High-strength corrosion-resistant steel strand and production process thereof
By using a specific composition of epoxy coating raw materials and modified aluminum nitride on steel strands, the problem of insufficient strength and corrosion resistance of the epoxy coating on epoxy-coated steel strands is solved, and the strength of the steel strands is significantly improved. Tensile strength and corrosion resistance extend its service life.
Patent Information
- Application Number
- CN202411108930.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The epoxy coating of existing epoxy-coated steel strands has poor strength and corrosion resistance, resulting in a shortened service life in harsh environments.
Epoxy coating raw materials including epoxy resin, furan resin, chlorosulfonated polyethylene, aluminum nitride, degassing agent and curing agent are used. Through the specific weight ratio and the use of modified aluminum nitride, the coating properties are improved. strength and corrosion resistance, and the coating is applied to the bare stranded wires via a spray coating process.
Significantly improves the tensile strength and corrosion resistance of the steel strand epoxy coating and extends its service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel strands, and in particular to a high-strength corrosion-resistant steel strand and a production process thereof. Background Art
[0002] Steel strands are metal products made of multiple strands of steel wires. They can be used as load-bearing cables, tension wires and reinforcing cores. They are widely used in bridges, buildings, water conservancy, energy and geotechnical engineering. Steel strands can be divided into galvanized steel strands, epoxy-coated steel strands and aluminum-clad steel strands according to the surface coating layer. Among them, epoxy-coated steel strands are favored by the market due to their high surface hardness and good wear resistance.
[0003] At present, epoxy coated steel strands have the problem of poor strength and corrosion resistance of epoxy coating, which will cause the steel strands to be easily exposed to harsh natural environments, thereby shortening their service life. Therefore, it is of great significance to develop a steel strand with high epoxy coating strength and good corrosion resistance. Summary of the invention
[0004] The invention provides a high-strength corrosion-resistant steel strand and a production process thereof, which solves the problem of poor strength and corrosion resistance of epoxy coating of steel strand in the related art.
[0005] The technical solution of the present invention is as follows: The present invention provides a high-strength corrosion-resistant steel strand, comprising a bare strand and an epoxy coating sprayed on the surface of the bare strand, wherein the raw materials of the epoxy coating include the following components in parts by weight: 150 parts of epoxy resin, 15-30 parts of furan resin, 10-55 parts of chlorosulfonated polyethylene, 20-40 parts of aluminum nitride, 3-5 parts of a degassing agent, and 2-6 parts of a curing agent.
[0006] As a further technical solution, the material of the bare stranded wire includes one of 60Si2Mn, SWRH82BCr, and 82MnA.
[0007] As a further technical solution, the number of strands of the bare stranded wire is 7 to 19.
[0008] As a further technical solution, the weight ratio of the furan resin to the chlorosulfonated polyethylene is 1:1 to 1.5.
[0009] In the present invention, when the weight ratio of the furan resin to the chlorosulfonated polyethylene is 1:1-1.5, it helps to further improve the strength and corrosion resistance of the epoxy coating of the steel strand.
[0010] As a further technical solution, the chlorine content of the chlorosulfonated polyethylene is ≥40wt%.
[0011] In the present invention, when the chlorine content of the chlorosulfonated polyethylene is ≥40wt%, it helps to further improve the strength and corrosion resistance of the epoxy coating of the steel strand.
[0012] As a further technical solution, the aluminum nitride is modified aluminum nitride, and the components of the modified aluminum nitride include aluminum nitride, o-carboxyphenylacetic acid and p-nitrophenol.
[0013] In the present invention, although the addition of aluminum nitride can enhance the strength and corrosion resistance of the epoxy coating of the steel strand, the inventors found that the strength and corrosion resistance of the epoxy coating of the steel strand can be further improved by surface modification of aluminum nitride using o-carboxyphenylacetic acid and p-nitrophenol. It is speculated that this is because the modified aluminum nitride can form chemical crosslinks with the polymer resin inside the epoxy coating of the steel strand, further enhancing the complexity of the internal space of the epoxy coating.
[0014] As a further technical solution, in the modified aluminum nitride, the weight ratio of the aluminum nitride to o-carboxyphenylacetic acid and p-nitrophenol is 10-16:1:1.
[0015] In the present invention, when the weight ratio of aluminum nitride to o-carboxyphenylacetic acid and p-nitrophenol in the modified aluminum nitride is 10-16:1:1, it helps to further improve the strength and corrosion resistance of the epoxy coating of the steel strand.
[0016] As a further technical solution, the preparation method of the modified aluminum nitride comprises the following steps: dissolving o-carboxyphenylacetic acid and p-nitrophenol in ethanol, adding aluminum nitride and dispersing them evenly, and drying to obtain the modified aluminum nitride.
[0017] As a further technical solution, the degassing agent is polyamide wax powder or degassing agent KT961.
[0018] In the present invention, the addition of the degassing agent can remove bubbles, thereby improving the overall quality of the epoxy coating of the steel strand.
[0019] As a further technical solution, the curing agent includes one or more of aromatic amine, polyamide, and 2-methylimidazole.
[0020] The present invention also provides a production process for the high-strength corrosion-resistant steel strand, comprising the following steps: S1, blending, extruding, and granulating the raw materials of the epoxy coating to obtain a masterbatch; S2. Spraying the masterbatch on the surface of the bare stranded wire to obtain the steel stranded wire.
[0021] As a further technical solution, in step S1, the temperature during extrusion is 150-180°C.
[0022] As a further technical solution, in the steel strand, the thickness of the epoxy coating is 0.1-0.2 mm.
[0023] The working principle and beneficial effects of the present invention are: In the present invention, the raw materials of the steel strand epoxy coating include furan resin and chlorosulfonated polyethylene. The active groups of the two resins can be used to cooperate with the epoxy resin to increase the complexity of the internal space of the epoxy coating. This is beneficial to increase the ability of the epoxy coating to resist external forces and improve its strength. On the other hand, it can prevent the penetration of corrosive substances and improve its corrosion resistance. In addition, the addition of aluminum nitride can not only play the role of inorganic particle reinforcement, but also give the steel strand epoxy coating good corrosion resistance. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] In the following embodiments and comparative examples, unless otherwise specified, the material of the bare stranded wire is SWRH82BCr, the number of strands is 7; the model of the epoxy resin is BE-507; the model of the furan resin is HK-3; and the particle size of the aluminum nitride is 500 mesh.
[0026] Example 1 A production process for high-strength corrosion-resistant steel strand, comprising the following steps: S1. By weight, 150 parts of epoxy resin, 15 parts of furan resin, 10 parts of chlorosulfonated polyethylene (model CSM-3305, chlorine content of 33wt%~37wt%, sulfur content of 0.8wt%~1.2wt%), 20 parts of aluminum nitride, 3 parts of degassing agent KT961 and 2 parts of 2-methylimidazole are blended, extruded, granulated, and obtained a masterbatch; Among them, during extrusion, the temperature of zone 1 is 160°C, the temperature of zone 2 is 180°C, and the temperature of zone 3 is 150°C; S2, spraying the masterbatch on the surface of the bare stranded wire to obtain the steel stranded wire; In the steel strand, the thickness of the epoxy coating is 0.2 mm.
[0027] Example 2 A production process for high-strength corrosion-resistant steel strand, comprising the following steps: S1. By weight, 150 parts of epoxy resin, 30 parts of furan resin, 55 parts of chlorosulfonated polyethylene (model CSM-3305, chlorine content of 33wt%~37wt%, sulfur content of 0.8wt%~1.2wt%), 40 parts of aluminum nitride, 5 parts of degassing agent KT961 and 6 parts of 2-methylimidazole are blended, extruded, granulated, and obtained a masterbatch; Among them, during extrusion, the temperature of zone 1 is 160°C, the temperature of zone 2 is 180°C, and the temperature of zone 3 is 150°C; S2, spraying the masterbatch on the surface of the bare stranded wire to obtain the steel stranded wire; In the steel strand, the thickness of the epoxy coating is 0.2 mm.
[0028] Example 3 A production process for high-strength corrosion-resistant steel strand, comprising the following steps: S1. By weight, 150 parts of epoxy resin, 15 parts of furan resin, 35 parts of chlorosulfonated polyethylene (model CSM-3305, chlorine content of 33wt%~37wt%, sulfur content of 0.8wt%~1.2wt%), 36 parts of aluminum nitride, 5 parts of degassing agent KT961 and 6 parts of 2-methylimidazole are blended, extruded, granulated, and obtained a masterbatch; Among them, during extrusion, the temperature of zone 1 is 160°C, the temperature of zone 2 is 180°C, and the temperature of zone 3 is 150°C; S2, spraying the masterbatch on the surface of the bare stranded wire to obtain the steel stranded wire; In the steel strand, the thickness of the epoxy coating is 0.2 mm.
[0029] Example 4 The only difference between this embodiment and embodiment 3 is that in this embodiment, the weight parts of furan resin are 30 parts, and the weight parts of chlorosulfonated polyethylene are 20 parts.
[0030] Example 5 The only difference between this embodiment and embodiment 3 is that in this embodiment, the weight parts of furan resin are 25 parts, and the weight parts of chlorosulfonated polyethylene are 25 parts.
[0031] Example 6 The only difference between this embodiment and embodiment 3 is that in this embodiment, the weight parts of furan resin are 20 parts, and the weight parts of chlorosulfonated polyethylene are 30 parts.
[0032] Example 7 The only difference between this embodiment and embodiment 6 is that, in this embodiment, the model of the chlorosulfonated polyethylene resin is CSM-4010, the chlorine content is 40wt%~45wt%, and the sulfur content is 0.8wt%~1.2wt%.
[0033] Example 8 The only difference between this embodiment and embodiment 7 is that in this embodiment, the aluminum nitride is modified aluminum nitride, and the preparation method of the modified aluminum nitride comprises the following steps: dissolving 2 parts of o-carboxyphenylacetic acid in 40 parts of ethanol, adding 34 parts of aluminum nitride and dispersing them evenly, and drying to obtain modified aluminum nitride.
[0034] Example 9 The only difference between this embodiment and embodiment 8 is that, in the preparation of modified aluminum nitride in this embodiment, o-carboxyphenylacetic acid is replaced by an equal amount of p-nitrophenol.
[0035] Example 10 The only difference between this embodiment and embodiment 8 is that, when preparing modified aluminum nitride in this embodiment, 2 parts of o-carboxyphenylacetic acid are replaced by 1 part of o-carboxyphenylacetic acid and 1 part of p-nitrophenol.
[0036] Embodiment 11 The only difference between this embodiment and embodiment 10 is that, when preparing modified aluminum nitride in this embodiment, the weight parts of aluminum nitride are 28 parts, the weight parts of o-carboxyphenylacetic acid are 4 parts, and the weight parts of p-nitrophenol are 4 parts.
[0037] Example 12 The only difference between this embodiment and embodiment 10 is that, when preparing modified aluminum nitride in this embodiment, the weight parts of aluminum nitride are 30 parts, the weight parts of o-carboxyphenylacetic acid are 3 parts, and the weight parts of p-nitrophenol are 3 parts.
[0038] Example 13 The only difference between this embodiment and embodiment 10 is that, when preparing modified aluminum nitride in this embodiment, the weight parts of aluminum nitride are 32 parts, the weight parts of o-carboxyphenylacetic acid are 2 parts, and the weight parts of p-nitrophenol are 2 parts.
[0039] Comparative Example 1 The difference between this comparative example and Example 1 is that in this comparative example, no furan resin is added and 25 parts of chlorosulfonated polyethylene are added.
[0040] Comparative Example 2 The difference between this comparative example and Example 1 is that in this comparative example, no chlorosulfonated polyethylene is added and 25 parts of furan resin are added.
[0041] Comparative Example 3 The only difference between this comparative example and Example 1 is that in this comparative example, furan resin and chlorosulfonated polyethylene are not added.
[0042] Comparative Example 4 The only difference between this comparative example and Example 1 is that in this comparative example, aluminum nitride is not added.
[0043] The following performance tests were performed on the epoxy coatings of the steel strands in Examples 1 to 13 and Comparative Examples 1 to 4: ①Tensile strength: Cut the coating into strips of 25mm×150mm×0.2mm and use a WDW-5 single-arm microcomputer-controlled electronic tensile testing machine to test its tensile strength. The test speed is 10mm / min. ②Mass loss rate: According to GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test", a 480h neutral salt spray test was carried out to determine the mass loss rate. The test temperature was 35°C and the concentration of the sodium chloride solution was 50g / L.
[0044] The test results are shown in Table 1 below.
[0045] Table 1 Test results
[0046] Comparison between Example 1 and Comparative Examples 1 to 3 shows that the synergistic effect of furan resin and chlorosulfonated polyethylene can significantly improve the strength and corrosion resistance of the epoxy coating of steel strands. Comparison between Example 1 and Comparative Example 4 shows that the addition of aluminum nitride is beneficial to improving the strength and corrosion resistance of the epoxy coating of steel strands.
[0047] Comparison between Examples 3-4 and 5-6 shows that when the weight ratio of furan resin to chlorosulfonated polyethylene is 1:1-1.5, it helps to further improve the strength and corrosion resistance of the epoxy coating of the steel strand. Comparison between Example 6 and Example 7 shows that when the chlorine content of the chlorosulfonated polyethylene is ≥40wt%, it helps to further improve the strength and corrosion resistance of the epoxy coating of the steel strand.
[0048] Comparison between Example 7 and Examples 8 to 13 shows that the strength and corrosion resistance of the epoxy coating of the steel strand can be further improved by surface modification of aluminum nitride. Comparison between Examples 8 to 9 and Example 10 shows that compared with the modification of aluminum nitride by ortho-carboxyphenylacetic acid alone or by p-nitrophenol alone, the modification of aluminum nitride by ortho-carboxyphenylacetic acid and p-nitrophenol can further improve the strength and corrosion resistance of the epoxy coating of the steel strand. Comparison between Examples 10 to 11 and Examples 12 to 13 shows that when the weight ratio of aluminum nitride to ortho-carboxyphenylacetic acid and p-nitrophenol in the modified aluminum nitride is 10 to 16:1:1, it helps to further improve the strength and corrosion resistance of the epoxy coating of the steel strand.
[0049] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-strength, corrosion-resistant steel strand, comprising a bare strand and an epoxy coating sprayed on the surface of the bare strand, characterized in that: The raw materials of the epoxy coating include the following components in parts by weight: 150 parts of epoxy resin, 15-30 parts of furan resin, 10-55 parts of chlorosulfonated polyethylene, 20-40 parts of aluminum nitride, 3-5 parts of degassing agent, and 2-6 parts of curing agent.
2. A high-strength corrosion-resistant steel strand according to claim 1, characterized in that: The weight ratio of the furan resin to the chlorosulfonated polyethylene is 1:1 to 1.
5.
3. The high-strength corrosion-resistant steel strand according to claim 1, characterized in that: The chlorine content of the chlorosulfonated polyethylene is ≥40wt%.
4. The high-strength corrosion-resistant steel strand according to claim 1, characterized in that: The aluminum nitride is modified aluminum nitride, and the components of the modified aluminum nitride include aluminum nitride, o-carboxyphenylacetic acid and p-nitrophenol.
5. The high-strength corrosion-resistant steel strand according to claim 4, characterized in that: In the modified aluminum nitride, the weight ratio of the aluminum nitride to o-carboxyphenylacetic acid and p-nitrophenol is 10-16:1:
1.
6. The high-strength corrosion-resistant steel strand according to claim 4, characterized in that: The preparation method of the modified aluminum nitride comprises the following steps: dissolving o-carboxyphenylacetic acid and p-nitrophenol in ethanol, adding aluminum nitride to disperse uniformly, and drying to obtain the modified aluminum nitride.
7. A high-strength corrosion-resistant steel strand according to any one of claims 1 to 6, characterized in that: The degassing agent is polyamide wax micropowder or degassing agent KT961.
8. The high-strength corrosion-resistant steel strand according to any one of claims 1 to 6, characterized in that: The curing agent includes one or more of aromatic amine, polyamide and 2-methylimidazole.
9. A production process for high-strength corrosion-resistant steel strand according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, blending, extruding, and granulating the raw materials of the epoxy coating to obtain a masterbatch; S2. Spraying the masterbatch on the surface of the bare stranded wire to obtain the steel stranded wire.
10. The production process of a high-strength corrosion-resistant steel strand according to claim 9, characterized in that: In step S1, the temperature during extrusion is 150-180°C.
Citation Information
Patent Citations
Novel environment-friendly thermosetting powder coating material and preparation method thereof
CN108864904A
Epoxy coating unbonded steel strand and preparation method thereof
CN117089263A
Method for preparing furan-epoxy powder-like binder
US4254245A