Flame-retardant and heat-insulating composite material with impact protection function for battery and preparation method of flame-retardant and heat-insulating composite material

By using raw materials such as dimethylhydroxy silicone oil and boric acid to prepare shear-hardening adhesives in flame-retardant and thermal insulation composite materials for batteries, and combining them with other materials for mold compression molding and high-temperature foaming, the design of flame-retardant protective components for batteries has been solved. The problem of complex and viscous flow patterns of shear-thickening materials is achieved by simple preparation and good impact protection, flame retardant and heat insulation effects, and is suitable for battery packs of different specifications.

CN118745289APending Publication Date: 2024-10-08UNIV OF SCI & TECH OF CHINA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411050768.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The design of existing flame-retardant protective components for batteries is complex and difficult to adapt to battery packs of different specifications. Moreover, the shear-thickening material is in a viscous fluid state in its natural state, which poses a risk of leakage and is not suitable as a flame-retardant and thermal insulation material for batteries. Preparation process Complex and not conducive to mass production.

Method used

Use dimethylhydroxy silicone oil and boric acid to prepare shear-hardening glue, and add ammonium polyphosphate, ethylene-vinyl acetate copolymer, azodicarbonamide, methyl vinyl silicone rubber, benzoyl peroxide, and dihydrogen peroxide. Cumene and zinc oxide are used to prepare flame-retardant and heat-insulating composite materials with impact protection function through mold compression molding and high-temperature foaming.

Benefits of technology

It simplifies the preparation process, is suitable for large-scale industrial production, provides flexible size applications, has good impact resistance and flame retardant and heat insulation effects, slows down the spread of thermal runaway, and improves the safety of vehicles and personnel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a flame-retardant and heat-insulating composite material with an impact protection function for a battery and a preparation method of the flame-retardant and heat-insulating composite material, and relates to the technical field of heat insulation and protection of new energy automobile batteries. The composite material is prepared from the following components: dimethyl hydroxyl silicone oil, ammonium polyphosphate, an ethylene-vinyl acetate copolymer, azodicarbonamide, boric acid, methyl vinyl silicone rubber, benzoyl peroxide, dicumyl peroxide and zinc oxide. The preparation method comprises the following steps: preparing shear hardening rubber from silicone oil and boric acid; uniformly mixing the obtained shear hardening rubber with other components; and finally, carrying out high-pressure treatment and high-temperature foaming on the obtained mixture to obtain the composite material. The composite material can be processed into various corresponding shapes by designing various preparation molds according to requirements, the composite material is placed among battery cells in a battery pack to separate the battery cells, and the composite material filled in the battery pack can play roles in heat insulation, flame retardance and impact protection, and plays a role in protecting the safety of batteries and personnel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thermal insulation protection of power batteries for new energy vehicles, and in particular to a flame retardant thermal insulation composite material for batteries with an impact protection function and a preparation method thereof. Background Art

[0002] New energy vehicles use electricity, which is more environmentally friendly, sustainable, low-cost and easy to obtain than petroleum fuels. Therefore, the number of new energy vehicles has increased rapidly in recent years. New energy vehicles usually use lithium batteries to power them. The safety of automotive battery packs has also attracted much attention. There have been many cases of electric vehicle batteries spontaneously igniting and exploding. Batteries may cause thermal runaway when they are hit, squeezed or abused by heat. When a single battery has thermal runaway, the heat and fire it generates will quickly transfer to surrounding batteries, causing more batteries to be damaged, which can easily cause more serious battery damage and safety accidents.

[0003] Automotive batteries do not have heat-resistant and flame-retardant facilities between battery cells, resulting in poor safety of battery packs in the face of thermal runaway. Current solutions include related devices based on structural design, but customized insulation components of different sizes and shapes are required for battery packs of different specifications. In addition, the electrolyte must be modified to achieve thermal management of the battery, which can easily cause the electrochemical performance of the electrolyte to decrease. Other materials that focus on thermal insulation properties generally do not pay much attention to impact resistance.

[0004] Regarding the flame retardant and heat insulation protection technology of automobile batteries, there is a Chinese patent application with publication number CN117438711A, which discloses a flame retardant box for power batteries. The flame retardant box includes a box body and a box cover made of a fireproof material layer, providing a compact and high-temperature resistant flame retardant box for power batteries, which can avoid igniting surrounding batteries and causing fires when the battery has thermal runaway; the Chinese patent application with publication number CN117638369A discloses a heat-insulating flame-retardant lithium-ion battery structure, which includes a battery box, etc., and has the advantages of heat insulation and flame retardancy, high heat dissipation effect, high safety, etc.; there is also a Chinese patent application with publication number CN11737 The Chinese patent application No. 4502A discloses a lithium battery pack with a flame retardant mechanism, which includes a shell, and detects the lithium battery pack and accelerates the cooling effect by setting a cooling flame retardant component and a cooling pipe. When the lithium battery pack explodes, the lithium battery pack can be quickly extinguished and isolated to prevent the spread of the fire; and the patent with the authorization announcement number CN117477110B discloses a heat insulation protection component for power batteries, including a heat insulation sheet with a closed component and a ventilation slot. When the battery cell has thermal runaway, the thermal runaway battery cell can be isolated to reduce the impact on adjacent batteries, prolonging the time of the battery cell thermal runaway and the battery burning. The above patents require customized flame retardant boxes, protective components, etc. of different sizes and shapes for battery packs of different specifications, and the structural design is complex, which is not conducive to large-scale production and application. There is also a patent with authorization announcement number CN117431032B that discloses a foamed polyurethane sealant composition for batteries and a preparation method thereof. The foamed polyurethane sealant composition product obtained by the invention has good mechanical properties, high temperature aging resistance, hydrolysis resistance and waterproof properties. The product has the characteristics of good flame retardant effect, self-extinguishing when away from fire and no dripping. However, the foamed polyurethane sealant composition for batteries is a viscous substance and is not suitable for being placed between battery cells for flame retardancy and heat insulation.

[0005] Regarding the thermal insulation and impact protection technology based on shear thickening materials, there is a Chinese patent application with publication number CN116239818A, which discloses a method for preparing a composite material for impact protection, sound insulation and heat insulation. The method comprises mixing a shear hardening glue with ethanol, dissolving it ultrasonically, and then adding a solid porous amine matrix to obtain a homogeneous solution, impregnating, heating, and cooling to room temperature to obtain a composite material for impact protection, sound insulation and heat insulation. The composite material is a solid porous material in which the shear hardening glue is dispersed in a porous amine matrix, which can protect users from damage caused by various external stimuli such as impact, noise and temperature changes. However, the composite material adopts an impregnation method, has a certain risk of leakage, and does not have flame retardant properties; a Chinese patent application with publication number CN117089205A discloses a lightweight, impact protection, flame retardant, and heat insulation composite material and a method for preparing the composite material. The method for preparing the composite material comprises first preparing a shear hardening glue with silicone oil and a boride, and then mixing it with silicone rubber, sulfide, a microsphere foaming agent, and expandable graphite, and vulcanizing it to obtain a composite material. The composite material integrates impact protection, heat protection and lightweight, and can be widely used Applied to the human body, it protects the user from external stimulation and harm, but the composite material uses expandable graphite as a flame retardant. Graphite has good conductivity and is not suitable for use as a flame retardant and heat-insulating material for batteries; the patent with the authorization announcement number CN115179636B discloses a battery heat insulation cover for automobiles and its processing technology, wherein the modified silicon dioxide nanoparticles are prepared into a shear thickening liquid as a foaming agent to modify polyurethane, and the modified polyurethane foam material is hot-pressed in the mold through a mold to prepare a battery heat insulation cover for automobiles, which has good The invention discloses a method for preparing a shear thickening liquid having good heat insulation, heat resistance and strong impact resistance, but in this scheme, the silica nanoparticles need to be dispersed in a toluene solution of 3-mercaptopropyltrimethoxysilane, stirred, refluxed, centrifuged, washed with toluene and anhydrous ethanol and then vacuum dried to obtain modified silica nanoparticles, and then the modified silica nanoparticles are dispersed in anhydrous ethanol, homogenized once and then ultrasonically treated, polyethylene glycol is added and stirred, homogenized twice and ultrasonically treated, and then vacuum dried at a constant temperature to obtain a shear thickening liquid. The preparation process of the shear thickening liquid is complicated and not conducive to industrial production.

[0006] In general, there are currently flame-retardant boxes and protective components with different sizes, shapes and specifications that need to be customized for battery packs of different specifications, and the structural design of the protective components is complex, which is not conducive to large-scale production and application; or there is a risk of leakage of shear thickening materials, which is not suitable as flame-retardant and thermal insulation materials for batteries; and the preparation process of shear thickening materials is complicated, which is not conducive to industrial production and other technical problems that need to be solved urgently. Summary of the invention

[0007] In response to the above technical problems, the present invention provides a flame-retardant and heat-insulating composite material for batteries with impact protection function and a preparation method thereof, so as to solve the problems that the current flame-retardant protection components for batteries are complex in design, the buffer protection technology based on shear thickening materials is difficult to prepare, and the shear thickening materials are in a viscous flow state under natural conditions, so as to ensure the safety of vehicles and personnel.

[0008] To achieve the above object, the present invention provides the following technical solutions: A flame retardant and heat-insulating composite material for a battery with an impact protection function. The composite material is prepared by first preparing a shear-hardening glue from dimethyl hydroxy silicone oil and boric acid, then adding ammonium polyphosphate, ethylene-vinyl acetate copolymer, azodicarbonamide, methyl vinyl silicone rubber, benzoyl peroxide, diisopropylbenzene peroxide and zinc oxide, and pressing the uniformly mixed mixture in a mold, and then performing high-temperature foaming in an oven. The flame retardant and heat-insulating composite material is placed between single battery cells and on the periphery of a battery pack.

[0009] The present invention also provides a method for preparing a flame retardant and heat insulating composite material for a battery with an impact protection function, comprising the following steps: Step a. Add boric acid to dimethylhydroxy silicone oil, mix well, react at 180-200°C, and add octanoic acid to catalyze the reaction. Keep stirring during the reaction to allow the material to react fully until a shear-hardening glue is formed. Step b. mixing the shear hardening glue obtained in step a with ammonium polyphosphate, ethylene-vinyl acetate copolymer, azodicarbonamide, boric acid, methyl vinyl silicone rubber, benzoyl peroxide, dicumyl peroxide and zinc oxide; Step c. placing the product obtained in step b in a mold, flattening it at a pressure of 20 to 30 MPa and removing excess overflow; Step d. placing the flattened material in step c together with the mold at 160 to 190°C for 20 to 60 minutes to allow the product to fully foam; Step e. Cooling the product obtained in step d to room temperature.

[0010] Preferably, the high temperature foaming refers to a temperature condition of 160-190°C.

[0011] Preferably, the mass ratio of the dimethyl hydroxy silicone oil to boric acid is 20 to 40:1; the amount of n-octanoic acid added is 2.5 L Caprylic acid.

[0012] Preferably, the mass ratio of dimethyl hydroxy silicone oil to ammonium polyphosphate is 1:1-2.

[0013] Preferably, the mass ratio of dimethylhydroxysilicone oil to ethylene-vinyl acetate copolymer is 2:1-5.

[0014] Preferably, the mass ratio of ethylene-vinyl acetate copolymer to azodicarbonamide is 5 to 10:1.

[0015] Preferably, the mass ratio of dimethylhydroxy silicone oil to methylvinyl silicone rubber is 5 to 10:3.

[0016] Preferably, the mass ratio of dimethylhydroxysilicone oil to benzoyl peroxide is 10 to 20:1.

[0017] Preferably, the mass ratio of ethylene-vinyl acetate copolymer to dicumyl peroxide is 8 to 80:1.

[0018] Preferably, the mass ratio of ethylene-vinyl acetate copolymer to zinc oxide is 100:1.

[0019] Compared with the prior art, the present invention has the following beneficial effects: 1. The composite material proposed in the present invention is easy to prepare and is suitable for large-scale industrial production. It can be flexibly applied to various types of batteries by using molds of corresponding sizes and shapes according to needs. It also has the effects of impact protection and flame retardancy and heat insulation. When a single battery has thermal runaway, it can reduce the duration of its adverse effects on other batteries, and has a good additive effect on controlling the spread of fire.

[0020] 2. The present invention uses shear thickening substances to make the composite material have good impact resistance and has a better fixing effect than the dipping method, avoiding the possibility of damage to the battery pack caused by the flow and leakage of the shear thickening substances, and can more effectively protect the safety of vehicles and personnel. DETAILED DESCRIPTION

[0021] The technical scheme in the embodiment of the present invention is clearly and completely described below. Obviously, the described embodiment is only a part of the embodiment of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiment, it is carried out according to the conditions recommended by the normal conditions or the manufacturers. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0022] Embodiment 1: Take the following raw materials in mass ratio: Dimethylhydroxy silicone oil: boric acid = 30:1 Dimethylhydroxy silicone oil: methyl vinyl silicone rubber = 10:3 Dimethylhydroxy silicone oil:benzoyl peroxide=20:1 Dimethylhydroxy silicone oil: ammonium polyphosphate = 1:1 Dimethylhydroxy silicone oil: ethylene-vinyl acetate copolymer = 1:1 Ethylene-vinyl acetate copolymer: azodicarbonamide = 8:1 Ethylene-vinyl acetate copolymer: dicumyl peroxide = 40:1 Ethylene-vinyl acetate copolymer: zinc oxide = 100:1.

[0023] The method for preparing the composite material of this embodiment comprises the following steps: Dimethylhydroxy silicone oil and boric acid are mixed evenly, put into an oven at a temperature of 180°C, stirred every 5 minutes until a block product is generated, crushed and evenly mixed with the residual liquid, and after the liquid is basically agglomerated, n-octanoic acid is added and heated continuously. During the heating period, the product is stirred every 5 minutes until a homogeneous gel-like product is generated, then taken out and cooled to room temperature to obtain a shear hardening glue. The shear hardening glue is mixed evenly with ammonium polyphosphate, ethylene-vinyl acetate copolymer, azodicarbonamide, methyl vinyl silicone rubber, benzoyl peroxide, diisopropylbenzene peroxide and zinc oxide using a rubber mixer, the obtained mixture is pressed into a mold, and the mixture is flattened under a pressure of 25MPa. The treated sample is placed in an oven at 180°C and heated for high-temperature foaming treatment until the sample volume does not expand within ten minutes, that is, the foaming is completed, and the sample is taken out and cooled to room temperature.

[0024] Embodiment 2: Take the following raw materials in mass ratio: Dimethylhydroxy silicone oil: boric acid = 20:1 Dimethylhydroxy silicone oil: methyl vinyl silicone rubber = 3:1 Dimethylhydroxy silicone oil:benzoyl peroxide = 18:1 Dimethylhydroxy silicone oil: ammonium polyphosphate = 1:1 Dimethylhydroxy silicone oil: ethylene-vinyl acetate copolymer = 1:1 Ethylene-vinyl acetate copolymer: azodicarbonamide = 8:1 Ethylene-vinyl acetate copolymer: dicumyl peroxide = 40:1 Ethylene-vinyl acetate copolymer: zinc oxide = 100:1.

[0025] The preparation steps are the same as in Example 1.

[0026] Embodiment 3: Take the following raw materials in mass ratio: Dimethylhydroxy silicone oil: boric acid = 30:1 Dimethylhydroxy silicone oil: methyl vinyl silicone rubber = 10:3 Dimethylhydroxy silicone oil:benzoyl peroxide=20:1 Dimethylhydroxy silicone oil: ammonium polyphosphate = 1:2 Dimethylhydroxy silicone oil: ethylene-vinyl acetate copolymer = 1:2 Ethylene-vinyl acetate copolymer: azodicarbonamide = 10:1 Ethylene-vinyl acetate copolymer: dicumyl peroxide = 50:1 Ethylene-vinyl acetate copolymer: zinc oxide = 100:1.

[0027] The preparation steps are the same as in Example 1.

[0028] Embodiment 4: Take the following raw materials in mass ratio: Dimethylhydroxy silicone oil: boric acid = 30:1 Dimethylhydroxy silicone oil: methyl vinyl silicone rubber = 10:3 Dimethylhydroxy silicone oil:benzoyl peroxide=20:1 Dimethylhydroxy silicone oil: ammonium polyphosphate = 2:3 Dimethylhydroxy silicone oil: ethylene-vinyl acetate copolymer = 2:3 Ethylene-vinyl acetate copolymer: azodicarbonamide = 8:1 Ethylene-vinyl acetate copolymer: dicumyl peroxide = 40:1 Ethylene-vinyl acetate copolymer: zinc oxide = 100:1.

[0029] The preparation steps are the same as in Example 1.

[0030] Embodiment 5: Take the following raw materials in mass ratio: Dimethylhydroxy silicone oil: boric acid = 30:1 Dimethylhydroxy silicone oil: methyl vinyl silicone rubber = 10:3 Dimethylhydroxy silicone oil:benzoyl peroxide=20:1 Dimethylhydroxy silicone oil: ammonium polyphosphate = 1:1 Dimethylhydroxy silicone oil: ethylene-vinyl acetate copolymer = 1:1 Ethylene-vinyl acetate copolymer: azodicarbonamide = 9:1 Ethylene-vinyl acetate copolymer: dicumyl peroxide = 50:1 Ethylene-vinyl acetate copolymer: zinc oxide = 100:1.

[0031] The preparation steps are the same as in Example 1.

[0032] Embodiment 6: Take the following raw materials in mass ratio: Dimethylhydroxy silicone oil: boric acid = 30:1 Dimethylhydroxy silicone oil: methyl vinyl silicone rubber = 10:3 Dimethylhydroxy silicone oil:benzoyl peroxide=20:1 Dimethylhydroxy silicone oil: ammonium polyphosphate = 1:1 Dimethylhydroxy silicone oil: ethylene-vinyl acetate copolymer = 1:1 Ethylene-vinyl acetate copolymer: azodicarbonamide = 8:1 Ethylene-vinyl acetate copolymer: dicumyl peroxide = 40:1 Ethylene-vinyl acetate copolymer: zinc oxide = 100:1.

[0033] The preparation steps are the same as in Example 1.

[0034] Embodiment 7: Take the following raw materials in mass ratio: Dimethylhydroxy silicone oil: boric acid = 40:1 Dimethylhydroxy silicone oil: methyl vinyl silicone rubber = 10:3 Dimethylhydroxy silicone oil:benzoyl peroxide=20:1 Dimethylhydroxy silicone oil: ammonium polyphosphate = 1:1 Dimethylhydroxy silicone oil: ethylene-vinyl acetate copolymer = 2:1 Ethylene-vinyl acetate copolymer: azodicarbonamide = 10:1 Ethylene-vinyl acetate copolymer: dicumyl peroxide = 80:1 Ethylene-vinyl acetate copolymer: zinc oxide = 100:1.

[0035] The preparation steps are the same as in Example 1.

[0036] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A flame retardant and heat insulating composite material for batteries with impact protection function, characterized in that: A flame retardant and heat-insulating composite material mixed with a shear thickening substance is placed in the battery pack. The composite material is prepared by first preparing a shear-hardening glue from dimethyl hydroxy silicone oil and boric acid, and then adding ammonium polyphosphate, ethylene-vinyl acetate copolymer, azodicarbonamide, methyl vinyl silicone rubber, benzoyl peroxide, diisopropylbenzene peroxide and zinc oxide. The evenly mixed mixture is pressed into shape in a mold and then foamed at high temperature in an oven.

2. The flame retardant and heat-insulating composite material for batteries with impact protection function according to claim 1, characterized in that: Composite materials are placed between battery cells and around the battery pack for impact protection and heat insulation. The placement method and material shape are adjusted accordingly as the shape and size of the battery change.

3. A method for preparing a flame-retardant and heat-insulating composite material for batteries with impact protection function, characterized in that: The following steps are involved: Step a. Add boric acid to dimethylhydroxy silicone oil, mix well, react at 180-200°C, and add octanoic acid to catalyze the reaction. Keep stirring during the reaction to allow the material to react fully until a shear-hardening glue is formed. Step b. mixing the shear hardening glue obtained in step a with ammonium polyphosphate, ethylene-vinyl acetate copolymer, azodicarbonamide, boric acid, methyl vinyl silicone rubber, benzoyl peroxide, dicumyl peroxide and zinc oxide; Step c. placing the product obtained in step b in a mold, flattening it at a pressure of 20 to 30 MPa and removing excess overflow; Step d. placing the flattened material in step c together with the mold at 160 to 190°C for 20 to 60 minutes to allow the product to fully foam; Step e. Cooling the product obtained in step d to room temperature.

4. The preparation method according to claim 3, characterized in that: The high temperature foaming is achieved at a temperature of 160-190°C.

5. The preparation method according to claim 3, characterized in that: The mass ratio of dimethyl hydroxy silicone oil to boric acid is 20 to 40:1; the amount of n-octanoic acid added is 2.5 L Caprylic acid.

6. The preparation method according to claim 3, characterized in that: The mass ratio of dimethyl hydroxy silicone oil to ammonium polyphosphate is 1:1-2.

7. The preparation method according to claim 3, characterized in that: The mass ratio of dimethylhydroxy silicone oil to ethylene-vinyl acetate copolymer is 2:1-5.

8. The preparation method according to claim 3, characterized in that: The mass ratio of ethylene-vinyl acetate copolymer to azodicarbonamide is 5 to 10:

1.

9. The preparation method according to claim 3, characterized in that: The mass ratio of dimethylhydroxy silicone oil to methyl vinyl silicone rubber is 5 to 10:

3.

10. The preparation method according to claim 3, characterized in that: The mass ratio of dimethylhydroxysilicone oil to benzoyl peroxide is 10-20:

1.

11. The preparation method according to claim 3, characterized in that: The mass ratio of ethylene-vinyl acetate copolymer to dicumyl peroxide is 8 to 80:

1.

12. The preparation method according to claim 3, characterized in that: The mass ratio of ethylene-vinyl acetate copolymer to zinc oxide is 100:1.

Citation Information

Patent Citations

  • Preparation method of composite material with impact protection, sound insulation and heat insulation functions

    CN116239818A

  • Lightweight, impact-protective, flame-retardant and heat-insulating composite material and preparation method thereof

    CN117089205A

  • Lightweight, impact-resistant and heat-insulating composite material and preparation method thereof

    CN117624772A

  • Protective plate, battery pack and vehicle

    CN220021408U

  • Adhesive sealing composition for solid polymer electrolyte fuel cell separator, separator seal, and separator