Staged loading method of waste steel for converter
By adopting the method of loading scrap steel in stages during converter smelting, and gradually adding scrap steel according to the oxygen supply conditions, the problems of low smelting efficiency and inaccurate temperature control caused by the one-time addition of scrap steel are solved, and a more efficient smelting process and More stable endpoint temperature control.
Patent Information
- Application Number
- CN202410790792.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-08
AI Technical Summary
In the existing converter smelting technology, the full amount of scrap steel is added at one time, which causes the temperature of the molten iron to rise slowly in the early stage of smelting, prolongs the decarburization reaction time, affects the smelting efficiency and the melting of slagging materials, and makes it difficult to accurately control the end temperature.
The method of loading scrap steel in stages is adopted, and scrap steel is gradually added under different oxygen supply conditions. The amount of scrap steel is accurately controlled according to the heat balance calculation of the converter, and the thermal effect and carbon-oxygen reaction process are optimized.
It improves the smelting efficiency, shortens the smelting time, ensures precise control of the smelting end point temperature, avoids temperature fluctuations, and improves the protective effect of the furnace lining.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method for charging scrap steel into a converter in stages. Background Art
[0002] Scrap steel is one of the main raw materials for converter steelmaking. Its main purpose is to serve as a coolant to adjust the temperature of molten steel. In the existing converter smelting technology, the method of adding scrap steel generally follows the principle of adding all the scrap steel at once. This method loads all the scrap steel into the converter at once before the start of oxygen blowing smelting. Although the simplicity of this method is conducive to the rapid progress of the process, it has obvious shortcomings in terms of improving smelting efficiency, shortening smelting time, and accurately controlling key temperatures.
[0003] In specific operations, the large amount of scrap steel added at one time will cause the temperature of the molten iron to rise slowly in the early stage of smelting. This phenomenon directly affects the rate of decarburization reaction. Decarburization reaction is a very critical step in the converter smelting process, and its rate directly affects the efficiency of the entire smelting process. The slow temperature rise leads to a slow decarburization reaction, which indirectly prolongs the smelting time and reduces production efficiency. The large amount of scrap steel added at one time may also affect the melting of slag material. The melting of slag material is crucial to the converter smelting process. It not only helps to adjust the composition and properties of the slag, but also effectively protects the furnace lining and prolongs the service life of the converter. Under the traditional one-time addition method, since the addition of scrap steel will slow down the rate of molten iron temperature, the melting of slag material will also be affected, which in turn affects the protection effect of the furnace lining, and it is difficult to achieve the ideal converter terminal temperature; and the amount of scrap steel added to the existing converter has been determined by the scrap steel ratio before the start of smelting, and cannot be adjusted according to the actual smelting conditions of the converter. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a method for charging scrap steel into a converter in stages.
[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0006] A method for charging scrap steel in stages for a converter, wherein when charging the converter, only molten iron is added but no scrap steel is charged, and then oxygen blowing smelting is started; when the oxygen supply is 30-40 vol%, 5-10% of the mass of the molten iron scrap steel is added; when the oxygen supply is 50-60 vol%, 5-10% of the mass of the molten iron scrap steel is added; when the oxygen supply reaches 70 vol%, the required amount of scrap steel is added according to the calculation result of the heat balance of the converter.
[0007] As a preferred embodiment of the method for charging scrap steel into a converter in stages according to the present invention, during the smelting process, nitrogen is blown bottom when the oxygen supply is 0-70 vol%, and argon is blown bottom when the oxygen supply is 70-100 vol%.
[0008] As a preferred embodiment of the method for charging scrap steel into a converter in stages according to the present invention, the bottom blowing gas supply intensity is 0.02-0.10Nm 3 / (min·t 钢 ); During the blowing process, the oxygen lance position is controlled at 2.4-2.6m, and the oxygen supply intensity is controlled at 3.2-3.8Nm 3 / (min·t 钢 ).
[0009] As a preferred embodiment of the method for charging scrap steel into a converter in stages according to the present invention, when the oxygen supply is 7-20 vol%, lime and dolomite are added into the converter to control the slag basicity at 3.0-3.5.
[0010] As a preferred embodiment of the method for charging scrap steel into a converter in stages according to the present invention, the addition amount of lime and dolomite is 30-60 kg / t respectively. 钢 、10-30kg / t 钢 .
[0011] As a preferred solution of the method for loading scrap steel into a converter in stages according to the present invention, the scrap steel is added in the form of a high-level silo of the converter.
[0012] The beneficial effects of the present invention are as follows:
[0013] The present invention proposes a method for charging scrap steel in stages for a converter, wherein only molten iron is added but scrap steel is not charged when charging the converter, and oxygen blowing smelting is started; when the oxygen supply is 30-70 vol%, scrap steel is added in stages for multiple times. By adding different amounts of scrap steel in stages, the present invention can improve smelting efficiency, shorten smelting time, and accurately control the smelting end temperature. DETAILED DESCRIPTION
[0014] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0015] The present invention proposes a method for loading scrap steel in stages for a converter. In the initial stage of smelting, scrap steel is not loaded first, the temperature of molten iron rises rapidly, the slag material melts rapidly, the furnace lining can be protected, and the decarburization reaction rate is also rapidly increased. When the oxygen supply is 30-40%, 5-10% of the scrap steel by weight of the molten iron is added. At this time, the temperature of the molten iron in the converter is greater than 1390°C, and the decarburization reaction is intense; at the same time, due to the high temperature, the melting rate of the scrap steel is increased. When the oxygen supply is 50-60%, 5-10% of the scrap steel by weight of the molten iron is added. At this time, the temperature of the molten steel in the converter is relatively high, the decarburization rate can be maintained at a relatively high rate, and the melting rate of the scrap steel is also relatively high. When the oxygen supply reaches 70%, scrap steel is added according to the heat balance calculation of the converter. At this time, the amount of scrap steel to be added can be calculated relatively accurately according to the heat balance calculation of the converter, thereby accurately controlling the steel tapping temperature of the converter. At this time, the temperature of the molten steel in the converter is further increased, which can ensure that the scrap steel melts rapidly.
[0016] A method for charging scrap steel in stages for a converter. When charging the converter, only molten iron is added but no scrap steel is charged, and then oxygen blowing smelting is started. When the oxygen supply is 30-70 vol%, the scrap steel is added in stages for multiple times.
[0017] Specifically, when the oxygen supply is 30-40 vol%, 5-10% of the mass of molten iron scrap steel is added; when the oxygen supply is 50-60 vol%, 5-10% of the mass of molten iron scrap steel is added; when the oxygen supply reaches 70 vol%, the required amount of scrap steel is added according to the results of the converter heat balance calculation.
[0018] Adding scrap steel in stages can achieve precise control of the smelting process, optimize the thermal effect and carbon-oxygen reaction process, shorten the smelting time, and more effectively control the smelting end temperature. In the early stage of smelting, only adding molten iron and starting oxygen blowing without adding scrap steel can help quickly reach the necessary high temperature environment in the furnace and create favorable conditions for the subsequent addition of scrap steel. Not adding scrap steel in the early stage of oxygen blowing can avoid the drop in furnace temperature due to the excessive cooling effect of scrap steel, which is particularly critical for the initial reaction of the charge. As the smelting process deepens, 5-10% of the molten iron mass of scrap steel is added when the oxygen supply reaches 30-40vol% and 50-60vol%, respectively. This strategy of adding scrap steel in stages allows the furnace temperature to be properly controlled at each stage while ensuring the continuity and stability of the smelting process. By adjusting the timing and amount of scrap steel addition, the heat and chemical composition changes in the furnace can be better managed to avoid temperature fluctuations caused by the cooling effect of scrap steel. When the oxygen supply reaches 70 vol%, the required amount of scrap steel is added again according to the calculation results of the heat balance. This operation ensures the precise control of the smelting end point, improves the smelting efficiency, shortens the smelting time, and can more effectively control the smelting end point temperature.
[0019] Preferably, during the smelting process, nitrogen is blown from the bottom when the oxygen supply is 0-70 vol%, and argon is blown from the bottom when the oxygen supply is 70-100 vol%, and the bottom blowing gas supply intensity is 0.02-0.10 Nm 3 / (min·t 钢 ); During the blowing process, the oxygen lance position is controlled at 2.4-2.6m, and the oxygen supply intensity is controlled at 3.2-3.8Nm 3 / (min·t 钢 ), when the oxygen supply is 7-20vol%, lime and dolomite are added to the converter to control the slag basicity at 3.0-3.5, and the amount of lime and dolomite added is 30-60kg / t respectively 钢 、10-30kg / t 钢 Scrap steel is added in the form of a high-level silo in the converter. Other operations are carried out in accordance with the conventional operations of converter smelting, and steel tapping is carried out after blowing is completed.
[0020] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0021] Example 1
[0022] A method for charging scrap steel in stages for a 210t top and bottom combined blown converter, wherein only 180t of molten iron is added but no scrap steel is added during converter charging, and oxygen blowing smelting is started; when the oxygen supply is 30vol%, 10t of scrap steel is added; when the oxygen supply is 50vol%, 16t of scrap steel is added; when the oxygen supply reaches 70vol%, 7t of scrap steel is added according to the converter heat balance calculation result; during the smelting process, nitrogen is blown at the bottom when the oxygen supply is 0-70vol%, argon is blown at the bottom when the oxygen supply is 70-100vol%, and the bottom blowing gas supply intensity is 0.05Nm 3 / (min·t 钢 ); During the blowing process, the oxygen lance position is controlled at 2.4m, and the oxygen supply intensity is controlled at 3.3Nm 3 / (min·t 钢 ), when the oxygen supply is 8 vol%, 8 tons of lime and 4 tons of dolomite are added to the converter to control the slag basicity at 3.2, and scrap steel is added in the form of a high-level silo in the converter. Other operations are carried out in accordance with the conventional operation of converter smelting, and after the blowing is completed, the steel tapping operation is carried out. The smelting time required for this embodiment is 14.8 minutes, and the terminal temperature is 1659°C (target temperature: 1660°C).
[0023] Example 2
[0024] A method for charging scrap steel in stages for a 250t top and bottom combined blown converter, wherein only 212t of molten iron is added but no scrap steel is added during charging of the converter, and oxygen blowing smelting is started; when the oxygen supply is 38vol%, 11t of scrap steel is added; when the oxygen supply is 60vol%, 18t of scrap steel is added; when the oxygen supply reaches 70vol%, 8t of scrap steel is added according to the result of converter heat balance calculation; during the smelting process, nitrogen is blown at the bottom when the oxygen supply is 0-70vol%, argon is blown at the bottom when the oxygen supply is 70-100vol%, and the bottom blowing gas supply intensity is 0.10Nm 3 / (min·t 钢 ); During the blowing process, the oxygen lance position is controlled at 2.5m, and the oxygen supply intensity is controlled at 3.7Nm 3 / (min·t 钢 ), when the oxygen supply is 20 vol%, 9.5 t lime and 4.5 t dolomite are added to the converter to control the slag basicity at 3.5, and scrap steel is added in the form of a high-level silo in the converter. Other operations are carried out in accordance with the conventional operation of converter smelting, and after the blowing is completed, the steel tapping operation is carried out. The time required for converter smelting in this embodiment is 15.6 min, and the terminal temperature is 1670°C (target temperature: 1670°C).
[0025] Comparative Example 1
[0026] The difference from Example 1 is that 180 tons of molten iron is added to the converter during charging and all 33 tons of scrap steel are charged at one time before oxygen blowing smelting is started.
[0027] The time required for converter smelting in this comparative example is 16.2 minutes, and the final temperature is 1645°C (target temperature: 1660°C).
[0028] Comparative Example 2
[0029] The difference from Example 1 is that when the oxygen supply is 30 vol%, 21 tons of scrap steel are added; when the oxygen supply is 50 vol%, 7 tons of scrap steel are added; when the oxygen supply reaches 70 vol%, 5 tons of scrap steel are added according to the calculation results of the converter heat balance.
[0030] The time required for converter smelting in this comparative example is 15.5 minutes, and the final temperature is 1650°C (target temperature: 1660°C).
[0031] Comparative Example 3
[0032] The difference from Example 1 is that when the oxygen supply is 10 vol%, 10 t of scrap steel is added; when the oxygen supply is 45 vol%, 16 t of scrap steel is added; when the oxygen supply reaches 70 vol%, 7 t of scrap steel is added according to the calculation results of the converter heat balance.
[0033] The time required for converter smelting in this comparative example is 15.8 minutes, and the final temperature is 1652°C (target temperature: 1660°C).
[0034] Comparative Example 4
[0035] The difference from Example 1 is that 180 tons of molten iron is added to the converter during charging and all 33 tons of scrap steel is charged at once before oxygen blowing smelting is started. When the oxygen supply reaches 50 vol%, 200 kg of carburizer is added for temperature adjustment.
[0036] The time required for converter smelting in this comparative example is 16.6 minutes, and the final temperature is 1671°C (target temperature: 1660°C).
[0037] It can be seen from the above embodiments and comparative examples that the present invention only adds molten iron but does not add scrap steel when charging the converter and then starts oxygen blowing smelting; when the oxygen supply is 30-70 vol%, scrap steel is added in stages for multiple times. The present invention can improve smelting efficiency, shorten smelting time, and accurately control smelting end point temperature by adding different amounts of scrap steel in stages; if the timing or amount of addition is not within the range described in the present invention, the control accuracy of smelting time and smelting end point temperature will be affected.
[0038] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for charging scrap steel into a converter in stages, characterized in that: When charging the converter, only molten iron is added but no scrap steel is added, and then oxygen blowing smelting is started; when the oxygen supply is 30-40 vol%, 5-10% of the scrap steel by mass of the molten iron is added; when the oxygen supply is 50-60 vol%, 5-10% of the scrap steel by mass of the molten iron is added; when the oxygen supply reaches 70 vol%, the required amount of scrap steel is added according to the calculation results of the heat balance of the converter.
2. The method for charging scrap steel into a converter in stages according to claim 1, characterized in that: During the smelting process, nitrogen is blown bottom when the oxygen supply is 0-70 vol%, and argon is blown bottom when the oxygen supply is 70-100 vol%.
3. The method for charging scrap steel into a converter in stages according to claim 1, characterized in that: Bottom blowing air supply intensity is 0.02-0.10Nm 3 / (min·t 钢 ); During the blowing process, the oxygen lance position is controlled at 2.4-2.6m, and the oxygen supply intensity is controlled at 3.2-3.8Nm 3 / (min·t 钢 ).
4. The method for charging scrap steel into a converter in stages according to claim 1, characterized in that: When the oxygen supply is 7-20 vol%, lime and dolomite are added to the converter to control the slag basicity at 3.0-3.
5.
5. The method for charging scrap steel into a converter in stages according to claim 4, characterized in that: The addition amount of lime and dolomite is 30-60kg / t respectively 钢 、10-30kg / t 钢 .
6. The method for charging converter scrap in stages according to claim 1, characterized in that: Scrap steel is added into the converter in the form of a high-level silo.
Citation Information
Cited By
Blowing method for replacing Ar with CO2 for stainless steel smelting in AOD (Argon Oxygen Decarburization) furnace