Long-acting steel structure anticorrosive paint and preparation method thereof

By optimizing the formula and process of anti-corrosion coatings and combining components such as oxygen resin and zinc phosphate, the problems of high cost and unstable performance of traditional anti-corrosion coatings are solved, achieving high cost performance and excellent anti-corrosion performance, and is suitable for a variety of steel structure projects.

CN118745312APending Publication Date: 2024-10-08SICHUAN PINZHONG STEEL STRUCTURE CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410874329.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing anti-corrosion coatings have high costs, unstable performance and poor environmental protection, making it difficult to promote and apply them in more fields, especially for the protection of steel structures with large dynamic loads.

Method used

Using components such as oxygen resin, zinc phosphate and aluminum tripolyphosphate, and optimizing the formula and process, a long-lasting anti-corrosion coating for steel structures is prepared, including 20%-30% of oxygen resin, 2%-5% of coloring pigments, and Pigment 30%-40%, special anti-rust pigment 10%-20%, solvent 10%-15%, additive 1%-3%, curing agent 8%-12%, and adjust the viscosity and Fineness.

Benefits of technology

It reduces the cost of anti-corrosion coatings, improves cost performance, provides high anti-corrosion performance, good adhesion and corrosion resistance, is suitable for various harsh environments, meets environmental protection requirements, and is suitable for a variety of steel structure projects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745312A_ABST
    Figure CN118745312A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of anticorrosive paint, and discloses long-acting steel structure anticorrosive paint which comprises the following components in percentage by weight: 20-30% of oxygen resin, 2-5% of tinting pigment, 30-40% of extender pigment, 10-20% of special antirust pigment, 10-15% of solvent, 1-3% of assistant and 8-12% of curing agent. The invention also discloses a preparation method of the long-acting steel structure anticorrosive paint, which comprises the following steps: a) adding the epoxy resin, the tinting pigment and the extender pigment into the solvent, and uniformly stirring; b) grinding until the fineness of the coating is less than 50 microns; and c) adding an auxiliary agent while stirring, and continuously stirring. Zinc phosphate and aluminum triphosphate are used for replacing part of zinc powder, meanwhile, a more economical epoxy resin and solvent formula is adopted, the cost of the anti-corrosion coating is greatly reduced, through reasonable formula design, the coating has high anti-corrosion performance, meanwhile, the cost is relatively low, the cost performance of a product is improved, and the application prospect is wide. And more steel structure projects can bear the anti-corrosion treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anti-corrosion coatings, and in particular to a long-lasting anti-corrosion coating for steel structures and a preparation method thereof. Background Art

[0002] Anti-corrosion coatings refer to a type of liquid or solid material that can form a thin film under certain conditions when applied to the surface of an object to provide protection. During the use of the main steel structure components in various projects, the surface will be subjected to harsh environmental erosion and load for a long time, and its performance will inevitably decline over time. The use of anti-corrosion coatings can play an anti-corrosion role and protect the service life of non-ferrous metals.

[0003] Existing anti-corrosion coatings mainly include epoxy zinc-rich primers, inorganic zinc-rich primers, acrylic anti-corrosion coatings, etc., but these traditional anti-corrosion coatings have certain defects and shortcomings. First, the cost of traditional anti-corrosion primers is relatively high, and it is difficult to be promoted in a wider range of application fields; second, the performance of traditional anti-corrosion coatings is unstable and requires multiple repairs and maintenance during use. In addition, the coating also needs to have environmentally friendly and safe characteristics to avoid environmental pollution and protect the physical and mental health of construction workers, in line with national requirements for environmental protection.

[0004] Epoxy zinc-rich primer is widely used in the protection of steel structures due to its excellent anti-corrosion performance. However, its high cost and certain impact on the environment limit its promotion and application in some fields. Although the price of inorganic zinc-rich primer is relatively low, its construction performance is poor and the coating is brittle, so it is not suitable for the protection of some steel structures with large dynamic loads.

[0005] In view of the problems and shortcomings of the prior art, the present invention provides a long-lasting anti-corrosion coating for steel structures and a preparation method thereof. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a long-lasting anti-corrosion coating for steel structures and a preparation method thereof, which solves the problems of high cost, unstable performance and poor environmental protection of traditional anti-corrosion coatings.

[0007] To achieve the above objectives, the present invention is implemented through the following technical scheme: a long-lasting anti-corrosion coating for steel structures, comprising the following components by weight percentage: 20%-30% epoxy resin, 2%-5% coloring pigment, 30%-40% body pigment, 10%-20% special anti-rust pigment, 10%-15% solvent, 1%-3% additive, and 8%-12% curing agent.

[0008] Preferably, the auxiliary agent includes a dispersant and an adhesion promoter.

[0009] Preferably, the special anti-rust pigment consists of zinc phosphate and aluminum tripolyphosphate in a weight ratio of 2:1.

[0010] A method for preparing a long-lasting anticorrosive coating for steel structures comprises the following steps:

[0011] a) Add epoxy resin, coloring pigment and extender pigment into the solvent and stir evenly;

[0012] b) Grinding to make the coating fineness less than 50μm;

[0013] c) Add the additive while stirring and continue stirring;

[0014] d) Add curing agent under stirring and adjust the viscosity to less than 6000 cP;

[0015] e) Packaging after filtration

[0016] Preferably, the step a specifically comprises the following steps:

[0017] a1. Raw material preparation:

[0018] Weigh epoxy resin, coloring pigment, extender pigment and solvent according to proportion;

[0019] a2. Mixed:

[0020] Add epoxy resin to the stirring device;

[0021] Gradually add coloring pigments and extender pigments;

[0022] Finally, the solvent is added;

[0023] a3. Stirring:

[0024] Use a high-speed mixer to stir for at least 30 minutes until the mixture is uniform.

[0025] Preferably, the step b specifically includes the following steps:

[0026] b1. Grinding equipment:

[0027] Use a bead mill;

[0028] b2. Grinding process:

[0029] Pour the well-stirred coating mixture into a bead mill;

[0030] Set appropriate grinding parameters and the grinding time is 1-2h;

[0031] Grind until the paint fineness reaches less than 50μm.

[0032] Preferably, the step c specifically includes the following steps:

[0033] c1. Preparation of additives:

[0034] Weigh the required additives according to the formula, including dispersants and adhesion promoters;

[0035] c2. Adding additives:

[0036] Add the additive gradually to the ground coating;

[0037] c3. Continue stirring:

[0038] Continue stirring for 25-35 minutes to ensure that the additive and the coating are fully mixed.

[0039] Preferably, the step d specifically comprises the following steps:

[0040] d1. Preparation of curing agent:

[0041] Weigh the required curing agent according to the formula;

[0042] d2. Add curing agent:

[0043] Gradually add the curing agent to the stirring paint;

[0044] d3. Adjust viscosity:

[0045] Continue stirring until the viscosity of the coating is adjusted to less than 6000cP;

[0046] Measure viscosity regularly using a viscometer to ensure requirements are met.

[0047] The present invention provides a long-lasting steel structure anticorrosion coating and a preparation method thereof. It has the following beneficial effects:

[0048] 1. The present invention uses zinc phosphate and aluminum tripolyphosphate to replace part of the zinc powder, and adopts a more economical epoxy resin and solvent formula, which greatly reduces the cost of the anti-corrosion coating. Moreover, through reasonable formula design, the coating has high anti-corrosion performance and relatively low cost, which improves the cost performance of the product and enables more steel structure projects to afford anti-corrosion treatment.

[0049] 2. The present invention not only provides excellent anti-rust effect by using zinc phosphate and aluminum tripolyphosphate, but also forms excellent adhesion and corrosion resistance with epoxy resin, ensuring the long-term anti-corrosion requirements of steel structures in harsh environments.

[0050] 3. The present invention effectively improves the salt spray resistance of the epoxy anticorrosion primer by adding zinc, aluminum and magnesium compounds. Compared with the traditional epoxy zinc-rich primer, the anticorrosion performance is close to or even better than the traditional products. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0052] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0053] Please see attached Figure 1 The embodiment of the present invention provides a long-lasting anti-corrosion coating for steel structures, which includes the following components by weight percentage: 20%-30% epoxy resin, 2%-5% coloring pigment, 30%-40% body pigment, 10%-20% special anti-rust pigment, 10%-15% solvent, 1%-3% additive, and 8%-12% curing agent.

[0054] Additives include dispersants and adhesion promoters.

[0055] The special anti-rust pigment is composed of zinc phosphate and aluminum tripolyphosphate in a weight ratio of 2:1.

[0056] A method for preparing a long-lasting anticorrosive coating for steel structures comprises the following steps:

[0057] a) Add epoxy resin, coloring pigment and extender pigment into the solvent and stir evenly;

[0058] b) Grinding to make the coating fineness less than 50μm;

[0059] c) Add the additive while stirring and continue stirring;

[0060] d) Add curing agent under stirring and adjust the viscosity to less than 6000 cP;

[0061] e) Packaging after filtering.

[0062] Step a specifically includes the following steps:

[0063] a1. Raw material preparation:

[0064] Weigh epoxy resin, coloring pigment, extender pigment and solvent according to proportion;

[0065] a2. Mixed:

[0066] Add epoxy resin to the stirring device;

[0067] Gradually add coloring pigments and extender pigments;

[0068] Finally, the solvent is added;

[0069] a3. Stirring:

[0070] The mixture is stirred with a high-speed mixer for not less than 30 minutes until the mixture is uniform. Step b specifically includes the following steps:

[0071] b1. Grinding equipment:

[0072] Use a bead mill;

[0073] b2. Grinding process:

[0074] Pour the well-stirred coating mixture into a bead mill;

[0075] Set appropriate grinding parameters and the grinding time is 1-2h;

[0076] Grind until the paint fineness reaches less than 50μm.

[0077] Step c specifically includes the following steps:

[0078] c1. Preparation of additives:

[0079] Weigh the required additives according to the formula, including dispersants and adhesion promoters;

[0080] c2. Adding additives:

[0081] Add the additive gradually to the ground coating;

[0082] c3. Continue stirring:

[0083] Continue stirring for 25-35 minutes to ensure that the additive and the coating are fully mixed.

[0084] Step d specifically includes the following steps:

[0085] d1. Preparation of curing agent:

[0086] Weigh the required curing agent according to the formula;

[0087] d2. Add curing agent:

[0088] Gradually add the curing agent to the stirring paint;

[0089] d3. Adjust viscosity:

[0090] Continue stirring until the viscosity of the coating is adjusted to less than 6000cP;

[0091] Measure viscosity regularly using a viscometer to ensure requirements are met.

[0092] Embodiment 1:

[0093] Recipe composition:

[0094] Epoxy resin: 20%

[0095] Coloring Pigment: 2%

[0096] Body pigment: 30%

[0097] Special anti-rust pigment: 10% (weight ratio of zinc phosphate to aluminum tripolyphosphate is 2:1)

[0098] Solvent: 15%

[0099] Additives: 3% (dispersant and adhesion promoter)

[0100] Curing agent: 10%

[0101] Preparation steps:

[0102] a) Raw material preparation:

[0103] Weigh epoxy resin, coloring pigment, extender pigment and solvent according to proportion.

[0104] b) Mixing:

[0105] Add epoxy resin to the stirring device.

[0106] Gradually add coloring pigments and extenders.

[0107] The solvent is added last.

[0108] Blend in a high-speed blender for at least 30 minutes until the mixture is smooth.

[0109] c) Grinding:

[0110] Grind using a bead mill.

[0111] The uniformly stirred coating mixture is poured into a bead mill and ground for 1 hour until the coating fineness reaches less than 50 microns.

[0112] d) Adding additives:

[0113] Weigh the required additives according to the formula, including dispersants and adhesion promoters.

[0114] Gradually add the additives to the ground paint and continue stirring for 30 minutes to ensure that the additives and paint are fully mixed.

[0115] e) Add curing agent:

[0116] Weigh the required curing agent according to the formula.

[0117] Gradually add the curing agent to the stirring coating and continue stirring until the viscosity of the coating is adjusted to less than 6000 centipoise.

[0118] Measure viscosity regularly using a viscometer to ensure requirements are met.

[0119] f) Filtration and packaging:

[0120] Filter the paint using a 200 mesh filter to remove undispersed particles and impurities.

[0121] Put the filtered paint into a clean paint bucket and seal it.

[0122] Summarize:

[0123] This embodiment produces a highly efficient and economical anti-corrosion coating by optimizing the formula and simplifying the preparation process, which is suitable for the anti-corrosion protection of various steel structures.

[0124] Embodiment 2:

[0125] Recipe composition:

[0126] Epoxy resin: 25%

[0127] Coloring Pigment: 3%

[0128] Extender Pigment: 35%

[0129] Special anti-rust pigment: 12% (weight ratio of zinc phosphate to aluminum tripolyphosphate is 2:1)

[0130] Solvent: 12%

[0131] Additives: 2% (dispersant and adhesion promoter)

[0132] Curing agent: 11%

[0133] Preparation steps:

[0134] a) Raw material preparation:

[0135] Weigh epoxy resin, coloring pigment, extender pigment and solvent according to proportion.

[0136] b) Mixing:

[0137] Add epoxy resin to the stirring device.

[0138] Gradually add coloring pigments and extenders.

[0139] The solvent is added last.

[0140] Blend in a high-speed blender for at least 30 minutes until the mixture is smooth.

[0141] c) Grinding:

[0142] Grind using a bead mill.

[0143] The uniformly stirred coating mixture was poured into a bead mill and ground for 1.5 hours until the coating fineness reached less than 50 microns.

[0144] d) Adding additives:

[0145] Weigh the required additives according to the formula, including dispersants and adhesion promoters.

[0146] Gradually add the additives to the ground paint and continue stirring for 30 minutes to ensure that the additives and paint are fully mixed.

[0147] e) Add curing agent:

[0148] Weigh the required curing agent according to the formula.

[0149] Gradually add the curing agent to the stirring coating and continue stirring until the viscosity of the coating is adjusted to less than 6000 centipoise.

[0150] Measure viscosity regularly using a viscometer to ensure requirements are met.

[0151] f) Filtration and packaging:

[0152] Filter the paint using a 200 mesh filter to remove undispersed particles and impurities.

[0153] Put the filtered paint into a clean paint bucket and seal it.

[0154] Summarize:

[0155] This embodiment uses a medium ratio of epoxy resin and additives, and further improves the anti-corrosion performance and workability of the coating by properly adjusting the grinding time and the ratio of additives.

[0156] Embodiment 3:

[0157] Recipe composition:

[0158] Epoxy resin: 30%

[0159] Coloring Pigment: 4%

[0160] Extender Pigment: 38%

[0161] Special anti-rust pigment: 15% (weight ratio of zinc phosphate to aluminum tripolyphosphate is 2:1)

[0162] Solvent: 10%

[0163] Additives: 1% (dispersant and adhesion promoter)

[0164] Curing agent: 12%

[0165] Preparation steps:

[0166] a) Raw material preparation:

[0167] Weigh epoxy resin, coloring pigment, extender pigment and solvent according to proportion.

[0168] b) Mixing:

[0169] Add epoxy resin to the stirring device.

[0170] Gradually add coloring pigments and extenders.

[0171] The solvent is added last.

[0172] Blend in a high-speed blender for at least 30 minutes until the mixture is smooth.

[0173] c) Grinding:

[0174] Grind using a bead mill.

[0175] The uniformly stirred coating mixture is poured into a bead mill and ground for 2 hours until the coating fineness reaches less than 50 microns.

[0176] d) Adding additives:

[0177] Weigh the required additives according to the formula, including dispersants and adhesion promoters.

[0178] Gradually add the additives to the ground paint and continue stirring for 35 minutes to ensure that the additives are fully mixed with the paint.

[0179] e) Add curing agent:

[0180] Weigh the required curing agent according to the formula.

[0181] Gradually add the curing agent to the stirring coating and continue stirring until the viscosity of the coating is adjusted to less than 6000 centipoise.

[0182] Measure viscosity regularly using a viscometer to ensure requirements are met.

[0183] f) Filtration and packaging:

[0184] Filter the paint using a 200 mesh filter to remove undispersed particles and impurities.

[0185] Put the filtered paint into a clean paint bucket and seal it.

[0186] Summarize:

[0187] The ratio of epoxy resin to curing agent in this embodiment is the highest, which makes the coating have stronger adhesion and durability and is suitable for use in harsh environments.

[0188] Embodiment 4:

[0189] Recipe composition:

[0190] Epoxy resin: 22%

[0191] Coloring Pigment: 3%

[0192] Extender Pigment: 32%

[0193] Special anti-rust pigment: 18% (weight ratio of zinc phosphate to aluminum tripolyphosphate is 2:1)

[0194] Solvent: 12%

[0195] Additives: 2% (dispersant and adhesion promoter)

[0196] Curing agent: 11%

[0197] Preparation steps

[0198] a) Raw material preparation:

[0199] Weigh epoxy resin, coloring pigment, extender pigment and solvent according to proportion.

[0200] b) Mixing:

[0201] Add epoxy resin to the stirring device.

[0202] Gradually add coloring pigments and extenders.

[0203] The solvent is added last.

[0204] Blend in a high-speed blender for at least 30 minutes until the mixture is smooth.

[0205] c) Grinding:

[0206] Grind using a bead mill.

[0207] The uniformly stirred coating mixture was poured into a bead mill and ground for 1.5 hours until the coating fineness reached less than 50 microns.

[0208] d) Adding additives:

[0209] Weigh the required additives according to the formula, including dispersants and adhesion promoters.

[0210] Gradually add the additives to the ground paint and continue stirring for 30 minutes to ensure that the additives are fully mixed with the paint.

[0211] e) Add curing agent:

[0212] Weigh the required curing agent according to the formula.

[0213] Gradually add the curing agent to the stirring coating and continue stirring until the viscosity of the coating is adjusted to less than 6000 centipoise.

[0214] Measure viscosity regularly using a viscometer to ensure requirements are met.

[0215] f) Filtration and packaging:

[0216] Filter the paint using a 200 mesh filter to remove undispersed particles and impurities.

[0217] Put the filtered paint into a clean paint bucket and seal it.

[0218] Summarize:

[0219] In this embodiment, the proportion of the anti-rust pigment is increased, the anti-corrosion performance of the coating is improved, and it is suitable for the protection of steel structures in high humidity and high salt environments.

[0220] Embodiment 5:

[0221] Recipe composition:

[0222] Epoxy resin: 28%

[0223] Coloring Pigment: 4%

[0224] Extender Pigment: 36%

[0225] Special anti-rust pigment: 12% (weight ratio of zinc phosphate to aluminum tripolyphosphate is 2:1)

[0226] Solvent: 10%

[0227] Additives: 1% (dispersant and adhesion promoter)

[0228] Curing agent: 9%

[0229] Preparation steps:

[0230] a) Raw material preparation:

[0231] Weigh epoxy resin, coloring pigment, extender pigment and solvent according to proportion.

[0232] b) Mixing:

[0233] Add epoxy resin to the stirring device.

[0234] Gradually add coloring pigments and extenders.

[0235] The solvent is added last.

[0236] Use a high-speed blender to stir for at least 30 minutes until the mixture is homogeneous.

[0237] c) Grinding:

[0238] Grind using a bead mill.

[0239] The uniformly stirred coating mixture is poured into a bead mill and ground for 1 hour until the coating fineness reaches less than 50 microns.

[0240] d) Adding additives:

[0241] Weigh the required additives according to the formula, including dispersants and adhesion promoters.

[0242] Gradually add the additives to the ground paint and continue stirring for 25 minutes to ensure that the additives are fully mixed with the paint.

[0243] e) Add curing agent:

[0244] Weigh the required curing agent according to the formula.

[0245] Gradually add the curing agent to the stirring coating and continue stirring until the viscosity of the coating is adjusted to less than 6000 centipoise.

[0246] Measure viscosity regularly using a viscometer to ensure requirements are met.

[0247] f) Filtration and packaging:

[0248] Filter the paint using a 200 mesh filter to remove undispersed particles and impurities.

[0249] Put the filtered paint into a clean paint bucket and seal it.

[0250] Summarize:

[0251] This embodiment optimizes the ratio of additives and grinding time so that the coating has excellent construction performance and high anti-corrosion performance, and is suitable for steel structure protection in complex construction environments.

[0252] Summary:

[0253] The above five examples demonstrate the diversified applications of the coating of the present invention in terms of cost, performance, workability and applicable environment through different formulations and process parameter adjustments. Each example achieves the purpose of optimizing specific performance by fine-tuning the proportions of different components and operating steps while maintaining the basic formulation. Overall, the coating of the present invention has the following advantages:

[0254] High cost performance: effectively reduce raw material costs and improve product economy.

[0255] Excellent anti-corrosion performance: Provides long-term anti-corrosion protection, suitable for various harsh environments.

[0256] Environmental protection and safety: Use environmentally friendly raw materials to comply with national environmental protection requirements.

[0257] Good construction performance: easy to construct, improving work efficiency and coating quality.

[0258] Widely used: Suitable for a variety of steel structure projects, including bridges, buildings and ships.

[0259] Test experiment:

[0260] Purpose:

[0261] Through a series of test experiments, the superiority of the long-lasting steel structure anti-corrosion coating of the present invention in terms of anti-corrosion performance, mechanical properties, adhesion, water resistance and salt spray resistance was verified.

[0262] Experimental steps:

[0263] 1. Experimental sample preparation

[0264] Tinplate metal coating samples (200mm x 65mm x 0.8mm) were used.

[0265] 2. Spraying experiment

[0266] Using high-pressure air spraying, the coating thickness of the mechanical properties test sample is 30μm, and the coating thickness of the salt spray performance test sample is 60μm.

[0267] 3. Drying time test

[0268] Surface drying time: the time it takes for the coating surface to become non-sticky.

[0269] Drying time: the time it takes for the coating to completely dry.

[0270] 4. Bending test

[0271] According to the General Technical Conditions for Protective Coatings for Steel Structures (GB / T28699-2012), the performance of the coating under bending is tested.

[0272] 5. Adhesion test

[0273] Use an adhesion tester to assess the coating adhesion in accordance with the Technical Conditions for Anti-corrosion Coating of Highway Bridge Steel Structures (JT / T722-2023).

[0274] 6. Impact resistance test

[0275] The impact resistance of the coating was tested using an impact tester.

[0276] 7. Water resistance test

[0277] Immerse the sample in water and test the coating condition after 240 hours.

[0278] 8. Salt spray resistance test

[0279] Use a salt spray machine to carry out accelerated salt spray test, with 5% sodium chloride, 0.2% copper chloride, 0.1% acetic acid, pH value 3.1, and salt spray box temperature 50°C, to test the coating state after 1000 hours.

[0280] Table 1:

[0281]

[0282]

[0283] Summary of experimental results:

[0284] 1. Drying time:

[0285] The surface drying time of the coatings in all embodiments was within 2 hours, and the actual drying time was more than 24 hours, indicating that the coatings dried quickly and had high construction efficiency.

[0286] 2. Bending test:

[0287] The coatings of all the examples performed well in the bending test, with the bending diameters being less than 3 mm, indicating that the coatings had good flexibility and bending resistance.

[0288] 3. Adhesion test:

[0289] The coating adhesion level of all examples is level 1, which means that the coating has strong adhesion to the substrate and can effectively prevent the coating film from peeling off.

[0290] 4. Impact resistance test:

[0291] The coatings of all examples have an impact resistance of more than 40 cm, showing excellent impact resistance.

[0292] 5. Water resistance test:

[0293] The coatings of all the examples showed no bubbling, falling off or wrinkling after being immersed in water for 240 hours, indicating that the coatings had excellent water resistance.

[0294] 6. Salt spray resistance test:

[0295] The coatings of all embodiments performed well in the salt spray test. After 1000 hours of salt spray test, no blistering, peeling or wrinkling occurred on the surface of the coating film, indicating that the coating has good salt spray resistance and is suitable for anti-corrosion applications in marine environments or high-salt areas.

[0296] Comparative experiment 1: Performance comparison between traditional epoxy zinc-rich primer and the coating of the present invention

[0297] Purpose:

[0298] The superiority of the coating of the present invention is verified by comparing the anticorrosion performance, mechanical properties, adhesion, water resistance and salt spray resistance of the traditional epoxy zinc-rich primer and the coating of the present invention.

[0299] Experimental steps:

[0300] 1. Experimental sample preparation

[0301] Tinplate metal coating samples (200mm x 65mm x 0.8mm) were used.

[0302] 2. Spraying experiment

[0303] Using high-pressure air spraying, the coating thickness of the mechanical properties test sample is 30μm, and the coating thickness of the salt spray performance test sample is 60μm.

[0304] 3. Drying time test

[0305] Surface drying time: the time it takes for the coating surface to become non-sticky.

[0306] Drying time: the time it takes for the coating to completely dry.

[0307] 4. Bending test

[0308] According to the General Technical Conditions for Protective Coatings for Steel Structures (GB / T28699-2012), the performance of the coating under bending is tested.

[0309] 5. Adhesion test

[0310] Use an adhesion tester to assess the coating adhesion in accordance with the Technical Conditions for Anti-corrosion Coating of Highway Bridge Steel Structures (JT / T722-2023).

[0311] 6. Impact resistance test

[0312] The impact resistance of the coating was tested using an impact tester.

[0313] 7. Water resistance test

[0314] Immerse the sample in water and test the coating condition after 240 hours.

[0315] 8. Salt spray resistance test

[0316] Use a salt spray machine to carry out accelerated salt spray test, with 5% sodium chloride, 0.2% copper chloride, 0.1% acetic acid, pH value 3.1, and salt spray box temperature 50°C, to test the coating state after 1000 hours.

[0317] Table 2:

[0318] Experimental Project Traditional epoxy zinc-rich primer Coating Example 1 of the present invention Surface drying time (h) ≤4 ≤2 Drying time (h) ≥48 ≥24 Bending test(mm) ≤5 ≤3 Adhesion(grade) ≤3 ≤1 Impact resistance (cm) ≥20 ≥40 Water resistance (240h) Bubbling, shedding No bubbles, no shedding Salt spray resistance (1000h) Blistering, peeling, wrinkling No bubbles, no shedding, no wrinkles

[0319] Experimental summary:

[0320] This experiment compares the performance of the traditional epoxy zinc-rich primer and the coating of the present invention, and verifies the superiority of the coating of the present invention in terms of drying time, bending performance, adhesion, impact resistance, water resistance and salt spray resistance. The coating of the present invention has fast drying speed, good flexibility, strong adhesion, excellent impact resistance, and excellent performance in water resistance and salt spray resistance tests, and is suitable for steel structure protection in various harsh environments.

[0321] Comparative experiment 2: Performance comparison between the coating of the present invention and the mainstream anti-corrosion coating on the market

[0322] Purpose:

[0323] By comparing the performance of the coating of the present invention with that of other mainstream anti-corrosion coatings on the market, the market competitiveness and superior performance of the coating of the present invention are verified.

[0324] Experimental procedures

[0325] 1. Preparation of experimental samples:

[0326] Tinplate metal coating samples (200mm x 65mm x 0.8mm) were used.

[0327] 2. Spraying experiment:

[0328] Using high-pressure air spraying, the coating thickness of the mechanical properties test sample is 30μm, and the coating thickness of the salt spray performance test sample is 60μm.

[0329] 3. Drying time test:

[0330] Surface drying time: the time it takes for the coating surface to become non-sticky.

[0331] Drying time: the time it takes for the coating to completely dry.

[0332] 4. Bending test:

[0333] According to the General Technical Conditions for Protective Coatings for Steel Structures (GB / T28699-2012), the performance of the coating under bending is tested.

[0334] 5. Adhesion test

[0335] Use an adhesion tester to assess the coating adhesion in accordance with the Technical Conditions for Anti-corrosion Coating of Highway Bridge Steel Structures (JT / T722-2023).

[0336] 6. Impact resistance test:

[0337] The impact resistance of the coating was tested using an impact tester.

[0338] 7. Water resistance test:

[0339] Immerse the sample in water and test the coating condition after 240 hours.

[0340] 8. Salt spray resistance test:

[0341] Use a salt spray machine to carry out accelerated salt spray test, with 5% sodium chloride, 0.2% copper chloride, 0.1% acetic acid, pH value 3.1, and salt spray box temperature 50°C, to test the coating state after 1000 hours.

[0342] Table 3:

[0343]

[0344] Experimental summary:

[0345] This experiment compared the performance of mainstream anti-corrosion coatings on the market with the coating of the present invention, and verified the competitiveness of the coating of the present invention in various performances. The coating of the present invention is superior to the mainstream anti-corrosion coatings on the market in terms of drying time, adhesion, impact resistance, water resistance and salt spray resistance, indicating that the coating of the present invention has strong market competitiveness and broad application prospects.

[0346] Comparative experiment 3: Performance comparison between the coating of the present invention and the environmentally friendly anticorrosive coating

[0347] Purpose:

[0348] By comparing the performance of the coating of the present invention with that of an environmentally friendly anti-corrosion coating, the advantages of the coating of the present invention in terms of environmental performance and anti-corrosion performance are verified.

[0349] Experimental procedures

[0350] 1. Experimental sample preparation

[0351] Tinplate metal coating samples (200mm x 65mm x 0.8mm) were used.

[0352] 2. Spraying experiment

[0353] Using high-pressure air spraying, the coating thickness of the mechanical properties test sample is 30μm, and the coating thickness of the salt spray performance test sample is 60μm.

[0354] 3. Drying time test

[0355] Surface drying time: the time it takes for the coating surface to become non-sticky.

[0356] Drying time: the time it takes for the coating to completely dry.

[0357] 4. Bending test

[0358] According to the General Technical Conditions for Protective Coatings for Steel Structures (GB / T28699-2012), the performance of the coating under bending is tested.

[0359] 5. Adhesion test

[0360] Use an adhesion tester to assess the coating adhesion in accordance with the Technical Conditions for Anti-corrosion Coating of Highway Bridge Steel Structures (JT / T722-2023).

[0361] 6. Impact resistance test

[0362] The impact resistance of the coating was tested using an impact tester.

[0363] 7. Water resistance test

[0364] Immerse the sample in water and test the coating condition after 240 hours.

[0365] 8. Salt spray resistance test

[0366] Use a salt spray machine to carry out accelerated salt spray test, with 5% sodium chloride, 0.2% copper chloride, 0.1% acetic acid, pH value 3.1, and salt spray box temperature 50°C, to test the coating state after 1000 hours.

[0367] Table 4:

[0368]

[0369]

[0370] Experimental summary:

[0371] This experiment verifies the advantages of the coating of the present invention in environmental protection and anti-corrosion performance by comparing the performance of the environmentally friendly anti-corrosion coating and the coating of the present invention. The coating of the present invention not only meets the environmental protection requirements, but also performs well in drying time, adhesion, impact resistance, water resistance and salt spray resistance, further proving the comprehensive advantages of the coating of the present invention in environmental protection and performance.

[0372] Summary:

[0373] The above comparative experiments show that the long-lasting anti-corrosion coating for steel structures of the present invention performs excellently in various performance tests. Whether compared with traditional epoxy zinc-rich primers, mainstream anti-corrosion coatings on the market or environmentally friendly anti-corrosion coatings, the coating of the present invention shows obvious advantages in drying time, adhesion, impact resistance, water resistance and salt spray resistance, and has significant market competitiveness and application prospects.

[0374] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A long-lasting anti-corrosion coating for steel structures, characterized in that: Calculated by weight percentage, it includes the following components: 20%-30% epoxy resin, 2%-5% coloring pigment, 30%-40% body pigment, 10%-20% special anti-rust pigment, 10%-15% solvent, 1%-3% auxiliary agent and 8%-12% curing agent.

2. The long-lasting anti-corrosion coating for steel structures according to claim 1, characterized in that: The auxiliary agents include dispersants and adhesion promoters.

3. The long-lasting anti-corrosion coating for steel structures according to claim 1 is characterized in that: The special anti-rust pigment consists of zinc phosphate and aluminum tripolyphosphate in a weight ratio of 2:

1.

4. A method for preparing a long-lasting anticorrosive coating for steel structures, characterized in that: The long-lasting anti-corrosion coating for steel structures according to any one of claims 1 to 3 is prepared, comprising the following steps: a) Add epoxy resin, coloring pigment and extender pigment into the solvent and stir evenly; b) Grinding to make the coating fineness less than 50μm; c) Add the additive while stirring and continue stirring; d) Add curing agent under stirring and adjust the viscosity to less than 6000 cP; e) Packaging after filtering.

5. The method for preparing a long-lasting anticorrosive coating for steel structures according to claim 4, characterized in that: The step a specifically comprises the following steps: a1. Raw material preparation: Weigh epoxy resin, coloring pigment, extender pigment and solvent according to proportion; a2. Mixed: Add epoxy resin to the stirring device; Gradually add coloring pigments and extender pigments; Finally, the solvent is added; a3. Stirring: Use a high-speed mixer to stir for at least 30 minutes until the mixture is uniform.

6. The method for preparing a long-lasting anticorrosive coating for steel structures according to claim 4, characterized in that: The step b specifically comprises the following steps: b1. Grinding equipment: Use a bead mill; b2. Grinding process: Pour the well-stirred coating mixture into a bead mill; Set appropriate grinding parameters and the grinding time is 1-2h; Grind until the paint fineness reaches less than 50μm.

7. The method for preparing a long-lasting anticorrosive coating for steel structures according to claim 4, characterized in that: The step c specifically includes the following steps: c1. Preparation of additives: Weigh the required additives according to the formula, including dispersants and adhesion promoters; c2. Adding additives: Add the additive gradually to the ground coating; c3. Continue stirring: Continue stirring for 25-35 minutes to ensure that the additive and the coating are fully mixed.

8. The method for preparing a long-lasting anticorrosive coating for steel structures according to claim 4, characterized in that: The step d specifically comprises the following steps: d1. Preparation of curing agent: Weigh the required curing agent according to the formula; d2. Add curing agent: Gradually add the curing agent to the stirring paint; d3. Adjust viscosity: Continue stirring until the viscosity of the coating is adjusted to less than 6000cP; Measure viscosity regularly using a viscometer to ensure requirements are met.

Citation Information

Patent Citations

  • Environmental-friendly waterborne epoxy zinc phosphate anti-corrosion paint for steel structures and preparation method thereof

    CN102533053A

  • High-solid low-corrosion-spreading epoxy primer and preparation method thereof

    CN115678388A

  • Low-surface-treatment epoxy anticorrosive paint as well as preparation method and application thereof

    CN116751498A