Ultralow-alkalinity sintered ore for replacing pellet ore for blast furnace and production and application method of ultralow-alkalinity sintered ore

By using ultra-low alkalinity sinter to replace traditional acidic pellets in the blast furnace, the cost of molten iron is reduced and the metallurgical performance is improved. The problem of high pellet costs is solved, and dual optimization of cost and performance is achieved.

CN118745490APending Publication Date: 2024-10-08YANCHENG LIANXIN IRON & STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410860349.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The production cost of pellets in existing blast furnace smelting is high and unstable, resulting in a corresponding increase in the cost of molten iron, threatening the profits and survival of long-process steel companies.

Method used

Using an ultra-low alkalinity sinter, by mixing iron ore powder, lightly burned dolomite and coal powder, and controlling the sintering parameters to reduce the alkalinity and increase the iron content, a sinter with excellent metallurgical properties is formed, replacing traditional acidic pellets. mine.

Benefits of technology

The batching cost of the blast furnace has been significantly reduced, the cost of molten iron has been reduced by about 40 yuan/ton, and the annual benefits have exceeded 160 million yuan. At the same time, the metallurgical performance of the blast furnace and the smooth operation of the furnace conditions have been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses ultralow-alkalinity sintered ore replacing pellets for a blast furnace and a production and application method of the ultralow-alkalinity sintered ore, and relates to the field of blast furnace burden, the ultralow-alkalinity sintered ore comprises the following raw materials: iron ore powder, light-burned dolomite and pulverized coal, the content of the pulverized coal accounts for 4.8-5.1% of the total mass of the raw materials, the content of the iron ore powder accounts for 92-93% of the total mass of the raw materials, and the content of the light-burned dolomite powder accounts for 1.95-2.80% of the total mass of the raw materials; according to the batching principle of the low-alkalinity sintered ore, the standard binary alkalinity R2 is controlled to be 0.3-0.38 times, the quaternary alkalinity R4 is controlled to be larger than 0.40 times, the SiO2 content is 6.90-7.20%, the TFe content is larger than or equal to 61.00%, the Al2O3 / SiO2 content is 0.20-0.22 times, and the MgO / Al2O3 content is 0.90-1.14 times. The raw materials are sintered through a sintering machine to obtain the ultralow-alkalinity sintered ore. And the high-temperature metallurgical performance of the ultralow-alkalinity sintered ore is superior to that of pellet ore, and smooth operation of the furnace condition of a blast furnace is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of blast furnace charge materials, and in particular relates to an ultra-low basicity sintered ore that can replace pelletized ore for blast furnaces and a production and application method thereof. Background Art

[0002] As iron ore resources become increasingly scarce, especially high-grade iron ore, and environmental pressure continues to increase, the production cost of iron ore concentrate for pelletizing has been further pushed up, causing its purchase price to increase accordingly. The cost of long-process steel enterprises has increased, and the profit margin has been continuously compressed, which directly threatens the survival of enterprises. Therefore, new technologies and processes to replace blast furnace pellets are an inevitable trend for enterprises to reduce costs and develop production.

[0003] The existing technology is: the current charge structure of the blast furnace is basically: basic sintered ore + acidic pellets + lump ore, among which the proportion of basic sintered ore is about 74%, the proportion of acidic pellets is about 13%, and the proportion of lump ore is about 13%, that is, the clinker rate of the blast furnace is about 87%.

[0004] The existing technical solution is reasonable from the perspective of blast furnace smelting itself, but its disadvantage is that the main raw material of acidic pellets is iron ore concentrate. Iron ore concentrate is obtained by grinding iron ore powder (0-10mm) very finely and magnetic separation. The magnetic separation process will produce pollutants such as tailings and wastewater, and magnetic separation will result in different total iron content and gangue component content. Due to the shortage of upstream iron ore concentrate resources, high prices and large fluctuations, the price of acidic pellets is high and the stability is poor, which in turn causes the price of blast furnace iron to be high and fluctuate greatly, which brings great risks to the company's profits and long-term stable profitability. Summary of the invention

[0005] The technical problem solved by the present application is: to overcome the shortcomings of the prior art and provide a production method to replace pellets for blast furnaces, to replace pellets for blast furnace production, to reduce the blast furnace batching cost, thereby achieving the purpose of reducing molten iron costs, and is one of the most important measures to reduce the cost of long-process steel enterprises.

[0006] The technical solutions provided by this application are as follows:

[0007] The invention discloses an ultra-low basicity sintered ore which can replace pelletized ore for blast furnace, comprising the following raw materials: mixed iron ore powder, light-burned dolomite and coal powder, wherein the content of coal powder is 4.8-5.1% of the total mass of the raw materials, the content of mixed iron ore powder is 92-93% of the total mass of the raw materials, and the content of light-burned dolomite powder is 1.95-2.80% of the total mass of the raw materials; the above raw materials are sintered by a sintering machine to obtain the ultra-low basicity sintered ore; the control parameters of the low basicity sintered ore are: the reference binary basicity R2 is controlled at 0.3-0.38 times, the quaternary basicity R4 is controlled at more than 0.40 times, the SiO2 content is 6.90-7.20%, the TFe content is greater than or equal to 61.00%, the Al2O3 / SiO2 is 0.20-0.22 times, and the MgO / Al2O3 is 0.90-1.14 times.

[0008] Taking the mass of the mixed iron ore powder as 100%, the content of TFe is 61.93-62.50%, the content of SiO2 is 6.78-6.90%, the content of Al2O3 is 1.40-1.60%, the content of CaO is 0.92-1.10%, the content of MgO is 0.55-0.70%, the content of TiO2 is not more than 0.160%, the content of K2O+Na2O is not more than 0.090%, the content of Zn is not more than 0.010%, the content of Pb is not more than 0.030%, and the LOI is 2.65-3.20%.

[0009] Taking the mass of the light-burned dolomite as 100%, the content of SiO2 is 0.80-1.10%, the content of CaO is 53.00-55.00%, and the content of MgO is 34.00-36.00%.

[0010] Taking the mass of the coal powder as 100%, the fixed carbon content is greater than 80.00%, the ash content is not greater than 12.00%, and the volatile matter is not greater than 6.00%; in addition, the proportion of coal powder with a particle size less than 3 mm is greater than 75.00%, and the low calorific value is greater than 6600 Cal / g.

[0011] In the above raw material setting, due to the high gangue content in the mixture, the main bonding phases formed during the sintering process are iron olivine (2FeO.SiO2), calcium iron olivine (Ca.FeO.SiO2), glass quality and a small amount of free SiO2, etc. However, calcium ferrite cannot be formed in the process of producing ultra-low basicity acidic sintered ore. The consolidation of the ores into blocks is mainly achieved through the bonding phase, and the sintered ore is formed after cooling. It has the disadvantages of brittleness, poor drum strength, poor reduction phase, poor high-temperature softening and melting performance, poor permeability of the sintering material layer, and no powdering; therefore, appropriately increasing the ferrous oxide content of the ultra-low basicity sintered ore increases the strength of the sintered ore and improves the metallurgical properties, but the excessive ferrous oxide content causes excessive solid fuel consumption and a U-shaped process in which the reducibility first increases, then decreases, and then increases as the ferrous oxide content increases from low to high, which is also verified by laboratory and industrial tests. The limitation of the ferrous oxide content in this patent makes the reducibility at the top of the U-shaped process.

[0012] The basicity, chemical composition, aluminum-silicon ratio and magnesium-aluminum ratio required for ultra-low basicity sintered ore are achieved by batching within the specified range.

[0013] Through the calorific value of coal powder and the sintering performance of iron ore, the most suitable ratio of coal powder is obtained through sintering cup experiments and industrial tests, that is, the lowest ratio that satisfies the mineralization of raw materials and generates sufficient binding phase, so as to achieve the purpose of energy saving.

[0014] The binary basicity R2 of the ultra-low basicity sintered ore is 0.30 to 0.38 times, and the quaternary basicity R4 is 0.40 to 0.52 times.

[0015] In the ultra-low basicity sintered ore, the TFe content is 61.00-62.20%, the FeO content is 14.00-17.00%, the SiO2 content is controlled at 6.90-7.20%, and the drum index is ≥69.0%.

[0016] The particle size of the ultra-low basicity sintered ore is ≥60% of 10-40 mm, <10% of greater than 50 mm, and <10% of less than 10 mm. The particle size of the ultra-low basicity sintered ore is achieved by controlling the size of the sieve plate in the crushing and screening workshop to achieve the required particle size requirements. By controlling the particle size, the permeability of the upper part (block belt) of the blast furnace smelting is improved, the furnace condition is promoted to run smoothly, and conditions are created to obtain better smelting indicators.

[0017] The metallurgical properties of ultra-low basicity sintered ore are better than those of acidic pellets. The softening start temperature of ultra-low basicity sintered ore is greater than 1150℃, which is higher than the softening start temperature of pellets, which is 1050~1100℃. Therefore, ultra-low basicity sintered ore is more conducive to improving the permeability of the upper part of the blast furnace, which is conducive to the smooth operation of the blast furnace, improving indicators and reducing consumption.

[0018] The cost and difficulty of producing ultra-low basicity sintered ore are better than those of acidic pellets. Ultra-low basicity sintered ore can be mixed with a variety of iron ore powders, the composition is easy to control and the cost is low; while the iron ore concentrate required for producing pellets must be magnetic iron ore concentrate, which has a single variety and high cost. The strength of the sintered ore is controlled by controlling the FeO content of the ultra-low basicity sintered ore, thereby reducing the content of powder with a particle size of less than 5 mm.

[0019] The method for producing ultra-low basicity sintered ore as a substitute for blast furnace pellets as described above comprises:

[0020] According to the raw material ratio of iron ore powder, light-burned dolomite and coal powder, the raw materials are sintered by a sintering machine;

[0021] The sintering parameters include: solid fuel ratio 4.8-5.1%, ignition temperature 1130±30°C, trolley speed 29-33Hz, and terminal temperature control 300-350°C.

[0022] The sintering parameters also include: mixed material moisture 6.90-7.20%, material layer thickness 800-900 mm, material surface negative pressure 15.0-16.0 KPa.

[0023] In the above sintering process, the appropriate coal powder ratio provides the heat and reducing agent required for ore mineralization and the formation of a bonding phase; the appropriate ignition temperature ensures the sintering surface mineralization, reduces the amount of surface sintering return ore, and improves the permeability of the material layer. The appropriate trolley speed ensures that the sintering end temperature is within the specified wind box position range, reduces the cooling rate as much as possible, improves the yield rate, and reduces the return rate.

[0024] A method for applying any of the above-mentioned ultra-low basicity sintered ore that can replace pellets for blast furnaces, or any of the above-mentioned ultra-low basicity sintered ore prepared by the production method, as a charge structure, the charge structure includes basic sintered ore, lump ore and the ultra-low basicity sintered ore described in any of the above-mentioned items or the ultra-low basicity sintered ore prepared by the production method described in any of the above-mentioned items, the mass proportion of basic sintered ore is about 70-75%, the mass proportion of ultra-low basicity sintered ore is about 13-20%, and the mass proportion of lump ore is 13-15%.

[0025] 1. Alternative process principle

[0026] The key control indicators of acidic pellets are: binary alkalinity R2 is 0.15-0.35 times, quaternary alkalinity R4 (CaO+MgO) / (SiO2+Al2O3) ≤ 0.5 times, TFe ≥ 62%, drum index ≥ 90%, compressive strength ≥ 2000N / piece. The main raw material is iron ore concentrate, in which: TFe ≥ 65%, particle size -0.044㎜ is greater than 75%, and the roasting equipment is a vertical furnace, a chain grate rotary kiln or a belt roaster.

[0027] Ultra-low basicity sintered ore that replaces acidic pellets: produced by sintering machines, with binary basicity R2 (CaO / SiO2) controlled at 0.30-0.38 times, quaternary basicity R4 (CaO+MgO) / (SiO2+Al2O3) at 0.40-0.52 times, Fe≥61%, drum index greater than 69%, and its main raw material is iron ore powder that meets sintering requirements, and the quality requirements of iron ore powder are much lower than those of iron concentrate. Therefore, it can be completely replaced from the perspective of blast furnace batching, production and economy.

[0028] 2. Ultra-low basicity sinter production process control parameters

[0029] (1) Batching parameters: The binary basicity R2 of ultra-low basicity sinter is controlled at 0.34 times, the quaternary basicity R4 is controlled at 0.4-0.52 times, SiO2 is controlled at 7.0%, TFe ≥ 61.0%, Al2O3 / SiO2 is 0.20-0.22 times, and MgO / Al2O3 is 0.90-1.14 times;

[0030] (2) Process control parameters: solid fuel ratio 4.8-5.1%, ignition temperature 1130±30℃, trolley speed 29-33Hz, mixed material moisture 6.90-7.20%, end point temperature control 300-350℃, material layer thickness 800㎜-900㎜, material surface negative pressure 15.0-16.0KPa.

[0031] (3) Finished product control parameters: R2 is controlled at 0.30-0.38 times, R4 is controlled at 0.40-0.52 times, TFe ≥ 61.0%, Al2O3 / SiO2 is 0.20-0.22 times, MgO / Al2O3 is 0.90-1.14 times, FeO is 14.00-17.00%, SiO2 is controlled at 6.9-7.2%, drum index ≥ 69%, particle size control: the proportion of 10-40 mm is ≥ 60%, the proportion of more than 50 mm is < 10%, and the proportion of less than 10 mm is < 10%.

[0032] 3. Blast furnace charge structure

[0033] The charge structure of the blast furnace is basically: basic sintered ore + ultra-low basicity sintered ore + lump ore, of which the proportion of basic sintered ore is about 71%, the proportion of ultra-low basicity sintered ore is about 16%, and the proportion of lump ore is about 13%. This ensures that the clinker rate of 87% does not change fundamentally.

[0034] In summary, this application at least includes the following beneficial technical effects:

[0035] Since the cost of iron ore powder used in ultra-low basicity sinter is much lower than the price of iron concentrate used in pellets, after actual production, the average annual price difference between ultra-low basicity sinter and pellets is about 300 yuan / ton, affecting the cost of molten iron by about 45 yuan / ton;

[0036] Considering that the quality of ultra-low basicity sintering is somewhat different from that of pellets: the grade is reduced by about 3%, and FeO is increased by about 14%; it has a certain impact on blast furnace smelting: the comprehensive grade of entering the furnace is reduced by about 0.45%, and FeO is increased by about 2.24%, resulting in a 0.5% reduction in output, a 1kg / t increase in coke ratio, and an increase in molten iron cost of about 5 yuan / ton. At the same time, it has been proven in practice that the high-temperature metallurgical properties (softening start temperature is 50-80℃ higher, and the reduction expansion index RSI is low) and slag-making properties (mainly the MgO content of ultra-low basicity sintering is higher than that of acidic pellets) of ultra-low basicity sintering are better than those of pellets, which is conducive to the smooth operation of blast furnace conditions.

[0037] Taking into account the influence of the above two factors, the cost of molten iron is reduced by 45-5=40 yuan / ton, creating annual benefits of more than 160 million yuan, with a significant cost reduction effect. DETAILED DESCRIPTION

[0038] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.

[0039] A method for producing ultra-low basicity sintered ore that replaces pelletized ore for blast furnace, comprising:

[0040] The raw materials of ultra-low basicity sintered ore include: 92-93% of mixed iron ore powder, 2.5-3% of light-burned dolomite powder, and 4.8-5.1% of coal powder, based on the mass sum of all raw materials of ultra-low basicity sintered ore being 100%. The mixed iron ore powder is obtained by mixing one or more iron ore powders. The mixed raw material is obtained by mixing the mixed iron ore powder, light-burned dolomite powder, and coal powder.

[0041] Taking the mass of the light-burned dolomite powder as 100%, the content of SiO2 in the light-burned dolomite powder is 0.8-1.1%, the content of CaO is 53.00-55.00%; and the content of MgO is 34.00-36.00%.

[0042] Taking the mass of the coal powder as 100%, the fixed carbon content is greater than 80.00%, the ash content is not greater than 12.00%, and the volatile matter is not greater than 6.00%; in addition, the proportion of coal powder with a particle size less than 3 mm is greater than 75.00%, and the low calorific value is greater than 6600 Cal / g.

[0043] Taking the mass of the mixed iron ore powder as 100%, the content of TFe is 61.93-62.50%, the content of SiO2 is 6.78-6.90%, the content of Al2O3 is 1.40-1.60%, the content of CaO is 0.92-1.10%, the content of MgO is 0.55-0.70%, the content of TiO2 is not more than 0.160%, the content of K2O+Na2O is not more than 0.090%, the content of Zn is not more than 0.010%, the content of Pb is not more than 0.030%, and LOI is 2.65-3.20%.

[0044] By limiting the raw materials and raw material components of ultra-low basicity sintered ore, the content of TFe in the mixed raw material is 54.27-57.81%, the content of SiO2 is 6.56-6.62%, the content of Al2O3 is 1.43-1.45%, the content of MgO is 1.31-1.63%, the content of CaO is 2.01-2.50%, the content of TiO2 is not more than 0.160%, the content of K2O+Na2O is not more than 0.090%, the content of Zn is not more than 0.010%, the content of Pb is not more than 0.030%, and LOI is 6.67-6.74%.

[0045] The composition content of the ultra-low basicity sintered ore obtained after sintering the raw materials satisfies the following Table 1.

[0046] Table 1: Composition content of ultra-low basicity sintered ore, %

[0047]

[0048] Finished product parameters of ultra-low basicity sintered ore: R2 controlled at 0.30-0.38 times, R4 controlled at 0.40-0.52 times, TFe ≥ 61.0%, Al2O3 / SiO2 0.20-0.22 times, MgO / Al2O3 0.90-1.14 times, FeO14-17%, SiO2 controlled at 6.9-7.2%, drum index ≥ 69%, particle size control: the proportion of 10-40mm is ≥ 60%, the proportion of greater than 50mm is < 10%, and the proportion of less than 10mm is < 10%.

[0049] The production method of ultra-low basicity sintered ore includes:

[0050] S1: Ingredients: Lightly burned dolomite powder is mixed with iron ore powder as a flux containing CaO and MgO, and the standard binary basicity R2 of the ultra-low basicity sintered ore is controlled to be 0.30-0.38 times (preferably 0.34 times), the quaternary basicity R4 is controlled to be 0.40-0.52 times (preferably 0.46 times), SiO2 is controlled to be 6.90-7.20% (preferably 7.00%), TFe is controlled to be greater than or equal to 61.00% (preferably 61.5%), Al2O3 / SiO2 is 0.20-0.22 times (preferably 0.20 times), and MgO / Al2O3 is 0.90-1.14 times (preferably 1.00 times). Coal powder is added as solid fuel, and the solid fuel (coal powder) ratio is 4.80-5.10%.

[0051] According to the needs, the flux is crushed in a ball mill in advance, so that the proportion of light-burned dolomite with a particle size less than 3mm is greater than 90%, and the proportion greater than 5mm is not greater than 5%; after the anthracite is crushed by a double-roll mill and a four-roll mill, the proportion of the part with a particle size less than 3mm used for sintering is greater than 75%; when purchasing iron ore powder, the particle size requirements of the powder ore are: the proportion less than 3mm is not greater than 35.00%, the proportion greater than 10mm is not greater than 10.00%, and the proportion of fine powder greater than -200 mesh is greater than 55.00.

[0052] S2: Add the above iron ore powder, light-burned dolomite powder and coal powder into a sintering machine for sintering, with an ignition temperature of 1130±30℃, a trolley speed of 29-33Hz, a mixed material moisture of 6.90-7.20%, a terminal temperature of 300-350℃, a material layer thickness of 800㎜-900㎜, and a negative pressure of 15.0-16.0KPa. After the sintering process in the sintering machine, an ultra-low basicity sintered ore is obtained.

[0053] Blast furnace charge structure:

[0054] The charge structure of the blast furnace is basically: basic sintered ore + ultra-low basicity sintered ore + lump ore, among which the proportion of basic sintered ore is 70-75%, the proportion of ultra-low basicity sintered ore is 13-20%, and the proportion of lump ore is 13-15%. This ensures that the clinker rate of 86% does not change fundamentally.

[0055] The key points of the technical solution of the present invention are:

[0056] (1) The binary basicity R2 of ultra-low basicity sintered ore is controlled at 0.30-0.38 times to fully meet the blast furnace charge requirements, and its high softening start temperature improves the permeability during blast furnace smelting, which is the basis for achieving process replacement;

[0057] (2) The quaternary basicity R4 of ultra-low basicity sinter is controlled at 0.40 to 0.52 times, which is the prerequisite for reasonable slag making in blast furnaces;

[0058] (3) The key to ensuring the strength and grade of ultra-low basicity sintered ore is to control SiO2 at 6.90-7.20% and R2 at 0.30-0.38 times.

[0059] (4) The key to achieving both binary and quaternary basicity target control of ultra-low basicity sintered ore is the addition of light-burned dolomite powder.

[0060] (5) Slow machine speed and thick material layer are one of the key technical means to achieve energy saving and low consumption in ultra-low basicity sintering.

[0061] The iron ore powder used in the following examples includes TFe 61.94%, SiO2 6.78%, Al2O3 1.50%, CaO0.92%, MgO 0.55%, S 0.040%, P 0.075%, TiO2 0.141%, K2O 0.063%, Na2O 0.017%, Zn0.009%, Pb 0.030%, LOI 2.66%, and H2O 6.34%.

[0062] The lightly burned dolomite powder used in the following examples contains SiO2 0.90%, CaO 55.00%, MgO3 6.00%, Al2O3 0.20%, S 0.15%, P 0.040%, and LOI 10%.

[0063] The coal powder used in the following examples includes SiO2 7.77%, CaO 0.8%, MgO 0.01%, Al2O3 1.0%, S 0.50%, P 0.066%, and LOI 10%.

[0064] Example 1

[0065] A method for producing ultra-low basicity sintered ore that replaces pelletized ore for blast furnaces comprises the following steps:

[0066] S1: 92.14% of iron ore powder (dry basis), 2.55% of light-burned dolomite powder (dry basis), and 5.31% of coal powder (dry basis) are mixed evenly to obtain a mixed raw material;

[0067] The benchmark binary basicity R2 of the mixed raw material is 0.34 times, the quaternary basicity R4 is 0.47 times, the SiO2 content is 6.59%, the TFe content is 57.53%, the MgO / Al2O3 is 1.02 times, the Al2O3 / SiO2 is 0.22 times, the burn loss LOI is 6.71%, and the H2O content is 6.62%.

[0068] S2: adding the mixed raw material obtained in step S1 into a sintering machine for sintering; the sintering parameters include: ignition temperature 1130±30°C, trolley speed 29-33Hz, end temperature control 300-350°C, material layer thickness 800㎜-900㎜, material surface negative pressure 15.0-16.0KPa; ultra-low basicity sintered ore is obtained after sintering.

[0069] A charge structure for a blast furnace includes basic sintered ore + ultra-low basicity sintered ore + lump ore, wherein the mass proportion of the basic sintered ore is 71%, the mass proportion of the ultra-low basicity sintered ore is 16%, and the mass proportion of the lump ore is 13%. According to the above structure, the above raw materials are fed into the blast furnace to obtain molten iron.

[0070] Comparative Example 1

[0071] A charge structure for a blast furnace includes basic sintered ore + acidic pellets + lump ore, wherein the basic sintered ore accounts for 71% by mass, the acidic pellets account for 16% by mass, and the lump ore accounts for 13% by mass. The above raw materials are fed into the blast furnace according to the above structure to obtain molten iron.

[0072] The ultra-low basicity sintered ore obtained in Example 1 was sampled to obtain Sample 1 and Sample 2, and the components of Sample 1 and Sample 2 were tested. The results are shown in Table 2 below.

[0073] Table 2 Component contents of sample 1 and sample 2

[0074]

[0075] The molten iron obtained in Example 1 and Comparative Example 1 was tested for carbon, silicon, sulfur, phosphorus and titanium. The test results are shown in Table 3.

[0076] Table 3 molten iron test results, %

[0077] name [C] [Si] [S] [P] [Ti] Example 1 4.20~4.50 0.30~0.50 0.010~0.025 0.105~0.116 0.030~0.060 Comparative Example 1 4.40~4.70 0.25~0.60 0.013~0.028 0.114~0.125 0.045~0.070

[0078] According to the above test results, the stability of silicon in molten iron is shown in Table 3. The fluctuation range of Si content in molten iron of Example 1 is smaller. When ultra-low basicity sintered ore is used, the composition is easy to control, the high-temperature metallurgical performance is better, and the furnace condition is more stable. Therefore, the silicon, phosphorus, sulfur, etc. of the molten iron obtained in Example 1 are better than those of the molten iron obtained in Comparative Example 1, that is, the molten iron of Example 1 has lower sulfur and phosphorus, and good slag-making performance; the molten iron of Example 1 has lower Ti, which inhibits titanium reduction, so the high-temperature metallurgical performance and slag-making performance of ultra-low basicity sintered ore are better than those of pelletized ore.

[0079] The present application is described in detail above in conjunction with specific implementation methods and exemplary examples, but these descriptions cannot be understood as limiting the present application. Those skilled in the art understand that, without departing from the spirit and scope of the present application, a variety of equivalent replacements, modifications or improvements can be made to the technical solution of the present application and its implementation methods, all of which fall within the scope of the present application. The scope of protection of the present application shall be subject to the attached claims.

[0080] The contents not described in detail in this application specification belong to the common knowledge of those skilled in the art.

Claims

1. An ultra-low basicity sintered ore that replaces pellets for blast furnaces, characterized in that: The raw materials include: mixed iron ore powder, light-burned dolomite and coal powder, wherein the content of coal powder is 4.8-5.1% of the total weight of the raw materials, the content of mixed iron ore powder is 92-93% of the total weight of the raw materials, and the content of light-burned dolomite powder is 2.5-3% of the total weight of the raw materials; the above raw materials are sintered by a sintering machine to obtain ultra-low basicity sintered ore; The control parameters of low-basicity sintered ore are: the benchmark binary basicity R2 is controlled at 0.3-0.38 times, the quaternary basicity R4 is controlled at greater than 0.40 times, the SiO2 content is 6.9-7.2%, the TFe content is greater than or equal to 61.00%, Al2O3 / SiO2 is 0.20-0.22 times, and MgO / Al2O3 is 0.90-1.14 times.

2. The ultra-low basicity sintered ore for replacing blast furnace pellets according to claim 1, characterized in that: The mixed iron ore powder, light-burned dolomite powder and coal powder are mixed to obtain a mixed raw material. In the mixed raw material, the reference binary basicity R2 is controlled to be 0.3-0.38 times, the quaternary basicity R4 is controlled to be greater than 0.40 times, the TFe content is 54.27-57.81%, the SiO2 content is 6.56-6.62%, the Al2O3 content is 1.43-1.45%, the MgO content is 1.31-1.63%, the CaO content is 2.01-2.50%, the TiO2 content is not more than 0.160%, the K2O+Na2O content is not more than 0.090%, and the LOI is 6.67-6.74%.

3. The ultra-low basicity sintered ore for replacing blast furnace pellets according to claim 1, characterized in that: Taking the mass of the mixed iron ore powder as 100%, the content of TFe in the mixed iron ore powder is 61.93-62.50%, the content of SiO2 is 6.78-6.90%, the content of Al2O3 is 1.40-1.60%, the content of CaO is 0.92-1.10%, the content of MgO is 0.55-0.70%, the content of TiO2 is not more than 0.160%, the content of K2O+Na2O is not more than 0.090%, the content of Zn is not more than 0.010%, the content of Pb is not more than 0.030%, and LOI is 2.65-3.20%.

4. The ultra-low basicity sintered ore for replacing blast furnace pellets according to claim 1, characterized in that: Taking the mass of the light-burned dolomite as 100%, the content of SiO2 in the light-burned dolomite is 0.80-1.10%, the content of CaO is 53.00-55.00%, and the content of MgO is 34.00-36.00%.

5. The ultra-low basicity sintered ore for replacing blast furnace pellets according to claim 1, characterized in that: Taking the mass of the coal powder as 100%, the fixed carbon content of the coal powder is greater than 80.00%, the ash content is not greater than 12.00%, and the volatile matter is not greater than 6.00%; in addition, the proportion of coal powder with a particle size less than 3 mm is greater than 75.00%, and the low calorific value is greater than 6600Cal / g.

6. The ultra-low basicity sintered ore for replacing blast furnace pellets according to claim 1, characterized in that: In the ultra-low basicity sintered ore, the TFe content is 61.00-62.20%, the FeO content is 14.00-17.00%, the SiO2 content is controlled at 6.90-7.20%, and the drum index is ≥69.0%.

7. The ultra-low basicity sintered ore for replacing blast furnace pellets according to claim 1, characterized in that: The ultra-low basicity sintered ore has a particle size of 10 to 40 mm, with a proportion of ≥60%, a particle size of greater than 50 mm less than 10%, and a particle size of less than 10 mm less than 10%.

8. The method for producing ultra-low basicity sintered ore replacing blast furnace pellets according to any one of claims 1 to 7, characterized in that: include: According to the raw material ratio of iron ore powder, light-burned dolomite and coal powder, the raw materials are sintered by a sintering machine; The sintering parameters include: solid fuel ratio 4.8-5.1%, ignition temperature 1130±30°C, trolley speed 29-33Hz, and terminal temperature control 300-350°C.

9. The production method according to claim 8, characterized in that: The sintering parameters also include: mixed material moisture 6.90-7.20%, material layer thickness 800 mm-900 mm, material surface negative pressure 15.0-16.0 KPa.

10. The method for using the ultra-low basicity sintered ore replacing blast furnace pellets according to any one of claims 1 to 7, or the ultra-low basicity sintered ore prepared by the production method according to any one of claims 8 to 9, characterized in that: As a charge structure, the charge structure includes basic sintered ore, lump ore and ultra-low basicity sintered ore, the mass proportion of basic sintered ore is 70-75%, the mass proportion of ultra-low basicity sintered ore is 13-20%, and the mass proportion of lump ore is 13-15%, and the ultra-low basicity sintered ore is the ultra-low basicity sintered ore described in any one of claims 1-7 or is produced by the production method described in any one of claims 8-9.

Citation Information

Cited By

  • Flux pellet preparation method suitable for gas-based shaft furnace smelting and formula determination method