Water-based anti-corrosion wax capable of being sprayed on high-temperature electrophoresis frame as well as preparation method and application of water-based anti-corrosion wax
By using high melting point biomass hard wax and modified lecithin microsphere emulsifier in water-based anti-corrosion wax, combined with amino-functionalized macroporous graphene oxide, the poor film formation and poor aging resistance of water-based anti-corrosion wax under high temperature conditions are solved. solve the problem, achieve better anti-corrosion and scratch resistance properties, and meet the protection needs of commercial vehicle electrophoresis frames and chassis.
Patent Information
- Application Number
- CN202410743019.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Existing water-based anti-corrosion waxes have poor film formation, poor aging resistance, insufficient film hardness, and poor stain resistance caused by high-temperature anti-sticking of the wax film when applied under high-temperature conditions. They cannot effectively protect commercial vehicle electrophoresis frames and chassis.
It uses components such as high-melting-point biomass hard wax, slow-release modified lecithin microsphere emulsifier, and amino-functionalized macroporous graphene oxide to improve the hardness and anti-corrosion properties of the wax through chemical modification and microbial media. The pore structure provides a passage for the wax film to avoid water vapor sealing and form a stable emulsification system.
It achieves good film-forming effect under high temperature conditions, improves the water resistance, anti-corrosion and scratch resistance of the wax film, extends the service life of the wax film, and meets the needs of commercial vehicle OEMs for frame anti-corrosion quality. and reduce production costs.
Smart Images

Figure FDA0004885457610000011 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of anti-corrosion materials, and particularly relates to a water-based anti-corrosion wax material that can be sprayed on a high-temperature electrophoresis vehicle frame, and a preparation method and application thereof. Background Art
[0003] At present, the frame material used by major commercial vehicle OEMs is hot-rolled steel coated with cathodic electrophoretic paint. Although the electrophoretic paint has excellent anti-corrosion performance, its weather resistance is poor. If no secondary anti-corrosion is done, the electrophoretic paint will powder or fall off within 3-6 months after leaving the factory, which will lose its ability to protect the metal frame and chassis. Therefore, commercial vehicle OEMs will spray anti-corrosion wax on the electrophoretic frame to protect the electrophoretic paint, bolts, gaps and other locations to enhance the anti-corrosion ability of the entire frame and chassis. For anti-corrosion wax, traditional solvent-based anti-corrosion wax has been widely used because of its excellent anti-corrosion performance for frames and chassis. However, with the implementation of environmental protection policies this year, traditional solvent-based anti-corrosion wax has gradually been replaced by water-based, low-VOC, environmentally friendly products.
[0004] For the electrophoretic frame anti-corrosion of commercial vehicles, there is no obvious difference in the anti-corrosion ability between solvent-based anti-corrosion wax and water-based anti-corrosion wax. However, in terms of workability, anti-aging resistance, film hardness, high temperature resistance and dirt resistance, water-based anti-corrosion wax products still have the following disadvantages: ① In terms of workability, since the electrophoretic frame and chassis of commercial vehicles are black, the frame is exposed to high temperature and sunlight during construction in summer, and the surface temperature can reach up to 70-90°C. The wax spraying line of commercial vehicles is usually an outdoor or semi-outdoor construction environment. Therefore, it is impossible to cool the frame before spraying. In order to ensure the production rhythm, water-based anti-corrosion wax must be sprayed directly on the high-temperature electrophoretic frame. This causes the surface of the wax film to dry quickly after spraying, and the water vapor inside the wax film is sealed inside. This results in the wax film being unable to dry thoroughly, turning white in appearance, and losing its initial water resistance. During the rain test on the entire vehicle, the wax film is dissolved by water and cannot form an anti-corrosion wax film; ② In terms of aging resistance, water-based products often need to actively add UV aging and oxidation resistance additives to improve aging resistance, but such additives often have poor compatibility with water-based products, resulting in a reduction in the product's anti-corrosion ability; ③ In terms of film hardness, high temperature resistance, and dirt resistance, among existing products, whether solvent-based or water-based, the film hardness hardly reaches the HB level, so the wax film has almost no scratch resistance. In addition, at high temperatures in summer, the hardness of the wax film decreases rapidly and even becomes sticky, which causes a large amount of dust and sand to adhere to the frame, seriously affecting the anti-corrosion ability and appearance.
[0005] Therefore, in order to meet the requirements of construction performance, corrosion resistance, aging resistance, film hardness, high temperature resistance and dirt resistance under high temperature conditions in summer, it is a technical problem that needs to be solved urgently to develop a water-based anti-corrosion wax material that can be sprayed on high-temperature electrophoretic frames. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoretic frame to solve the technical problems of poor film formation, poor aging resistance, insufficient film hardness and poor dirt resistance caused by high-temperature anti-sticking of the wax film when the water-based anti-corrosion wax is constructed under high temperature conditions in summer.
[0007] The technical solution adopted by the present invention is: a water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis frame, comprising the following components in proportion by weight:
[0008] 30-40 parts of high melting point biomass hard wax
[0009] 5-8 parts of sustained-release modified lecithin microsphere emulsifier
[0010] 0.5-1 part of monoethanolamine
[0011] 35-50 parts of deionized water
[0012] Furthermore, the above-mentioned aqueous anti-corrosion wax that can be sprayed on a high-temperature electrophoresis frame, the high-melting-point biomass hard wax, has a preparation method comprising the following steps: taking 30-40 parts of Brazilian palm wax and 20-40 parts of a mixed organic solvent and adding them to a reactor, starting stirring, the stirring speed is 50-100 rpm, the temperature is controlled at 25-37°C, 5-8 parts of palmitic acid are added, stirred for 1-2h, and then 15-20 parts of Pseudomonas aqueous dispersion are added, and the stirring reaction is continued for 10-15h, and finally the temperature of the reactor is increased to 100-110°C, and the pressure in the reactor is evacuated to -0.1-0.08mPa, and stirred for 1h, and the high-melting-point biomass hard wax is obtained by discharging the material.
[0013] Furthermore, in the above-mentioned aqueous anti-corrosion wax that can be sprayed on a high-temperature electrophoresis frame, the mixed organic solvent is a combination of ethyl acetate and propylene glycol butyl ether, and the mass ratio is ethyl acetate:propylene glycol butyl ether=1-3:5; the Pseudomonas aqueous dispersion is a Pseudomonas aeruginosa aqueous dispersion with a live bacteria concentration of 1000000 CFU / mL and a pH value of 6.5-7.5.
[0014] Furthermore, the above-mentioned aqueous anticorrosive wax that can be sprayed on a high-temperature electrophoresis frame, the sustained-release modified lecithin microsphere emulsifier, the preparation method comprises the following steps:
[0015] 1) Organic acid modified lecithin: 10-20 parts of organic acid and 30-40 parts of dimethylformamide are added to a stirring tank, stirring is started, the stirring speed is 200-300 rpm, stirring at room temperature for 1-2 hours, then 0.2-0.4 parts of organic acid activator are added, stirring at 20-25° C. for 1-2 hours, then 0.1-0.2 parts of deionized water are added, and then 30-50 parts of lecithin are added, the reaction temperature is increased to 50-60° C., stirring for 2-3 hours, and finally the above materials are vacuum dried to obtain organic acid modified lecithin;
[0016] 2) Amino-functionalized macroporous graphene oxide: Take 40-60 parts of graphene oxide powder and 30-40 parts of mixed acid aqueous solution, add them to a reactor, stir at a speed of 20-40 rpm, heat to 40-55°C under stirring, stir and react for 2-4 hours, filter the product after the reaction, and then wash it 1-3 times with an ice-water mixture, wash and dry to obtain macroporous graphene oxide powder. Take 30-50 parts of macroporous graphene oxide powder and add it to 20-30 parts of ethylenediamine, stir at a speed of 20-40 rpm, stir and react at room temperature for 1-3 hours, filter and dry the product after the reaction to obtain amino-functionalized macroporous graphene oxide.
[0017] 3) Sustained-release modified lecithin microsphere emulsifier: 50-60 parts of deionized water and 30-45 parts of organic acid modified lecithin are added to a high-speed dispersion reactor, the stirring speed is 1000-2000 rpm, and the mixture is stirred and dispersed at room temperature for 1-2 hours. Then 3-6 parts of amino-functionalized macroporous graphene oxide are added, the stirring speed is increased to 3000-5000 rpm, and the mixture is stirred and dispersed for 1-2 hours. Then 0.1-0.3 parts of phthaloyl chloride are slowly added dropwise, and the mixture is stirred and reacted at room temperature for 1-2 hours. Finally, 5-8 parts of proanthocyanidins are added to the high-speed dispersion reactor, and the mixture is stirred and reacted for 2-4 hours. After the reaction is completed, a sustained-release modified lecithin microsphere emulsifier is obtained.
[0018] Furthermore, in the above-mentioned water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis frame, the organic acid is a combination of palmitic acid and cerotic acid; in terms of mass ratio, palmitic acid:cerotic acid=10-20:1.
[0019] Furthermore, in the above-mentioned water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis frame, the organic acid activator is a combination of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysulfosuccinimide; in terms of mass ratio, 1-ethyl-(3-dimethylaminopropyl)carbodiimide:N-hydroxysulfosuccinimide=1:2-5.
[0020] Furthermore, in the above-mentioned water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoretic frame, the graphene oxide powder is graphene oxide with an oxidation degree of a carbon-oxygen ratio of 1-2:1.
[0021] Furthermore, in the above-mentioned water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoretic frame, the mixed acid aqueous solution is a combination of sulfuric acid, nitric acid and water; in terms of mass ratio, sulfuric acid: nitric acid: water = 7-8:1:2.
[0022] Furthermore, the above-mentioned method for preparing the water-based anti-corrosion wax that can be sprayed on the high-temperature electrophoresis frame comprises the following steps: adding monoethanolamine and deionized water to a high-speed dispersion reactor, starting stirring at a stirring speed of 500-800 rpm, heating to 90-95°C, adding high-melting point biomass hard wax, continuing stirring for 0.5-1h, adding a sustained-release modified lecithin microsphere emulsifier, and continuing stirring for 1-2h to obtain the water-based anti-corrosion wax that can be sprayed on the high-temperature electrophoresis frame.
[0023] The invention provides an application of a water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoretic frame in preparing a metal surface anti-corrosion wax on the electrophoretic frame and chassis surface of a commercial vehicle.
[0024] The present invention uses microorganisms as a modification medium to graft organic acids onto the molecular chain of Brazilian palm wax, thereby improving the hardness, water resistance, melting point and anti-corrosion properties of the wax, and using it as a film-forming material. In order to emulsify the modified Brazilian palm wax, the present invention specifically provides an amino-functionalized graphene oxide with a macroporous structure to coat the emulsifier microspheres to prepare an anti-corrosion wax. This structure can provide a sustained-release effect and maintain the viscosity of the emulsified system stable. Thanks to the porous structure of the modified graphene, under high temperature conditions, a path can be provided for the volatilization of water vapor in the wax liquid to avoid film defects caused by water vapor closure. This solves the problem that water-based anti-corrosion wax products cannot be directly sprayed on high-temperature frames and chassis, meets the summer construction needs of commercial vehicle main manufacturers, speeds up production rhythms, and also meets the main manufacturers' requirements for frame anti-corrosion quality.
[0025] The beneficial effects of the present invention are:
[0026] 1. The present invention provides a novel water-based anti-corrosion wax preparation technology, which is suitable for the secondary anti-corrosion of commercial vehicle electrophoretic frames and chassis. The most prominent beneficial effect is that when the electrophoretic frames and chassis of commercial vehicles are subjected to high temperature and exposure to the sun, the surface temperature is too high. At this time, spraying the water-based anti-corrosion wax of the present invention can form a good film without the common paint film defects of conventional water-based products, such as water vapor closure causing the wax film to be unable to dry thoroughly and a whitish appearance, which leads to poor initial water resistance. During the rain test of the whole vehicle, the wax film is washed away by water, which ultimately causes the secondary anti-corrosion failure of the frame and chassis.
[0027] 2. The difference between the present invention and conventional water-based wax is that conventional water-based anti-corrosion wax is prepared by emulsifying paraffin wax, Fischer-Tropsch wax, PE wax and other materials produced by petroleum refining, while the present invention adopts carnauba wax, a natural wax material of non-fossil energy, as the emulsification object, so it is more low-carbon and environmentally friendly in terms of material selection. In addition, in terms of film-forming performance, carnauba wax is widely used because of its good hardness, but its disadvantage is that carnauba wax molecules contain a large number of hydroxyl groups, which makes the wax film easily hydrophilic. Therefore, although unmodified carnauba wax is easy to emulsify, the film-forming material has poor corrosion resistance and water resistance. Therefore, the present invention uses organic acid to modify carnauba wax, and removes the surface hydroxyl groups of carnauba wax through chemical modification reaction, thereby improving corrosion resistance and water resistance.
[0028] 3. The present invention uses palmitic acid to modify carnauba wax, which has the beneficial effect that palmitic acid is grafted onto the carnauba wax molecular chain by reaction, increasing the chain length of the wax, thereby improving the crystallinity, melting point and hardness of the wax, which makes the water-based anti-corrosion wax of the present invention have better hardness, improves the scratch resistance, and can better protect the electrophoresis frame and chassis. In addition, the increase in the melting point of the wax can well improve the dryness of the wax film at high temperatures, avoid high-temperature anti-stickiness of the anti-corrosion wax after film formation, adhere to dust, and affect the neatness of the appearance. Palmitic acid is chosen because, on the one hand, palmitic acid and carnauba wax molecules have natural similarities, which allows the modified molecules to better form crystals with the original wax molecules to ensure hardness; on the other hand, the long alkyl molecular chain of palmitic acid helps to increase the melting point. In summary, palmitic acid is more advantageous than other organic acids in modifying palm wax.
[0029] 4. The present invention uses Pseudomonas aeruginosa to modify carnauba wax, and its outstanding beneficial effect is that the biosynthesis pathway can be used to obtain the product more economically, which can significantly reduce the production cost. Because biosynthesis technology can reduce energy consumption, compared with traditional chemical synthesis, it is carried out under relatively mild conditions, such as normal temperature and pressure, which is significantly helpful for controlling product costs.
[0030] 5. The present invention adopts a mixed organic acid modified lecithin emulsifier to emulsify the high melting point hard bio-based carnauba wax. The reason is that the hydrophobicity of the modified carnauba wax is improved and it is more difficult to emulsify, so the unmodified emulsifier lecithin is difficult to emulsify it. In order to improve the emulsification ability, lipophilicity and water resistance of the emulsifier, the mixed organic acid is selected to modify the lecithin, which can avoid the problem of water resistance and whitening after the aqueous wax film is dried. Both acids can be reactively grafted onto the lecithin molecular chain, increase the chain length of the emulsifier, and improve the lipophilicity. The two organic acids are prepared in a certain proportion because the lipophilicity of the palmitic acid emulsifier alone is insufficient, and the use of wax acid alone will make the hydrophilicity lack.
[0031] 6. In order to avoid excessive use of emulsifiers, which would result in insufficient water resistance of the dry film of the water-based anticorrosive wax, the present invention uses functionalized porous graphene oxide with a macroporous structure to coat the emulsifier microspheres. When the emulsifier is needed by the emulsifier system, the emulsifier microspheres can penetrate into the emulsion through the gaps in the graphene, thereby maintaining the viscosity of the emulsified system stable and avoiding demulsification.
[0032] 7. The present invention uses a certain proportion of acid to etch graphene oxide with a certain oxidation degree to obtain macroporous graphene oxide, and then the amino-functionalized graphene oxide has the beneficial effect that the etched porous graphene uses phthaloyl chloride as a bonding bridge to disperse the emulsifier and graphene sheets under high-speed shear conditions, and a three-dimensional structure is formed through a cross-linking reaction. The emulsifier is coated on the surface of the emulsifier, which can achieve a sustained release effect of the emulsifier. On the other hand, the pore size on the graphene surface can provide a path for water vapor to volatilize when the wax film is dried under high temperature conditions, thereby avoiding the problems of water resistance and film-forming defects caused by water vapor closure. This solves the problem that water-based anti-corrosion wax products cannot be directly sprayed on high-temperature frames and chassis, and helps OEMs to speed up production rhythms and improve the anti-corrosion quality of frames.
[0033] 8. The key reason for the present invention to modify graphene by amino functionalization is that the amino groups on the surface can chemically bond with the amino groups on the surface of the cathode epoxy electrophoretic paint of the electrophoretic frame, thus avoiding the migration of the emulsifier to the surface of the anti-corrosion wax, thereby reducing the water resistance and corrosion resistance of the anti-corrosion wax. In addition, since water-based anti-corrosion wax is a non-hiding product and has no reflective effect on ultraviolet rays, and the cathode electrophoretic paint is extremely sensitive to ultraviolet rays, it is necessary to add an ultraviolet absorber. In order to enhance the protection of water-based anti-corrosion wax against electrophoretic paint, the present invention adds natural bio-based ultraviolet absorber proanthocyanidins. While proanthocyanidins have poor dispersibility in emulsions, the technical means selected by the present invention is to utilize the hydroxyl groups of proanthocyanidins to hydrogen bond with the amino groups on the surface of graphene to ensure dispersibility and provide long-term anti-aging protection for the frame and chassis. DETAILED DESCRIPTION
[0034] The present invention is described in detail below with reference to the embodiments.
[0035] Example 1 A method for preparing a water-based anticorrosive wax (I) that can be sprayed on a high-temperature electrophoresis vehicle frame is as follows:
[0036] 1. Preparation of high melting point biomass hard wax:
[0037] Take 30kg of Brazilian palm wax and 5kg of ethyl acetate and add them to the reactor, then add 15kg of propylene glycol butyl ether, start stirring, the stirring speed is 80 rpm, the temperature is controlled at 30°C, add 5kg of palmitic acid, stir for 1-2h, then add 15kg of Pseudomonas aeruginosa aqueous dispersion with a live bacteria concentration of 1000000 CFU / mL at pH=7, continue stirring and reacting for 10h, finally increase the temperature of the reactor to 110°C, evacuate to the pressure in the reactor to -0.1mPa, stir for 1h, and obtain a high melting point biomass hard wax.
[0038] 2. Preparation of sustained-release modified lecithin microsphere emulsifier:
[0039] 1) Preparation of organic acid modified lecithin: 10 kg of palmitic acid and 1 kg of cerotic acid were added to a stirring tank, followed by 30 kg of dimethylformamide, stirring was started at 200 rpm, stirring was carried out at room temperature for 1 h, then 50 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 150 g of N-hydroxysulfosuccinimide were added, stirring was carried out at 20° C. for 1 h, then 100 g of deionized water was added, and then 40 kg of lecithin was added, the reaction temperature was raised to 55° C., stirring was carried out for 2 h, and finally the above materials were vacuum dried to obtain organic acid modified lecithin.
[0040] 2) Preparation of amino-functionalized macroporous graphene oxide: 40 kg of graphene oxide powder with a carbon-oxygen ratio of 1.5:1 and 30 kg of mixed acid aqueous solution (mass ratio is sulfuric acid: nitric acid: water = 7:1:2) are added to the reactor, the stirring speed is 20 rpm, the temperature is raised to 40°C under stirring, the reaction is stirred for 4 hours, and the product is filtered after the reaction is completed, and then washed with ice water mixture 3 times, and the macroporous graphene oxide powder is obtained after washing and drying. 30 kg of macroporous graphene oxide powder is added to 20 kg of ethylenediamine, the stirring speed is 20 rpm, the reaction is stirred at room temperature for 1 hour, and the product is filtered and dried after the reaction is completed to obtain amino-functionalized macroporous graphene oxide.
[0041] 3) Preparation of sustained-release modified lecithin microsphere emulsifier: 50 kg of deionized water and 30 kg of organic acid-modified lecithin are added to a high-speed dispersion reactor, the stirring speed is 2000 rpm, and the mixture is stirred and dispersed at room temperature for 1 hour. Then, 3 kg of amino-functionalized macroporous graphene oxide is added, the stirring speed is increased to 3000 rpm, and the mixture is stirred and dispersed for 1 hour. Then, 100 g of phthaloyl chloride is slowly added dropwise, and the mixture is stirred and reacted at room temperature for 1 hour. Finally, 5 kg of proanthocyanidins are added to the high-speed dispersion reactor, and the mixture is stirred and reacted for 2-4 hours. After the reaction, a sustained-release modified lecithin microsphere emulsifier is obtained.
[0042] 3. Preparation of water-based anti-corrosion wax that can be sprayed on high-temperature electrophoresis frames:
[0043] Add 0.5kg of monoethanolamine and 35kg of deionized water to a high-speed dispersion reactor, start stirring at a speed of 500-800 rpm, heat to 95°C, add 30kg of high melting point biomass hard wax, continue stirring for 1h, add 5kg of slow-release modified lecithin microsphere emulsifier, continue stirring for 1h, and obtain a water-based anticorrosive wax that can be sprayed on a high-temperature electrophoresis frame. Product performance indicators are shown in Table 1.
[0044] Example 2 A water-based anticorrosive wax (I) that can be sprayed on a high-temperature electrophoresis vehicle frame is prepared as follows:
[0045] 1. Preparation of high melting point biomass hard wax: same as Example 1.
[0046] 2. Preparation of sustained-release modified lecithin microsphere emulsifier: same as Example 1.
[0047] 3. Preparation of water-based anti-corrosion wax that can be sprayed on high-temperature electrophoresis frames:
[0048] Add 0.5kg of monoethanolamine and 35kg of deionized water to a high-speed dispersion reactor, start stirring at a speed of 500-800 rpm, heat to 95°C, add 35kg of high melting point biomass hard wax, continue stirring for 1h, add 5kg of slow-release modified lecithin microsphere emulsifier, continue stirring for 1h, and obtain a water-based anticorrosive wax that can be sprayed on a high-temperature electrophoresis frame. Product performance indicators are shown in Table 1.
[0049] Example 3 A method for preparing a water-based anticorrosive wax (I) that can be sprayed on a high-temperature electrophoresis vehicle frame is as follows:
[0050] 1. Preparation of high melting point biomass hard wax: same as Example 1.
[0051] 2. Preparation of sustained-release modified lecithin microsphere emulsifier: same as Example 1.
[0052] 3. Preparation of water-based anti-corrosion wax that can be sprayed on high-temperature electrophoresis frames:
[0053] Add 0.5kg of monoethanolamine and 35kg of deionized water to a high-speed dispersion reactor, start stirring at a speed of 500-800 rpm, heat to 95°C, add 40kg of high melting point biomass hard wax, continue stirring for 1h, add 5kg of slow-release modified lecithin microsphere emulsifier, continue stirring for 1h, and obtain a water-based anticorrosive wax that can be sprayed on a high-temperature electrophoresis frame. Product performance indicators are shown in Table 1.
[0054] Comparative Example 1 A method for preparing a water-based anticorrosive wax (I) that can be sprayed on a high-temperature electrophoresis vehicle frame is as follows:
[0055] 1. Selection of biomass hard wax:
[0056] Choose unmodified carnauba wax.
[0057] 2. Preparation of sustained-release modified lecithin microsphere emulsifier: same as Example 1.
[0058] 3. Preparation of water-based anti-corrosion wax that can be sprayed on high-temperature electrophoresis frames:
[0059] Add 0.5kg of monoethanolamine and 35kg of deionized water to a high-speed dispersion reactor, start stirring at a speed of 500-800 rpm, heat to 95°C, add 35kg of unmodified carnauba wax, continue stirring for 1h, add 5kg of sustained-release modified lecithin microsphere emulsifier, continue stirring for 1h, and obtain a water-based anticorrosive wax that can be sprayed on a high-temperature electrophoresis frame. Product performance indicators are shown in Table 1.
[0060] Comparative Example 2 A method for preparing a water-based anticorrosive wax (I) that can be sprayed on a high-temperature electrophoresis vehicle frame is as follows:
[0061] 1. Preparation of high melting point biomass hard wax: same as Example 1.
[0062] 2. Preparation of sustained-release lecithin microsphere emulsifier:
[0063] 1) Selection of lecithin: Use unmodified lecithin.
[0064] 2) Preparation of amino-functionalized macroporous graphene oxide: 40 kg of graphene oxide powder with a carbon-oxygen ratio of 1.5:1 and 30 kg of mixed acid aqueous solution (mass ratio is sulfuric acid: nitric acid: water = 7:1:2) are added to the reactor, the stirring speed is 20 rpm, the temperature is raised to 40°C under stirring, the reaction is stirred for 4 hours, and the product is filtered after the reaction is completed, and then washed with ice water mixture 3 times, and the macroporous graphene oxide powder is obtained after washing and drying. 30 kg of macroporous graphene oxide powder is added to 20 kg of ethylenediamine, the stirring speed is 20 rpm, the reaction is stirred at room temperature for 1 hour, and the product is filtered and dried after the reaction is completed to obtain amino-functionalized macroporous graphene oxide.
[0065] 3) Preparation of sustained-release lecithin microsphere emulsifier: 50 kg of deionized water and 30 kg of lecithin were added to a high-speed dispersion reactor, the stirring speed was 2000 rpm, and the mixture was stirred and dispersed at room temperature for 1 h. Then 3 kg of amino-functionalized macroporous graphene oxide was added, the stirring speed was increased to 3000 rpm, and the mixture was stirred and dispersed for 1 h. Then 100 g of phthaloyl chloride was slowly added dropwise, and the mixture was stirred and reacted at room temperature for 1 h. Finally, 5 kg of proanthocyanidins were added to the high-speed dispersion reactor, and the stirring reaction was continued for 2-4 h. After the reaction, a sustained-release lecithin microsphere emulsifier was obtained.
[0066] 3. Preparation of water-based anti-corrosion wax that can be sprayed on high-temperature electrophoresis frames:
[0067] Add 0.5kg of monoethanolamine and 35kg of deionized water to a high-speed dispersion reactor, start stirring at a speed of 500-800 rpm, heat to 95°C, add 35kg of high melting point biomass hard wax, continue stirring for 1h, add 5kg of sustained-release lecithin microsphere emulsifier, continue stirring for 1h, and obtain a water-based anticorrosive wax that can be sprayed on the electrophoresis frame at room temperature. Product performance indicators are shown in Table 1.
[0068] Comparative Example 3 A method for preparing a water-based anticorrosive wax (I) that can be sprayed on a high-temperature electrophoresis vehicle frame is as follows:
[0069] 1. Preparation of high melting point biomass hard wax: same as Example 1.
[0070] 2. Preparation of sustained-release modified lecithin microsphere emulsifier:
[0071] 1) Preparation of organic acid-modified lecithin: same as in Example 1.
[0072] 2) Preparation of amino-functionalized graphene: 30 kg of graphene oxide powder with a carbon-oxygen ratio of 1.5:1 was added to 20 kg of ethylenediamine, stirred at 20 rpm, and reacted at room temperature for 1 h. After the reaction, the product was filtered and dried to obtain amino-functionalized graphene.
[0073] 3) Preparation of coated modified lecithin microsphere emulsifier: 50 kg of deionized water and 30 kg of organic acid modified lecithin are added to a high-speed dispersion reactor, the stirring speed is 2000 rpm, and the mixture is stirred and dispersed at room temperature for 1 hour. Then 3 kg of amino-functionalized graphene is added, the stirring speed is increased to 3000 rpm, and the mixture is stirred and dispersed for 1 hour. Then 100 g of phthaloyl chloride is slowly added dropwise, and the mixture is stirred and reacted at room temperature for 1 hour. Finally, 5 kg of proanthocyanidins are added to the high-speed dispersion reactor, and the mixture is stirred and reacted for 2-4 hours. After the reaction, a coated modified lecithin microsphere emulsifier is obtained.
[0074] 3. Preparation of water-based anti-corrosion wax that can be sprayed on electrophoresis frames at room temperature:
[0075] Add 0.5kg of monoethanolamine and 35kg of deionized water to a high-speed dispersion reactor, start stirring at a speed of 500-800 rpm, heat to 95°C, add 35kg of high melting point biomass hard wax, continue stirring for 1h, add 5kg of coated modified lecithin microsphere emulsifier, continue stirring for 1h, and obtain a water-based anticorrosive wax that can be sprayed on a high-temperature electrophoresis frame. Product performance indicators are shown in Table 1.
[0076] Comparative Example 4 A method for preparing a water-based anticorrosive wax (I) that can be sprayed on a high-temperature electrophoresis vehicle frame is as follows:
[0077] 1. Preparation of high melting point biomass hard wax: same as Example 1.
[0078] 2. Preparation of sustained-release lecithin microsphere emulsifier:
[0079] 1) Preparation of organic acid-modified lecithin: same as in Example 1.
[0080] 2) Preparation of macroporous graphene oxide: 40 kg of graphene oxide powder with a carbon-oxygen ratio of 1.5:1 and 30 kg of a mixed acid aqueous solution (mass ratio of sulfuric acid: nitric acid: water = 7:1:2) were added to a reactor with a stirring speed of 20 rpm. The mixture was heated to 40°C with stirring and reacted for 4 h. After the reaction, the product was filtered and then washed 3 times with an ice-water mixture. After washing and drying, macroporous graphene oxide powder was obtained.
[0081] 3) Preparation of sustained-release modified lecithin microsphere emulsifier: 50 kg of deionized water and 30 kg of lecithin were added to a high-speed dispersion reactor, the stirring speed was 2000 rpm, and the mixture was stirred and dispersed at room temperature for 1 h. Then 3 kg of macroporous graphene oxide was added, the stirring speed was increased to 3000 rpm, and the mixture was stirred and dispersed for 1 h. Then 100 g of phthaloyl chloride was slowly added dropwise, and the mixture was stirred and reacted at room temperature for 1 h. Finally, 5 kg of proanthocyanidins were added to the high-speed dispersion reactor, and the stirring reaction was continued for 2-4 h. After the reaction, a sustained-release lecithin microsphere emulsifier was obtained.
[0082] 3. Preparation of water-based anti-corrosion wax that can be sprayed on high-temperature electrophoresis frames:
[0083] Add 0.5kg of monoethanolamine and 35kg of deionized water to a high-speed dispersion reactor, start stirring at a speed of 500-800 rpm, heat to 95°C, add 35kg of high melting point biomass hard wax, continue stirring for 1h, add 5kg of slow-release modified lecithin microsphere emulsifier, continue stirring for 1h, and obtain a water-based anticorrosive wax that can be sprayed on a high-temperature electrophoresis frame. Product performance indicators are shown in Table 1.
[0084] Comparative Example 5 A method for preparing a water-based anticorrosive wax (I) that can be sprayed on a high-temperature electrophoresis vehicle frame is as follows:
[0085] 1. Preparation of high melting point biomass hard wax: same as Example 1.
[0086] 2. Preparation of sustained-release modified lecithin microsphere emulsifier:
[0087] 1) Preparation of organic acid-modified lecithin: same as in Example 1.
[0088] 2) Preparation of amino-functionalized macroporous graphene: 40 kg of graphene oxide powder with a carbon-oxygen ratio of 1.5:1 and 30 kg of mixed acid aqueous solution (mass ratio is sulfuric acid: nitric acid: water = 7:1:2) are added to the reactor, the stirring speed is 20 rpm, the temperature is raised to 40°C under stirring, the reaction is stirred for 4 hours, and the product is filtered after the reaction is completed, and then washed with ice water mixture 3 times, and washed and dried to obtain macroporous graphene oxide powder. 30 kg of macroporous graphene oxide powder is added to 20 kg of ethylenediamine, the stirring speed is 20 rpm, the reaction is stirred at room temperature for 1 hour, and the product is filtered and dried after the reaction is completed to obtain amino-functionalized macroporous graphene oxide.
[0089] 3) Preparation of sustained-release modified lecithin microsphere emulsifier: 50 kg of deionized water and 30 kg of organic acid-modified lecithin are added to a high-speed dispersion reactor with a stirring speed of 2000 rpm. The mixture is stirred and dispersed at room temperature for 1 h. Then 3 parts of amino-functionalized macroporous graphene oxide are added. The stirring speed is increased to 3000 rpm and the mixture is stirred and dispersed for 1 h. Then 100 g of phthaloyl chloride is slowly added dropwise and the reaction is continued with stirring for 2-4 h. After the reaction is completed, a sustained-release modified lecithin microsphere emulsifier is obtained.
[0090] 3. Preparation of water-based anti-corrosion wax that can be sprayed on high-temperature electrophoresis frames:
[0091] Add 0.5kg of monoethanolamine and 35kg of deionized water to a high-speed dispersion reactor, start stirring at a speed of 500-800 rpm, heat to 95°C, add 35kg of high melting point biomass hard wax, continue stirring for 1h, add 5kg of slow-release modified lecithin microsphere emulsifier and 5kg of proanthocyanidins, continue stirring for 1h, and obtain a water-based anticorrosive wax that can be sprayed on a high-temperature electrophoresis frame. Product performance indicators are shown in Table 1.
[0092] Example 6 Application
[0093] 1. The spraying effect of the product on the high temperature substrate is to use the mixed air spraying method on the hot rolled electrophoretic steel plate coated at 90℃. The test results of the dryness of the wax liquid are shown in Table 1.
[0094] 2. Method: Take the coated hot-rolled electrophoretic steel plate, clean it until the surface is clean, and evenly apply the water-based anti-corrosion wax that can be sprayed on the electrophoretic frame prepared in Examples 1-3 and Comparative Examples 1-5 on the surface. After the wax coating layer is completely dried, the initial water resistance, dry film dropping point, pencil hardness, water resistance, and artificial ultraviolet aging are tested. The specific results are shown in Table 1.
[0095] 3. Method: Take a cold-rolled steel plate, degrease it, and then evenly coat the surface with the water-based anti-corrosion wax that can be sprayed on the electrophoretic frame prepared in Examples 1-3 and Comparative Examples 1-5, respectively. After the wax coating layer is completely dried, the salt spray resistance performance is tested. The specific results are shown in Table 1.
[0096] 4. Product physical properties: Viscosity stability was checked in a constant temperature box at 50°C, and emulsification stability was checked at room temperature. The specific results are shown in Table 1.
[0097] Table 1
[0098]
[0099] As can be seen from Table 1, the water-based anticorrosive wax prepared by the present invention that can be sprayed on a high-temperature electrophoresis frame, when the ratio of wax to emulsifier reaches 35:5 (Example 2), the water-based anticorrosive wax prepared by the material of the present invention that can be sprayed on a high-temperature electrophoresis frame has significantly enhanced spraying effect on a high-temperature substrate, initial water resistance, wax film drying (90°C), dry film dropping point, pencil hardness, neutral salt spray test (50μm), water resistance, artificial ultraviolet aging (1000h), viscosity stability and emulsification stability. The water-based anticorrosive wax prepared by Example 2 that can be sprayed on a high-temperature electrophoresis frame has better properties listed in Table 1 than Comparative Example 1, which shows that the palmitic acid-modified Brazilian palm wax technical means used in the present invention improves the molecular chain length, crystallinity, melting point, anticorrosiveness and hardness of the wax, which makes the water-based anticorrosive wax of the present invention have better hardness, improves scratch resistance, and can better protect the electrophoresis frame and chassis. In Comparative Example 2, since palmitic acid-modified Brazilian palm wax is not used, the performance in terms of workability, hardness, and corrosion resistance is relatively poor. Compared with Comparative Example 3, it can be explained that the slow-release emulsifier prepared by the present invention using amino-oxidized graphene with a macroporous structure can effectively solve the problem of workability on high-temperature substrates and effectively solve the film-forming defects caused by water vapor closure. In Comparative Example 4, since the macroporous graphene is not amino-functionalized, the emulsifier system cannot be bonded and fixed with the electrophoretic paint when the water-based anti-corrosion wax is formed, which causes the emulsifier to migrate to the surface of the wax film. Therefore, not only is the product stability poor, but also the film-forming corrosion resistance and water resistance are also poor. In Comparative Example 5, since the anti-ultraviolet aging proanthocyanidin is not fixed to the emulsifier through hydrogen bonding, the dispersibility is extremely poor, which affects the stability and protective effect of the entire product.
Claims
1. A water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis frame, characterized in that: The method comprises the following components in proportion by weight:
2. The water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis vehicle frame according to claim 1, characterized in that: The preparation method of the high melting point biomass hard wax comprises the following steps: adding 30-40 parts of carnauba wax and 20-40 parts of mixed organic solvent into a reaction kettle, starting stirring, controlling the temperature at 25-37°C, adding 5-8 parts of palmitic acid, continuing stirring, then adding 15-20 parts of Pseudomonas aqueous dispersion, continuing stirring for reaction, and finally raising the temperature of the reaction kettle to 100-110°C, evacuating the kettle to a pressure of -0.1-0.08mPa, stirring, and discharging to obtain the high melting point biomass hard wax.
3. The water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis vehicle frame according to claim 2, characterized in that: The mixed organic solvent is a combination of ethyl acetate and propylene glycol butyl ether, and the mass ratio is ethyl acetate:propylene glycol butyl ether=1-3:5; the Pseudomonas aqueous dispersion is a Pseudomonas aeruginosa aqueous dispersion with a pH value of 6.5-7.5 and a live bacteria concentration of 1000000 CFU / mL.
4. The water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis vehicle frame according to claim 1, characterized in that: The preparation method of the sustained-release modified lecithin microsphere emulsifier comprises the following steps: 1) Organic acid modified lecithin: 10-20 parts of organic acid and 30-40 parts of dimethylformamide are added to a stirring tank, stirred at room temperature for a period of time, then 0.2-0.4 parts of organic acid activator are added, stirred at 20-25° C., then 0.1-0.2 parts of deionized water and 30-50 parts of lecithin are added, the reaction temperature is raised to 50-60° C., stirred, and finally the above materials are vacuum dried to obtain organic acid modified lecithin; 2) Amino-functionalized macroporous graphene oxide: 40-60 parts of graphene oxide powder and 30-40 parts of mixed acid aqueous solution are added to a reactor, heated to 40-55° C. under stirring, and stirred for reaction. After the reaction is completed, the product is filtered, washed, and dried to obtain macroporous graphene oxide powder. 30-50 parts of macroporous graphene oxide powder are added to 20-30 parts of ethylenediamine, and stirred at room temperature for reaction. After the reaction is completed, the product is filtered and dried to obtain amino-functionalized macroporous graphene oxide; 3) Sustained-release modified lecithin microsphere emulsifier: Take 50-60 parts of deionized water and 30-45 parts of organic acid modified lecithin, add them to a high-speed dispersion reactor, stir and disperse at room temperature, add 3-6 parts of amino-functionalized macroporous graphene oxide, stir and disperse, then slowly drop 0.1-0.3 parts of phthaloyl chloride, stir and react at room temperature, finally add 5-8 parts of proanthocyanidins to the high-speed dispersion reactor, continue stirring and reacting, and obtain a sustained-release modified lecithin microsphere emulsifier after the reaction is completed.
5. The water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis vehicle frame according to claim 4, characterized in that: The organic acid is a combination of palmitic acid and cerotic acid; in terms of mass ratio, palmitic acid:cerotic acid=10-20:
1.
6. The water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis vehicle frame according to claim 4, characterized in that: The organic acid activator is a combination of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysulfosuccinimide; in terms of mass ratio, 1-ethyl-(3-dimethylaminopropyl)carbodiimide:N-hydroxysulfosuccinimide=1:2-5.
7. The water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis vehicle frame according to claim 4, characterized in that: The graphene oxide powder is graphene oxide with an oxidation degree of carbon-oxygen ratio between 1 and 2:
1.
8. The water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoresis vehicle frame according to claim 4, characterized in that: The mixed acid aqueous solution is a combination of sulfuric acid, nitric acid and water; in terms of mass ratio, sulfuric acid: nitric acid: water = 7-8: 1:
2.
9. A method for preparing a water-based anticorrosive wax that can be sprayed on a high-temperature electrophoresis vehicle frame according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: adding monoethanolamine and deionized water into a high-speed dispersion reactor, starting stirring, heating to 90-95°C, adding high-melting-point biomass hard wax, continuing stirring, adding a slow-release modified lecithin microsphere emulsifier, stirring, and obtaining a water-based anticorrosive wax that can be sprayed on a high-temperature electrophoresis frame.
10. Use of the water-based anti-corrosion wax that can be sprayed on a high-temperature electrophoretic frame as claimed in claim 1 in preparing metal surface anti-corrosion wax for electrophoretic frames and chassis surfaces of commercial vehicles.