Mixed molten salt with low melting point and high decomposition temperature and preparation method thereof

By mixing potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate in specific proportions, and adopting staged heating, melting and drying steps to prepare, the problem of the lack of low-cost, low-melting-point, high-decomposition-temperature mixed molten salts in the prior art is solved. The combination of low melting point and high decomposition temperature of molten salt is achieved, improving thermal energy storage efficiency and application range.

CN118745331APending Publication Date: 2024-10-08INNER MONGOLIA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410744497.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing technology lacks low-cost mixed molten salts with low melting point and high decomposition temperature, which cannot meet the needs of high-temperature applications above 600°C.

Method used

By mixing potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate in a specific mass ratio, and using staged heating, melting and drying steps to prepare a low melting point and high decomposition temperature mixed molten salt with a melting point less than 150°C and a decomposition temperature greater than 680°C. .

Benefits of technology

It achieves an expansion of the liquid use range of molten salt, improves thermal energy storage efficiency, and provides a new thermal storage material with a wider operating temperature range for high-temperature industrial heat transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745331A_ABST
    Figure CN118745331A_ABST
Patent Text Reader

Abstract

The invention discloses a low-melting-point high-decomposition-temperature mixed molten salt and a preparation method thereof, and belongs to the technical field of physical heat transfer and energy storage. The low-melting-point high-decomposition-temperature mixed molten salt is prepared from the following raw materials: potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate, wherein the mass ratio of the potassium nitrate to the sodium nitrate to the sodium nitrite to the calcium nitrate is 5: 2: 1: 2 or 5: 2: 2: 1. The low-cost, low-melting-point and high-decomposition-temperature mixed molten salt with the melting point lower than 150 DEG C and the decomposition temperature higher than 680 DEG C is prepared by changing the components of the mixed molten nitrate salt and the mass ratio of different components, so that the liquid use range of the mixed molten salt is widened, and the heat energy storage efficiency of the molten salt is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of physical heat transfer and energy storage, and in particular to a mixed molten salt with a low melting point and a high decomposition temperature and a preparation method thereof. Background Art

[0002] In thermal energy storage, the use of phase change materials is a very efficient way of energy storage, and molten salt has the advantages of a wide liquid temperature range (200-600°C), high operating temperature (200-800°C), good heat transfer performance, low viscosity, low cost, and low vapor pressure. It is an ideal high-temperature heat transfer and heat storage medium. Molten salt as a high-temperature heat transfer and heat storage medium has been used in large capacity and for a long time in the fields of solar thermal power generation, high-temperature industrial heat transfer, molten salt heat storage heating and power generation.

[0003] In terms of the preparation of mixed molten salt heat transfer and storage materials, the solar thermal power stations currently built and operated at home and abroad all use Solar Salt and Hetic Salt as heat transfer and storage media. Among them, Solar Salt has a high melting point (220°C), is easy to freeze and block pipelines, has a decomposition temperature of 585°C, and cannot be used above 600°C. Hitec salt has a melting point of 142°C, has a high operating temperature and excellent thermal conductivity, and has been widely used in high-temperature industrial heat transfer, but the sodium nitrite in Hitec salt will decompose at 454-538°C. Some scholars have adjusted the component ratio by adding carbonates on the basis of Solar salt, and prepared a mixed molten salt with a melting point of 100°C and a decomposition temperature of about 600°C. It was found that the higher the mass fraction of carbonate, the higher the melting point and decomposition temperature of the mixed salt. Some scholars gradually added up to 50% molar chloride (NaCl, KCl) of the same cation on the basis of Solar salt, and measured the melting point at about 220°C by DSC and TG tests on the mixed molten salt. The decomposition temperature increased with the increase of chloride content. When the chloride content was 50 mol%, the decomposition temperature was 642°C. Some scholars used Solar salt as the base salt, reduced the melting point of the molten salt to 157.4°C by adding Mg(NO3)2, and determined the optimal ratio of 17.5% Mg(NO3)2+49.5% NaNO3+33% KNO3.

[0004] In summary, mixed nitrates, mixed carbonates and mixed chlorides have been studied in depth at home and abroad, but there is a lack of research on low-cost, low-melting-point, high-decomposition-temperature mixed molten salts with a melting point less than 150°C and a decomposition temperature greater than 680°C. Summary of the invention

[0005] The purpose of the present invention is to provide a mixed molten salt with low melting point and high decomposition temperature and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art.

[0006] To achieve the above object, the present invention provides the following solutions:

[0007] One of the technical solutions of the present invention is a mixed molten salt with a low melting point and a high decomposition temperature, wherein the raw materials are composed of potassium nitrate (KNO3), sodium nitrate (NaNO3), sodium nitrite (NaNO2) and calcium nitrate (Ca(NO3)2), and the mass ratio of potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate is 5:2:1:2 or 5:2:2:1. That is, in terms of mass ratio, potassium nitrate: sodium nitrate: sodium nitrite: calcium nitrate = 5:2:1:2 or 5:2:2:1.

[0008] Furthermore, the melting point of the low-melting-point and high-decomposition-temperature mixed molten salt is less than 150°C, and the decomposition temperature is greater than 680°C.

[0009] The different crystal structures and atomic sizes of the components in the eutectic system will cause changes in the crystal ionic bonds during the mixed melting process, making the melting point of the mixed molten salt lower than that of the pure component substances. The present invention reduces the melting point by adding sodium nitrite (sodium ions have an 8-electron configuration, and the polarization effect of sodium ions is greater than that of sodium ions, so there are more covalent bond components, smaller lattice energy, and lower melting point). In addition, NO2 - The addition of can increase the decomposition temperature.

[0010] The second technical solution of the present invention: A method for preparing the above-mentioned low melting point and high decomposition temperature mixed molten salt, comprising the following steps: mixing and grinding potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate to obtain a mixed salt; heating and melting the mixed salt in stages, and then cooling to obtain the low melting point and high decomposition temperature mixed molten salt.

[0011] Furthermore, the grinding time is 1 hour.

[0012] Furthermore, the specific operation of the staged heating and melting is: heating to 350°C at a heating rate of 10°C / min, keeping the temperature constant for 12 hours, and then continuing to heat to 450°C at a heating rate of 10°C / min, and keeping the temperature constant for 2 hours.

[0013] The first stage is to completely evaporate the crystal water in the mixture to prevent salt climbing, and the second stage is to completely melt and mix all the substances under high temperature conditions. Heating in two stages can prevent the temperature from rising rapidly to the decomposition point of a component during the melting process, causing decomposition in the mixed salt, thereby improving the stability and heat transfer performance of the mixed molten salt.

[0014] Furthermore, before the mixed salt is heated and melted in stages, a constant temperature drying step of the mixed salt is also included, specifically, constant temperature drying at 100° C. for 12 hours.

[0015] Furthermore, the step of mixing and grinding potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate also includes a constant temperature drying step for each raw material, specifically, constant temperature drying at 100° C. for 48 hours.

[0016] The present invention discloses the following technical effects:

[0017] The present invention prepares a low-cost, low-melting-point, high-decomposition-temperature mixed molten salt with a melting point of less than 150°C and a decomposition temperature of more than 680°C by changing the components of the mixed nitrate molten salt and the mass ratio of different components, thereby increasing the liquid use range of the mixed molten salt and facilitating improving the thermal energy storage efficiency of the molten salt.

[0018] The present invention develops a molten salt combination with a wide operating temperature range, providing a theoretical basis for the development of new thermal storage materials with high operating temperatures. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 The DSC diagram of the mixed molten salt prepared in Example 1 of the present invention;

[0021] Figure 2 TG curve of the mixed molten salt prepared in Example 1 of the present invention;

[0022] Figure 3 The DSC diagram of the mixed molten salt prepared in Example 2 of the present invention;

[0023] Figure 4 TG curve of the mixed molten salt prepared in Example 2 of the present invention;

[0024] Figure 5 The DSC graph of the mixed molten salt prepared in Comparative Example 1 of the present invention;

[0025] Figure 6 TG curve of the mixed molten salt prepared in Comparative Example 1 of the present invention;

[0026] Figure 7 The DSC graph of the mixed molten salt prepared in Comparative Example 2 of the present invention;

[0027] Figure 8 This is the TG curve of the mixed molten salt prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0029] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0030] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0031] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0032] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0033] The invention discloses a low melting point and high decomposition temperature mixed molten salt, wherein the raw materials are composed of potassium nitrate (KNO3), sodium nitrate (NaNO3), sodium nitrite (NaNO2) and calcium nitrate (Ca(NO3)2), wherein the mass ratio of the potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate is 5:2:1:2 or 5:2:2:1. That is, in terms of mass ratio, potassium nitrate: sodium nitrate: sodium nitrite: calcium nitrate = 5:2:1:2 or 5:2:2:1.

[0034] As a preferred embodiment of the present invention, the melting point of the low melting point and high decomposition temperature mixed molten salt is less than 150°C, and the decomposition temperature is greater than 680°C.

[0035] The present invention also provides a method for preparing the above-mentioned low-melting-point and high-decomposition-temperature mixed molten salt, comprising the following steps: mixing and grinding potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate to obtain a mixed salt; heating and melting the mixed salt in stages, and then cooling to obtain the low-melting-point and high-decomposition-temperature mixed molten salt.

[0036] As a preferred embodiment of the present invention, the grinding time is 1 hour.

[0037] As a preferred embodiment of the present invention, the specific operation of the staged heating and melting is: heating to 350°C at a heating rate of 10°C / min, keeping the temperature constant for 12 hours, and then continuing to heat to 450°C at a heating rate of 10°C / min and keeping the temperature constant for 2 hours.

[0038] The first stage is to completely evaporate the crystal water in the mixture to prevent salt climbing, and the second stage is to completely melt and mix evenly under high temperature conditions. The reason for heating twice is that during the melting process, it is important to note that the temperature should not rise to its decomposition point, which would cause decomposition in the mixed salt.

[0039] As a preferred embodiment of the present invention, before the mixed salt is heated and melted in stages, a constant temperature drying step of the mixed salt is also included, specifically, constant temperature drying at 100° C. for 12 hours.

[0040] As a preferred embodiment of the present invention, the process of mixing and grinding potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate also includes a constant temperature drying step for each raw material, specifically, constant temperature drying at 100° C. for 48 hours.

[0041] The low melting point and high decomposition temperature mixed molten salt of the present invention is further described below in conjunction with specific examples.

[0042] Example 1

[0043] A mixed molten salt with low melting point and high decomposition temperature

[0044] The raw material composition is:

[0045] By mass ratio, potassium nitrate: sodium nitrate: sodium nitrite: calcium nitrate = 5:2:1:2.

[0046] The preparation steps are:

[0047] The raw materials potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate are placed in a drying oven at a constant temperature of 100°C and dried for 48 hours. After the dried potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate are cooled to room temperature, they are weighed on an electronic balance according to the mass ratio of different components, mixed and put into a mortar and fully ground for 1 hour to obtain a mixed salt; the mixed salt is put into a corundum crucible, and then placed in a drying oven for constant temperature drying, the heating temperature is set to 100°C, and the constant temperature time is 12 hours; the cooled mixed salt is then placed in a muffle furnace and heated to 350°C at a heating rate of 10°C / min, and after keeping the temperature constant for 12 hours, the muffle furnace is continuously heated to 450°C at a heating rate of 10°C / min and kept at the temperature constant for 2 hours to completely melt the mixed salt and mix it evenly; after cooling, it is taken out and ground in a mortar for 2 hours to obtain a mixed molten salt; finally, the crushed mixed molten salt is placed in a drying oven at a constant temperature of 100°C and dried for use in experiments.

[0048] Figure 1 The DSC (differential scanning calorimetry) diagram of the mixed molten salt prepared in Example 1 is shown in FIG. Figure 1 It can be seen that the melting point of the mixed molten salt is 149.98°C.

[0049] Figure 2 is the TG (thermogravimetric analysis) curve of the mixed molten salt obtained in Example 1, Figure 2 It can be seen that the decomposition temperature of the mixed molten salt is 698.3°C. When the temperature rises to 799.4°C, the mass of the mixed molten salt loses 74.66%.

[0050] Example 2

[0051] A mixed molten salt

[0052] The raw material composition is:

[0053] Calculated by mass ratio, potassium nitrate: sodium nitrate: sodium nitrite: calcium nitrate = 5:2:2:1.

[0054] The preparation steps are the same as in Example 1.

[0055] Figure 3 The DSC (differential scanning calorimetry) diagram of the mixed molten salt prepared in Example 2 is shown in FIG. Figure 3 It can be seen that the melting point of the mixed molten salt is 91.61°C.

[0056] Figure 4 is the TG (thermogravimetric analysis) curve of the mixed molten salt obtained in Example 2, Figure 4 It can be seen that the decomposition temperature of the mixed molten salt is 703.8°C.

[0057] Comparative Example 1

[0058] A mixed molten salt

[0059] The raw material composition is:

[0060] Calculated by mass ratio: potassium nitrate: sodium nitrate: sodium nitrite: calcium nitrate = 5:1:1:2.

[0061] The preparation steps are the same as in Example 1.

[0062] Figure 5 The DSC (differential scanning calorimetry) diagram of the mixed molten salt prepared in Comparative Example 1 is shown in FIG. Figure 5 It can be seen that the melting point of the mixed molten salt is 147.23°C.

[0063] Figure 6 The TG (thermogravimetric analysis) curve of the mixed molten salt prepared in Comparative Example 1 is shown in FIG. Figure 6 It can be seen that the decomposition temperature of the mixed molten salt is 616.1°C.

[0064] Comparative Example 2

[0065] A mixed molten salt

[0066] The raw material composition is:

[0067] Calculated by mass ratio, potassium nitrate: sodium nitrate: sodium nitrite: calcium nitrate = 6:1:1:2.

[0068] The preparation steps are the same as in Example 1.

[0069] Figure 7 The DSC (differential scanning calorimetry) diagram of the mixed molten salt prepared in Comparative Example 2 is shown in FIG. Figure 7 It can be seen that the melting point of the mixed molten salt is 148.89°C.

[0070] Figure 8 The TG (thermogravimetric analysis) curve of the mixed molten salt obtained in Comparative Example 2 is shown in FIG. Figure 8 It can be seen that the decomposition temperature of the mixed molten salt is 668°C.

[0071] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A mixed molten salt with a low melting point and a high decomposition temperature, characterized in that: The raw materials consist of potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate, and the mass ratio of the potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate is 5:2:1:2 or 5:2:2:

1.

2. The low melting point and high decomposition temperature mixed molten salt according to claim 1, characterized in that: The low melting point and high decomposition temperature mixed molten salt has a melting point of less than 150°C and a decomposition temperature of greater than 680°C.

3. A method for preparing a low melting point and high decomposition temperature mixed molten salt as claimed in claim 1 or 2, characterized in that: The following steps are involved: Potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate are mixed and ground to obtain a mixed salt; the mixed salt is heated and melted in stages, and then cooled to obtain the mixed molten salt with a low melting point and a high decomposition temperature.

4. The low melting point and high decomposition temperature mixed molten salt according to claim 3, characterized in that: The grinding time is 1 h.

5. The low melting point and high decomposition temperature mixed molten salt according to claim 3, characterized in that: The specific operation of the staged heating and melting is: heating to 350°C at a heating rate of 10°C / min, keeping the temperature constant for 12 hours, and then continuing to heat to 450°C at a heating rate of 10°C / min, and keeping the temperature constant for 2 hours.

6. The low melting point and high decomposition temperature mixed molten salt according to claim 3, characterized in that: Before the mixed salt is heated and melted in stages, a constant temperature drying step of the mixed salt is also included, specifically, constant temperature drying at 100° C. for 12 hours.

7. The low melting point and high decomposition temperature mixed molten salt according to claim 3, characterized in that: The method further includes a constant temperature drying step for each raw material before mixing and grinding potassium nitrate, sodium nitrate, sodium nitrite and calcium nitrate, specifically, constant temperature drying at 100° C. for 48 hours.