Chloride-ion-resistant steel bar carbonization corrosion-resistant coating material and brushing process of chloride-ion-resistant steel bar carbonization corrosion-resistant coating material

By using a carbonized rust-resistant coating composed of inorganic cementitious materials such as phosphoaluminate cement, combined with the inner and outer coatings and carbonized curing processes, the problems of aging and insufficient rust-resistant performance of steel bar coatings are solved, and efficient protection of steel bars is achieved. Improved rust and long-term durability of the structure.

CN118745293APending Publication Date: 2024-10-08UNIV OF JINAN
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410852103.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing steel bar coatings are prone to aging and peeling off after long-term use, and have insufficient rust-inhibiting properties and cannot effectively prevent chloride ion erosion, resulting in steel bar corrosion and reduced durability of the concrete structure.

Method used

The carbonized rust-resistant coating material composed of inorganic cementitious materials such as phosphoaluminate cement, CS, C3S2, and γ-C2S is used to form a dense rust-resistant coating through the combined structure of the inner and outer coatings and the carbonization curing process. Block the penetration of chloride ions.

Benefits of technology

It significantly improves the corrosion resistance of steel bars, extends its service life, avoids coating aging and peeling, provides good adhesion and chlorine fixation effects, and enhances the load-bearing capacity of the structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a chloride-ion-resistant steel bar carbonization corrosion-resistant coating material and a brushing process thereof, and belongs to the field of steel bar corrosion-resistant materials. The coating material is composed of a component a and a component b, the component a is composed of an inorganic cementing material a, an early strength agent and a water reducing agent; the component b is prepared from an inorganic cementing material b, an early strength agent and a water reducing agent. According to the invention, the cement is used as a main material of the steel bar corrosion-resistant coating, so that on one hand, the coating has a longer service life and does not age, and on the other hand, the phosphoaluminate cement does not cause adverse influence on the steel bar. The phosphoaluminate cement is adopted as a composition phase, the prepared coating has good performance of curing chloride ions, meanwhile, CS, C3S2 and gamma-C2S are prone to carbonization, the compactness is improved after carbonization, the structure of the coating can be more compact, permeation of the chloride ions is blocked, and the phosphoaluminate cement and the CS, C3S2 and gamma-C2S synergistically play a role, and the rust inhibition effect can be effectively achieved. The coating provided by the invention has good adhesion, not only can play a good chlorine fixation role when being used in a chlorine salt environment, but also can play a role similar to a binder, so that the corrosion-resistant coating is not easy to age and peel off.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a steel bar carbonization rust-proof coating material capable of resisting chloride ions and a coating process thereof, and belongs to the field of steel bar anti-corrosion materials. Background Art

[0002] Chloride ions, as one of the main corrosive ions in seawater, pose a serious threat to reinforced concrete structures built in marine engineering. Due to the erosion of chloride ions, steel bars are prone to rust, thereby reducing the durability and safety of concrete structures. Chloride ions can cause pitting of steel bars, which then develop into cracks, and concrete can crack and peel, reducing the bearing capacity of the overall structure and affecting normal use.

[0003] Steel bar corrosion prevention measures include concrete densification, concrete surface coating, steel bar cathodic protection and rust inhibitors. Among them, an important research direction of steel bar rust prevention is the development and utilization of steel bar rust prevention coatings. Steel bar coatings protect steel bars from corrosion by blocking chloride ions from contacting the steel bar surface. Existing steel bar coatings include organic coatings and inorganic coatings, but they generally have the problem of aging and peeling off from the surface due to long-term use, and the rust prevention performance needs to be further improved. Therefore, the development of a steel bar coating with high-efficiency rust prevention performance has become an urgent problem to be solved. Summary of the invention

[0004] The invention provides a steel bar carbonization rust-proof coating material resistant to chloride ions, which can solve the problem of reduced service life caused by corrosion of steel bars in a chloride salt environment, and can significantly improve the corrosion resistance of steel bars and extend their service life.

[0005] The present invention also provides a coating process for the above-mentioned steel bar carbonization rust-proof coating material capable of resisting chloride ions.

[0006] The technical solution adopted by the present invention to achieve the above-mentioned purpose is: The present invention provides a steel bar carbonization rust-proof coating material resistant to chloride ions, which is composed of component a and component b; The component a is composed of the following raw materials in parts by weight: 1) Inorganic gelling material a: 96~97 parts Early strength agent: 2~4 parts Water reducing agent: 0.1~0.5 parts; The component b is composed of the following raw materials in parts by weight: 2) Inorganic gelling material b: 97~98 parts Early strength agent: 1~3 parts Water reducing agent: 0.1~0.5 parts.

[0007] Furthermore, the inorganic cementitious material a is composed of phosphate aluminate cement and other gel components; the other cementitious materials are one or a combination of aluminate, sulphoaluminate and ferroaluminate cement.

[0008] Furthermore, the mass ratio of the aluminophosphate cement, aluminate, aluminoferrate cement and sulphoaluminate is 20-40:15-30:10-30:5-25.

[0009] Furthermore, the inorganic cementitious material b is composed of phosphate aluminate cement and carbon-fixing cementitious material components; the carbon-fixing cementitious material is one or a combination of CS, C3S2, and γ-C2S.

[0010] Furthermore, in the inorganic gelling material b, the mass ratio of the phosphate aluminate cement, CS, C3S2 and γ-C2S is 40~60:10~30:10~20:5~15.

[0011] Furthermore, the early strength agent is one or a combination of calcium nitrate, calcium nitrite, sodium sulfate, and sodium borate; and the water reducer is one or a combination of polycarboxylic acid, naphthalene, and fatty acid salt water reducers.

[0012] Furthermore, in the inorganic cementitious material a and the inorganic cementitious material b, the phosphate aluminate cement is fired from industrial raw materials, and its mineral phase composition is as follows: Calcium phosphate aluminate: 20~30 parts Tricalcium phosphate: 15~20 parts Calcium aluminate: 40~50 parts Magnesium aluminum spinel: 10~20 parts Furthermore, the mass fractions of the aluminophosphate cement, CS, C3S2 and γ-C2S are as follows: Aluminophosphate cement: Bauxite: 30~35 parts Apatite: 15~20 parts Limestone: 35~40 parts Hematite: 10~15 parts CS: Limestone: 60~65 parts Gold tailings: 35~40 parts C3S2: Limestone: 70~75 parts Gold tailings: 25~30 parts γ-C2S: Limestone: 75~80 parts Gold tailings: 20~25 parts.

[0013] The present invention also provides a coating process using the above steel bar rust-proof coating material, comprising the following steps: (1) Add the early strength agent and water reducing agent in component a in parts by weight to the inorganic gelling material a, add water according to a certain water-solid ratio, and use it as an inner layer of rust-proof coating, evenly brush it on the cleaned steel bar surface, and wait for it to solidify; (2) Add the weight parts of early strength agent and water reducing agent in component b to the inorganic gelling material b, add water according to a certain water-solid ratio, use it as the outer rust-proof coating, apply the outer layer to the solidified inner layer, and wait for it to solidify; (3) The coated steel bars can then be carbonized and cured. Furthermore, in steps (1) and (2), the water-solid ratio is 0.3-0.5; in step (3), the carbonization curing conditions are: controlling the CO2 gas pressure to 0.2 MPa, the temperature to 25°C, and the carbonization time to 24 hours.

[0014] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses cement as the main material of the steel bar rust-proof coating. On the one hand, the coating can have a longer service life and will not age. On the other hand, phosphate aluminate cement will not have adverse effects on the steel bars.

[0015] 2. The present invention adopts phosphate aluminate cement as the constituent phase, and the prepared coating has good performance in solidifying chloride ions. At the same time, CS, C3S2, and γ-C2S are easy to carbonize, and the density is improved after carbonization, which can make the coating structure denser and thus block the penetration of chloride ions. The two work synergistically to effectively play a rust-proof role.

[0016] 3. The coating provided by the present invention has good adhesion and viscosity. When used in a chloride salt environment, it can not only play a good role in fixing chlorine, but also play a role similar to that of an adhesive, making the rust-resistant coating less prone to aging and peeling. DETAILED DESCRIPTION

[0017] The present invention provides a preparation method for a steel bar rust-proof coating material capable of resisting chloride ions, which is prepared from the following raw materials: The inorganic cementitious material a is one or more of phosphate aluminate cement, aluminate cement, ferroaluminate cement and sulphoaluminate cement.

[0018] The inorganic gelling material b is one or more of phosphate aluminate cement, CS, C3S2, and γ-C2S.

[0019] The CS, C3S2, and γ-C2S compositions include limestone and gold tailings; In the present invention, the materials and equipment used are all commercially available products in the art.

[0020] In the present invention, when the inorganic gelling material a in the steel bar coating material is composed of phosphate aluminate cement, aluminate cement, ferroaluminate cement, and sulphoaluminate cement, the mass ratio is preferably 20-40:15-30:10-30:5-25; more preferably 35-40:20-25:15-20:15-25; and most preferably 40:20:15:25. When the inorganic gelling material b in the steel bar coating material is composed of PAC, CS, C3S2, and γ-C2S, the mass ratio is preferably 40-60:10-30:10-20:5-15, more preferably 50-55:15-20:20-25:5-10; and most preferably 55:15:20:10. The coating material obtained by using the mass ratio can meet the requirements of steel bar corrosion protection.

[0021] In the inorganic gelling material a provided by the present invention, the preparation method of aluminophosphate cement comprises: (1) Weigh a certain amount of formula, pour it into a ball mill, add an appropriate amount of water, and use a ball mill to wet mix it and mix it thoroughly.

[0022] (2) Pour the mixed raw material into a previously cleaned plate, and then place it in a constant temperature drying oven at 60°C for drying. Take out the dried raw material, add an appropriate amount of deionized water to wet it, use a mold to shape the raw material powder into raw material cakes, and then place the raw material cakes in a drying oven at 55°C for drying.

[0023] (3) Place the dried raw material cake into a high-temperature furnace for calcination, set the sintering temperature to 1380°C, and keep it warm for 2 hours.

[0024] (4) The calcined aluminophosphate cement clinker is taken out and rapidly cooled, and then crushed to obtain clinker blocks. The clinker blocks are then ground into fine powder, and the ground clinker powder is passed through a 200-mesh sieve to obtain cement clinker.

[0025] In the inorganic gelling material b provided by the present invention, the preparation method of CS comprises: (1) Take 60-65 parts of limestone and 35-40 parts of gold tailings, add appropriate amount of water and mix well.

[0026] (2) The mixed material is formed and calcined to 1500°C and kept at this temperature for 180 min, then rapidly cooled and ground into powder.

[0027] In the inorganic gelling material b provided by the present invention, the preparation method of C3S2 comprises: (1) Take 70-75 parts of limestone and 25-30 parts of gold tailings, add appropriate amount of water and mix well.

[0028] (2) The mixed material is formed and calcined to 1440°C and kept at this temperature for 180 min, then rapidly cooled and ground into powder.

[0029] In the inorganic gelling material b provided by the present invention, the preparation method of γ-C2S comprises: (1) Take 75-80 parts of limestone and 20-25 parts of gold tailings, add appropriate amount of water and mix well.

[0030] (2) The mixed material is formed and calcined to 1450°C and kept at this temperature for 180 min, then rapidly cooled and ground into powder.

[0031] In the present invention, there is no special requirement for the raw materials used, and the raw materials commonly used in the construction industry can be selected.

[0032] The present invention will be further described below in conjunction with examples. The following examples are only used to more clearly illustrate the technical solutions of the present invention and are not intended to limit the protection scope of the present invention.

[0033] Example 1 Component a: Weigh a certain amount of raw materials according to the mass ratio of 36:23:18:23 = phosphate aluminate cement: aluminate cement: ferroaluminate cement: sulphoaluminate cement; Component b: Weigh a certain amount of raw materials according to the mass ratio of 52:17:21:10=PAC:CS:C3S2:γ-C2S.

[0034] The coating preparation process is as follows: 1) Brush the surface of the steel bar to remove rust, oil stains and dust on the surface to ensure that the surface of the steel bar is clean and flat.

[0035] 2) Component a: Add water to the inorganic cementitious material a at a water-cement ratio of 0.4, and add 2% calcium nitrate and calcium nitrite (the mass ratio of calcium nitrate and calcium nitrite is 1:1) and 0.3% polycarboxylic acid, mix them well to form an inner rust-resistant coating, and evenly apply the prepared inner rust-resistant coating on the cleaned steel bar surface.

[0036] 3) Component b: Mix the inorganic gelling material b according to a certain mass fraction, add 3% sodium sulfate, 0.3% polycarboxylic acid, add appropriate amount of water according to the water-solid ratio of 0.4 and mix well to make the outer rust-proof coating. After the inner rust-proof coating is solidified, apply the outer rust-proof coating, and then perform carbonization curing to make the coating dense.

[0037] 4) Connect the CO2 cylinder to the carbonization kettle, first pass CO2 for 2 minutes to exhaust the air in the kettle, then put the painted test block into the reactor, and pass CO2 gas for carbonization curing. Set the CO2 gas pressure in the carbonization kettle to 0.2MPa, the temperature to 20℃, and the carbonization time to 24h.

[0038] Example 2 Component a: Weigh a certain amount of raw materials according to the mass ratio of 32:25:19:24 = phosphate aluminate cement: aluminate cement: ferroaluminate cement: sulphoaluminate cement; Component b: Weigh a certain amount of raw materials according to the mass ratio of 54:16:23:7=PAC:CS:C3S2:γ-C2S.

[0039] Different from Example 1, in the coating preparation process, the water-cement ratio of the inorganic gelling material a is set to 0.3, the early strength agent in the inorganic gelling material b is sodium borate and sodium sulfate (the mass ratio of sodium borate to sodium sulfate is 2:1), the dosage is 4%, and the water reducer is a naphthalene-based high-concentration water reducer, the dosage is 0.2%. The CO2 gas pressure in the carbonization kettle is set to 0.1MPa, the temperature is 20°C, and the carbonization time is 24h.

[0040] Example 3 Component a: Weigh a certain amount of raw materials according to the mass ratio of 35:21:16:28 = phosphate aluminate cement: aluminate cement: ferroaluminate cement: sulphoaluminate cement; Component a: Weigh a certain amount of raw materials according to the mass ratio of 50:18:24:8=PAC:CS:C3S2:γ-C2S.

[0041] Different from Example 1, in the coating preparation process, the water-solid ratio of the inorganic gelling material b is set to 0.5, the early strength agent in the inorganic gelling material b is calcium nitrate and calcium nitrite (the mass ratio of calcium nitrate to calcium nitrite is 1:1), the dosage is 2%, and the water reducing agent is fatty acid salt, the dosage is 0.4%. The CO2 gas pressure in the carbonization kettle is set to 0.2MPa, the temperature is 30°C, and the carbonization time is 24h.

[0042] Example 4 Component a: Weigh a certain amount of raw materials according to the mass ratio of 40:20:15:25 = phosphate aluminate cement: aluminate cement: ferroaluminate cement: sulphoaluminate cement; Component b: Weigh a certain amount of raw materials according to the mass ratio of 55:15:20:10=PAC:CS:C3S2:γ-C2S.

[0043] Different from Example 1, in the coating preparation process, the water-cement ratio of the inorganic gelling material a is set to 0.3, the early strength agent in the inorganic gelling material a is sodium borate and sodium sulfate (the mass ratio of sodium borate to sodium sulfate is 2:1), the dosage is 4%, the water reducer is a naphthalene-based high-concentration water reducer, the dosage is 0.2%, and the early strength agent in the inorganic gelling material b is sodium borate, the dosage is 2%. The CO2 gas pressure in the carbonization kettle is set to 0.2MPa, the temperature is 25°C, and the carbonization time is 24h.

[0044] Comparative Example 1 Component a: Weigh a certain amount of raw materials according to the mass ratio of 40:20:15:25 = phosphate aluminate cement: aluminate cement: ferroaluminate cement: sulphoaluminate cement; Component b: Weigh a certain amount of raw materials according to the mass ratio of 55:15:20:10=PAC:CS:C3S2:γ-C2S.

[0045] Different from Example 1, in the coating preparation process, the water-cement ratio of the inorganic gelling material a is set to 0.3, the early strength agents used are sodium borate and sodium sulfate, the ratio of the two is 2:1, and the dosage is 4%; the early strength agent in the inorganic gelling material b is sodium borate, and the dosage is 2%; the CO2 gas pressure in the carbonization kettle is 0.2MPa, the temperature is 25°C, and the carbonization time is 24h.

[0046] The inorganic gelling material a is used as the outer coating, and the inorganic gelling material b is used as the inner coating.

[0047] Comparative Example 2 Component a: Weigh a certain amount of raw materials according to the mass ratio of 60:40 = phosphate aluminate cement: sulphoaluminate cement; Component b: Weigh a certain amount of raw materials according to the mass ratio of 55:45 = C3S2:γ-C2S.

[0048] Different from Example 1, in the coating preparation process, the water-cement ratio of the inorganic gelling material a is set to 0.3, and the early strength agent used is sodium borate with an addition amount of 3%; the early strength agent in the inorganic gelling material b is calcium nitrate with an addition amount of 2%; the CO2 gas pressure in the carbonization kettle is 0.2MPa, the temperature is 25°C, and the carbonization time is 24h.

[0049] Effect Example The coating materials prepared in Examples 1-4 and the comparative examples were tested for performance according to GB / T 17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)" and JGJ / T 322-2013 "Technical Code for Detection of Chloride Ion Content in Concrete". The specific results are shown in Table 1.

[0050] Table 1

Claims

1. A steel bar carbonization rust-proof coating material resistant to chloride ions, It is characterized in that Composed of component a and component b; The component a is composed of the following raw materials in parts by weight: 1) Inorganic gelling material a: 96~97 parts Early strength agent: 2~4 parts Water reducing agent: 0.1~0.5 parts; The component b is composed of the following raw materials in parts by weight: 2) Inorganic gelling material b: 97~98 parts Early strength agent: 1~3 parts Water reducing agent: 0.1~0.5 parts.

2. The steel bar carbonization rust-proof coating material according to claim 1, It is characterized in that The inorganic cementitious material a is composed of phosphate aluminate cement and other gel components; the other cementitious materials are one or a combination of aluminate, sulphoaluminate and ferroaluminate cement.

3. The steel bar carbonization rust-proof coating material according to claim 2, It is characterized in that The mass ratio of the aluminophosphate cement, aluminate, aluminoferrate cement and sulphoaluminate is 20-40:15-30:10-30:5-25.

4. The steel bar carbonization rust-proof coating material according to claim 1, It is characterized in that The inorganic cementitious material b is composed of phosphate aluminate cement and carbon-fixing cementitious material components; the carbon-fixing cementitious material is one or a combination of CS, C3S2, and γ-C2S.

5. The steel bar carbonization rust-proof coating material according to claim 4, It is characterized in that In the inorganic gelling material b, the mass ratio of the phosphate aluminate cement, CS, C3S2 and γ-C2S is 40~60:10~30:10~20:5~15.

6. The steel bar carbonization rust-proof coating material according to claim 1, It is characterized in that The early strength agent is one or a combination of calcium nitrate, calcium nitrite, sodium sulfate, sodium borate; the water reducer is one or a combination of polycarboxylic acid, naphthalene series, fatty acid salt water reducers.

7. The steel bar carbonization rust-proof coating material according to any one of claims 2 to 5, It is characterized in that In the inorganic cementitious material a and the inorganic cementitious material b, the phosphate aluminate cement is made by burning industrial raw materials, and its mineral phase composition is as follows: Calcium phosphate aluminate: 20~30 parts Tricalcium phosphate: 15~20 parts Calcium aluminate: 40~50 parts Magnesium aluminum spinel: 10~20 parts.

8. The steel bar carbonization rust-proof coating material according to claim 1, It is characterized in that The mass fractions of the aluminophosphate cement, CS, C3S2 and γ-C2S are as follows: Aluminophosphate cement: Bauxite: 30~35 parts Apatite: 15~20 parts Limestone: 35~40 parts Hematite: 10~15 parts CS: Limestone: 60~65 parts Gold tailings: 35~40 parts C3S2: Limestone: 70~75 parts Gold tailings: 25~30 parts γ-C2S: Limestone: 75~80 parts Gold tailings: 20~25 parts.

9. A coating process using the steel bar rust-proof coating material according to any one of claims 1 to 7, It is characterized in that The steps include: (1) Add the early strength agent and water reducing agent in component a in parts by weight to the inorganic gelling material a, add water according to a certain water-solid ratio, and use it as an inner layer of rust-proof coating, evenly brush it on the cleaned steel bar surface, and wait for it to solidify; (2) Add the weight parts of early strength agent and water reducing agent in component b to the inorganic gelling material b, add water according to a certain water-solid ratio, use it as the outer rust-proof coating, apply the outer layer to the solidified inner layer, and wait for it to solidify; (3) The coated steel bars can then be carbonized and cured.

10. The coating process according to claim 8, It is characterized in that In steps (1) and (2), the water-solid ratio is 0.3-0.5; in step (3), the carbonization curing conditions are: controlling the CO2 gas pressure to 0.2 MPa, the temperature to 25°C, and the carbonization time to 24 hours.

Citation Information

Patent Citations

  • Exposed reinforcing steel bar rust-proof cement paste in building construction and processing method

    CN102718454A

  • Autogenously-pulverizable low calcium cement, and making method of prefabricated products thereof

    CN105347706A

  • High-corrosion-resistance maritime work cementing material as well as preparation method and application thereof

    CN111704419A