of dimethylaminoethyl methacrylate on the imprinting effect showed that the best imprinting effect was obtained when the concentration of dimethylaminoethyl methacrylate monomer was 0.008 M.

[0205] Embodiment 18

[0206] The effect of the amount of polyglutamic acid polypeptide cross-linker used, that is, the degree of cross-linking of the system, on the imprinting effect.

[0207] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0208] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0209] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg of acrylamide (0.84 mg / mL), 35 μL of methacrylic acid (0.008 M) and 89 μL of dimethylaminoethyl methacrylate (0.011 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, the crosslinking degree of the system is controlled to be 4%, and 2362 mg of a polypeptide crosslinker with a degree of polymerization of 22 is dissolved in the above solution to obtain a prepolymer solution.

[0210] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0211] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0212] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0213] Imprinting Effect Research:

[0214] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, and the adsorption isotherm was plotted (see Appendix). Figure 4 B) The Langmuir model was used to fit the curve to obtain the imprinted capacity Q of BSA-PC-Fe3O4@MIP. max The adsorption of BSA on BSA-PC-Fe3O4@MIP was 140 mg / g, the imprinting factor was 10.4, and BSA-PC-Fe3O4@MIP could reach adsorption equilibrium when the initial concentration of BSA solution was 0.5 mg / mL. At the same time, the adsorption process of BSA-PC-Fe3O4@MIP reached equilibrium in about 30 minutes. Compared with the common surface imprinted microspheres, it has the ability to quickly reach adsorption equilibrium. See Appendix Figure 4A. The polymerization reaction time of the surface imprinted microspheres in the reference (LI X, ZHOU J, et al. Effect of crosslinking degree and thickness of thermosensitive imprinted layers on recognition and elution efficiency of protein imprinted magnetic microspheres [J]. Sensors and Actuators B: Chemical, 2016, 225: 436-445.) is 24h, the adsorption equilibrium time is 150min, the imprinting effect is optimal when the crosslinking degree of the system is 30%, the imprinting capacity is 49.66mg / g, and the imprinting factor is 4.56. The surface imprinted microsphere system prepared in this embodiment has the best imprinting effect when the crosslinking degree is only 4%, and the polymerization reaction time, the time to reach adsorption equilibrium, the specific selection ability of the template protein and the imprinting effect are greatly improved.

[0215] Embodiment 19

[0216] The effect of the amount of polypeptide cross-linking agent used, that is, the degree of cross-linking of the system, on the imprinting effect.

[0217] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0218] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0219] 3) Add 40 mg of bovine serum albumin to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg of acrylamide (0.84 mg / mL), 35 μL of methacrylic acid (0.008 M) and 89 μL of dimethylaminoethyl methacrylate (0.011 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, the crosslinking degree of the system is controlled to be 5%, and 3290 mg of a polypeptide crosslinker with a degree of polymerization of 22 is dissolved in the above solution to obtain a prepolymer solution.

[0220] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0221] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0222] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0223] Imprinting Effect Research:

[0224] Different concentrations of bovine serum albumin solutions were prepared with 20 mM pH 5.0 phosphate buffer solution. BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BSA-PC-Fe3O4@MIP. max It is 132 mg / g and the imprinting factor is 9.8.

[0225] Embodiment 20

[0226] Changing the template protein used and selecting different template proteins will affect the imprinting properties of the prepared nanoimprinted microspheres.

[0227] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0228] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0229] 3) Add 40 mg of other proteins, such as bovine hemoglobin (BHb), to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg of acrylamide (0.84 mg / mL), 35 μL of methacrylic acid (0.008 M) and 89 μL of dimethylaminoethyl methacrylate (0.011 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, the crosslinking degree of the system is controlled to be 4%, and 2362 mg of a polypeptide crosslinker with a degree of polymerization of 22 is dissolved in the above solution to obtain a prepolymer solution.

[0230] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0231] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0232] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0233] Imprinting Effect Research:

[0234] BHb solutions of different concentrations were prepared with 20 mM pH 5.0 phosphate buffer solution. BHb-PC-Fe3O4@MIP or BHb-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of BHb-PC-Fe3O4@MIP. max It is 129 mg / g and the imprinting factor is 9.58.

[0235] Embodiment 21

[0236] Changing the template protein used and selecting different template proteins will affect the imprinting properties of the prepared nanoimprinted microspheres.

[0237] 1) HRP and carboxyl-functionalized Fe3O4 nanospheres are covalently fixed on the surface of the microspheres to obtain HRP-modified nanospheres.

[0238] 2) The HRP-modified nanospheres prepared in step 1 were dispersed into 50 mL of phosphate buffer solution by ultrasonication to obtain a dispersion.

[0239] 3) Add 40 mg of other proteins, such as human serum albumin (HSA), to the dispersion in step 2, stir for 5 min to mix evenly, then add 42 mg of acrylamide (0.84 mg / mL), 35 μL of methacrylic acid (0.008 M) and 89 μL of dimethylaminoethyl methacrylate (0.011 M) to the solution. Then add 2 g of the main monomer N-isopropylacrylamide (40 mg / mL) and stir for 10 min to fully dissolve. Subsequently, the crosslinking degree of the system is controlled to be 4%, and 2362 mg of a polypeptide crosslinker with a degree of polymerization of 22 is dissolved in the above solution to obtain a prepolymer solution.

[0240] 4) Pass N2 into the prepolymer solution of step 3 to remove O2.

[0241] 5) The pH of the prepolymer solution after excluding O2 in step 4 was adjusted to 5.0, and 2.04 mL of acetylacetone and 0.75 mL of hydrogen peroxide were added under N2 atmosphere to initiate free radical polymerization on the surface of the nanospheres through surface enzymatic reaction. Mechanical stirring was performed for 4 hours under N2 atmosphere and 25°C. The surface imprinted microspheres were washed three times with ultrapure water.

[0242] 6) The template protein was eluted from the surface-imprinted microspheres in step 5 with 40 mL of 20 mM pH 7.4 phosphate buffer (containing 154 mM NaCl), and the template protein in the supernatant of the eluate was measured using a UV spectrophotometer. After two elutions, no template protein was detected in the supernatant.

[0243] Imprinting Effect Research:

[0244] HSA solutions of different concentrations were prepared with 20 mM pH 5.0 phosphate buffer solution. HSA-PC-Fe3O4@MIP or HSA-PC-Fe3O4@NIP was added at 25°C. After reaching adsorption equilibrium, the concentration of bovine serum albumin in the supernatant was detected by UV spectrophotometer, the adsorption amount was calculated, the adsorption isotherm was plotted, and the Langmuir model was used for curve fitting to obtain the imprinting capacity Q of HSA-PC-Fe3O4@MIP. max The concentration of the imprinted protein was 134 mg / g, and the imprinting factor was 9.9. The results show that the method used in the present invention can be used to prepare surface imprinted microspheres of various template proteins, and still have excellent specific adsorption effects.

[0245] Specific adsorption studies:

[0246] Various protein solutions with a concentration of 0.5 mg / mL were prepared with 20 mM pH 5.0 phosphate buffer solution, including bovine serum albumin, lactate dehydrogenase (LDH), glucose oxidase (GOX), trypsin inhibitor (Try), myoglobin (Mb) and cytochrome C (Cyt C). BSA-PC-Fe3O4@MIP or BSA-PC-Fe3O4@NIP was added at 25°C. After sufficient adsorption, the absorbance of the supernatant was detected by ultraviolet light to calculate the adsorption amount. The imprinting factors of various proteins were 10.4 (BSA), 1.9 (LDH), 1.7 (GOX), 1.53 (Try), 1.3 (Mb), and 1.26 (Cyt C), see the attached manual. Figure 5 This result shows that the BSA-PC-Fe3O4@MIP surface imprinted microspheres prepared by the present invention can selectively adsorb BSA with high specificity and have high affinity for BSA, while the specific selectivity for non-template proteins is much lower.

[0247] Extraction of BSA from fetal bovine serum:

[0248] Fetal bovine serum was diluted 50 times with 20mM pH 5.0 phosphate buffer solution. 20mg BSA-PC-Fe3O4@MIP surface imprinted microspheres were swollen in pH 5.0 phosphate buffer solution (20mM) at 25°C for 1h. The imprinted microspheres were magnetically separated and added to 5mL of 50-fold diluted fetal bovine serum and adsorbed at 25°C for 1h. After the adsorption, the imprinted microspheres were magnetically separated and eluted with 20mM pH 7.4 phosphate buffer solution containing 154mMNaCl to recover the adsorbed BSA. The extraction results were analyzed by SDS-PAGE. Figure 6 In the figure, the first lane is natural BSA, the second lane is untreated fetal bovine serum sample, the third lane is egg white sample treated with nano-imprinted microspheres, and the fourth lane is the sample of surface imprinted microsphere eluate. Figure 6 The results in the above show that the BSA surface imprinted microspheres synthesized in Example 18 can selectively extract BSA from fetal bovine serum with high specificity. In the third lane, the BSA in the fetal bovine serum is almost completely extracted, and in the fourth lane, only the BSA band appears in the eluate. The above sample extraction results were analyzed by HPLC, and the purity of the extracted BSA was above 95%.

[0249] As can be seen from the above examples, the surface imprinted microspheres prepared by HRP-mediated free radical polymerization provided by the present invention, by fixing HRP on the surface of the imprinted microspheres as the active core, using acetylacetone and hydrogen peroxide as the initiation system to initiate polymerization in situ on the surface of the microspheres, effectively avoid the agglomeration problem that may occur in traditional free radical polymerization. In addition, this polymerization method confirms the feasibility of the method for preparing surface imprinted microspheres by enzyme-mediated free radical polymerization under conditions of a higher monomer concentration (40 mg / mL). This method promotes the full preassembly of monomers and template molecules, improves the integrity and specificity of the imprinted sites, and the obtained BSA-PC-Fe3O4@MIP has a higher adsorption capacity (Q max =140mg / g) and imprinting factor (IF=10.4). In addition, this polymerization method is simpler, the polymerization process is easier to control, and the polymerization reaction can be completed within 4h. For the introduction of polypeptide cross-linkers, because of their pH-responsive helix-coil conformational transition, when the pH is adjusted to 4.5-5.0, the polypeptide cross-linker exists in the helix conformation and will not precipitate from the reaction solution. The imprinted cavity can accurately restore the shape complementary to the size and spatial configuration of the template protein under the condition of changing pH, and can accurately identify the template protein, thereby further improving the specific selection ability for the template protein. At the same time, due to the presence of the polypeptide cross-linker, the cross-linking degree of the imprinted shell is reduced and the swelling degree is increased. The combined effect of the above conditions makes the BSA-PC-Fe3O4@MIP surface imprinted microspheres have a high degree of specific selection ability for the template protein.

Claims

1. A method for preparing surface-imprinted polymer microspheres by horseradish peroxidase-mediated surface initiation; characterized in that: The following steps are involved: 1) horseradish peroxidase (HRP) is subjected to an amidation reaction with activated carboxyl-functionalized nanospheres to immobilize HRP on the surface of the microspheres as active sites, thereby obtaining HRP-modified nanoimprinted microspheres; 2) dispersing the HRP-modified nanospheres obtained in step 1) in a phosphate buffer solution under ultrasound to obtain a dispersion of HRP nanoimprinted microspheres; 3) adding the main monomer N-isopropyl acrylamide, the functional monomers acrylamide, methacrylic acid and dimethylaminoethyl methacrylate, the polypeptide cross-linking agent and the template protein bovine serum albumin (BSA) to the dispersion of the HRP nanoimprinted microspheres in step 2); after being completely dissolved, stirring and mixing evenly, and standing to complete the full pre-assembly process, to obtain a pre-polymerized mixed solution; 4) passing N2 into the prepolymerized mixed solution obtained in step 3) to remove O2 in the system; 5) Under mechanical stirring and N2 atmosphere, the pH of the solution after excluding the system O2 in step 4) is adjusted, so that when the polypeptide cross-linking agent is in a helix conformation condition, acetylacetone and hydrogen peroxide are added thereto to initiate a free radical polymerization reaction under HRP catalysis; after the reaction, the microspheres in the solution are magnetically separated, and then washed twice with ultrapure water to obtain surface-imprinted microspheres with templates. 6) The surface imprinted nanospheres obtained in step 5) are placed in a phosphate buffer solution to elute the template, and then nanospheres with imprinted cavities are obtained.

2. The method for preparing surface imprinted polymer microspheres by horseradish peroxidase-mediated surface initiation as claimed in claim 1; characterized in that: Based on the volume of the phosphate buffer solution used in step 2), the concentration of the main monomer N-isopropylacrylamide added in step 3) in the phosphate buffer solution is 5-50 mg / mL, the concentration of the functional monomer acrylamide (AAM) is 0.1-1.1 mg / mL, the concentration of methacrylic acid (MAA) is 0.001-0.011 M, and the concentration of dimethylaminoethyl methacrylate (DMAEMA) is 0.001-0.011 M.

3. The method for preparing surface imprinted polymer microspheres by horseradish peroxidase-mediated surface initiation as claimed in claim 1; characterized in that: The cross-linking agent used in step 3) is a polyglutamic acid polypeptide cross-linking agent having double bonds at both ends of the chain segment, a degree of polymerization ranging from 18 to 25, and a pH-responsive helix-coil conformational transition.

4. The method for preparing surface imprinted polymer microspheres by horseradish peroxidase-mediated surface initiation according to claim 1; characterized in that: The total amount is the sum of the amounts of the monomers and functional monomers used in step 3), and the amount of the polypeptide cross-linking agent added in step 3) is 1-5% of the total amount.

5. The method for preparing surface imprinted polymer microspheres by horseradish peroxidase-mediated surface initiation according to claim 1; characterized in that: In step 5), the pH of the solution is adjusted to 4.5-5.

0. The polypeptide cross-linking agent is in a helix conformation in this pH range, and the polypeptide cross-linking agent will not precipitate from the solution in this pH range.

6. The method for preparing surface imprinted polymer microspheres by horseradish peroxidase-mediated surface initiation according to claim 1, characterized in that: In step 5), the HRP-mediated free radical polymerization has a reaction temperature of 20° C. to 35° C. and a reaction time of 2.5 to 6 hours.

7. The method for preparing surface imprinted polymer microspheres by horseradish peroxidase-mediated surface initiation according to claim 1; characterized in that: In step 6), the template is eluted in a solution similar to the human body fluid environment, and a phosphate buffer solution with a pH of 7.4 containing 154 mM NaCl is selected as the elution medium. At this time, the polypeptide cross-linking agent is in a coil conformation.

8. The surface imprinted polymer microspheres prepared by horseradish peroxidase-mediated surface initiation according to claim 1 are used as adsorption materials in high-specific recognition and selection, rapid separation and purification of BSA.

Citation Information

Patent Citations

  • Rapid method of determining clearance of prion protein

    CA2262066A1

  • Preparation method of thymopentin molecularly-imprinted magnetic microspheres

    CN103333295A

  • Method for detecting glycoprotein by molecularly imprinted microspheres based on boric acid fluorescence probe

    CN104483295A

  • Preparation method and use of horseradish peroxidase molecularly imprinted fluorescent sensing material

    CN108341915A

  • Polyeptide crosslinked protein molecularly imprinted polymer, and preparation method and application thereof

    CN109897144A