Heat treatment process of large low alloy steel Q460D forge piece
By controlling the alloy composition and improving the water-cooling quenching and tempering process, the problem of mechanical property decline during heat treatment of large low-alloy steel Q460D forgings is solved, achieving high strength and high impact properties of the material, meeting customer needs, and simplifying process operations.
Patent Information
- Application Number
- CN202410698198.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-08
AI Technical Summary
The mechanical properties of large low-alloy steel Q460D forgings decrease due to the increase in wall thickness during heat treatment, making it difficult to meet customers' high performance requirements.
By controlling the alloy composition and improving the water-cooling quenching and tempering process, including post-forging heat treatment and performance heat treatment steps, the specific steps include heating, insulation, quenching and tempering, controlling water temperature and cooling time, optimizing the quenching effect, and improving the grain size and grain size of the material. Tissue strength.
The mechanical properties of the material, especially the impact value and strength, are significantly improved, meeting the high requirements of large-wall-thickness forgings, and the process is simple and easy to operate, reducing the risk of material cracking.
Smart Images

Figure CN118745498A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal materials, in particular to a heat treatment process for a large low alloy steel Q460D forging. Background Art
[0002] Q460D is a commonly used low-alloy high-strength steel and is often used in large engineering structures, maritime vessels, port machinery, and energy technology industries.
[0003] As the size and weight of large forgings continue to increase, the effective thickness of heat treatment becomes thicker and thicker. The mechanical properties of the body are not only limited by the hardenability of the material, but also by the heat treatment of large forgings. Normally, as the wall thickness increases, the mechanical properties decrease from the surface downward, but the customer's performance requirements remain basically unchanged.
[0004] Therefore, it is expected to provide a heat treatment process for large low alloy steel Q460D forgings that can solve the above technical problems. Summary of the invention
[0005] The purpose of the present invention is to provide a heat treatment process for large low alloy steel Q460D forgings, which can improve mechanical properties and meet customer requirements by controlling alloy composition and improving water cooling quenching and tempering process.
[0006] In order to achieve the purpose of the above invention, a heat treatment process for large low alloy steel Q460D forgings is provided, comprising the following steps:
[0007] S1, heat treatment after forging;
[0008] S2. Performance heat treatment: After rough machining of the forgings after post-forging heat treatment, put them into a heat treatment furnace for performance heat treatment, wherein they are heated to 650±10℃ at 50-100℃ / h, kept warm for 3-4h, then heated to 900±10℃ at 50-150℃ / h, kept warm for 10-11h, taken out of the furnace, water-cooled in a quenching pool to below 100℃, taken out of the quenching pool, tempered in a heat treatment furnace, heated to 520-540℃ at 50-100℃ / h, kept warm for 18-19h, and then air-cooled to room temperature.
[0009] Specifically, in step S1, the composition of the large low alloy steel Q460D forging is as follows, in terms of mass percentage:
[0010] C 0.15%~0.18%, Si 0.25%~0.35%, Mn 0.8%~1.2%, Cr 0.5%~1.0%, Ni 0.25%~0.6%, Mo 0.25%~0.3%, Nb 0.025%~0.05%, Ti 0.01%~0.03%, V 0.08%~0.12%, B 0.002%~0.004%, Cu 0.03%~0.1%, P ≤ 0.020%, S ≤ 0.010%, Al 0.025%~0.035%, N 0.005%~0.015%, and the rest is Fe.
[0011] Specifically, in step S1, the specific steps of post-forging heat treatment are: first air-cool the large low-alloy steel Q460D forging to 350±50℃, then load it into a heat treatment furnace, and keep it at 300-350℃ for 8-10h; heat it to 650±10℃ at 50-150℃ / h, and keep it for 3-4h; then heat it to 920±10℃ at 50-100℃ / h, keep it for 10-12h, and air-cool it to 300±50℃ after it is taken out of the furnace; put it into a heat treatment furnace, heat it to 350±20℃, and keep it for 8-10h; heat it to 650±10℃ at 50-100℃ / h, and keep it for 22-24h; cool it to below 250℃ at 20-100℃ / h before taking it out of the furnace.
[0012] Specifically, in step S2, the transfer time of the large low alloy steel Q460D forging from the furnace to the quenching pool is controlled within 2 minutes.
[0013] Specifically, the water temperature in the quenching tank is 18-25°C.
[0014] Furthermore, the water temperature in the quenching tank is 20°C.
[0015] Preferably, the large low alloy steel Q460D forging is placed in the quenching pool and, after being immersed in cooling water, the forging must move in the water along the axial direction for 8 to 10 minutes.
[0016] Preferably, the temperature of the large low alloy steel Q460D forging is measured after it has been cooled in the quenching pool for 30 minutes and the temperature of the forging has stabilized after it has been removed from the water.
[0017] Specifically, the outlet water temperature is controlled below 100°C. If the workpiece temperature exceeds 100°C, water is added to continue cooling. If the workpiece temperature is below 100°C, quenching is terminated.
[0018] The heat treatment process of the large low alloy steel Q460D forging of the present invention has the following advantages compared with the prior art:
[0019] (1) Performance heat treatment quenching heating rate is increased, so that the material grain size is refined and the performance is optimized; the quenching stirring is increased and the workpiece is moved during quenching, so that the cooling of the material in the initial stage of quenching is accelerated, the quenching effect is increased, and the structure is tougher after tempering, which greatly improves the performance; the water temperature is controlled at 18-25℃, at which the water cooling effect is better, and there is no risk of cracking for the material;
[0020] (2) By properly adjusting the alloy composition and adding some effective measures in the heat treatment and quenching process, the mechanical properties of large-walled forgings at all positions can meet high requirements; the obtained complete bainite + a small amount of ferrite structure has higher strength and impact value than the mixed combination (bainite + pearlite + ferrite) obtained by the previous process, especially the impact value, and the grain size does not change much;
[0021] (3) The process is simple and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a metallographic structure photograph of the forging prepared in Example 1 when magnified 100 times;
[0023] Figure 2 is a metallographic structure photograph of the forging prepared in Example 2 when magnified 100 times;
[0024] Figure 3 is a metallographic structure photograph of the forging prepared in Example 3 when magnified 100 times;
[0025] Figure 4 is a metallographic structure photograph of the forging prepared in Example 1 at a magnification of 500 times;
[0026] Figure 5 is a metallographic structure photograph of the forging prepared in Example 2 when magnified 500 times;
[0027] Figure 6 is a metallographic structure photograph of the forging prepared in Example 3 when magnified 500 times;
[0028] Figure 7 is a metallographic grain size photograph of the forging prepared in Example 1 when magnified 100 times;
[0029] Figure 8 is a metallographic grain size photograph of the forging prepared in Example 2 when magnified 100 times;
[0030] Fig. 9 This is a metallographic grain size photograph of the forging prepared in Example 3 at a magnification of 100 times. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0032] Example 1
[0033] The heat treatment process of the large low alloy steel Q460D forging of this embodiment includes the following steps:
[0034] S1, heat treatment after forging;
[0035] S2. Performance heat treatment: After rough processing, the forgings that have been heat treated after forging are placed in a heat treatment furnace for performance heat treatment, wherein they are heated to 650°C at 80°C / h, kept warm for 3h, then heated to 900°C at 100°C / h, kept warm for 10h, taken out of the furnace, water-cooled in a quenching pool, water-cooled to below 100°C, taken out of the quenching pool, tempered in a heat treatment furnace, heated to 520°C at 80°C / h, kept warm for 18h, and then taken out of the furnace and air-cooled to room temperature.
[0036] In this embodiment, in step S1, the composition of the large low alloy steel Q460D forging is as follows, in terms of mass percentage:
[0037] C0.16%, Si0.28%, Mn0.98%, Cr0.63%, Ni0.41%, Mo0.26%, Nb0.030%, Ti0.015%, V0.090%, B0.0025%, Cu0.06%, P0.017%, S0.0050%, Al0.031%, N0.0055%, and the rest is Fe.
[0038] In this embodiment, in step S1, the specific steps of post-forging heat treatment are: first air-cool the large low-alloy steel Q460D forging to 300°C, then load it into a heat treatment furnace and keep it at 320°C for 8 hours; heat it to 650°C at 100°C / h and keep it for 3 hours; then heat it to 920°C at 80°C / h and keep it for 11 hours, then air-cool it to 300°C after it is taken out of the furnace; put it into a heat treatment furnace and keep it at 340°C for 8 hours; heat it to 650°C at 80°C / h and keep it for 22 hours; cool it to below 250°C at 50°C / h and take it out of the furnace.
[0039] In this embodiment, in step S2, the transfer time of the large low alloy steel Q460D forging from the furnace to the quenching pool is controlled within 2 minutes.
[0040] In this embodiment, the water temperature in the quenching tank is 20°C.
[0041] In this embodiment, a large low alloy steel Q460D forging is placed in a quenching pool. After being immersed in cooling water, the forging must move in the water along the axial direction for 10 minutes.
[0042] In this embodiment, after the large low-alloy steel Q460D forging is cooled in the quenching pool for 30 minutes, the temperature of the forging is measured after the water temperature stabilizes, and the water outlet temperature is controlled below 100°C. If the workpiece temperature exceeds 100°C, it is further cooled in water. If the workpiece temperature is lower than 100°C, the quenching is completed.
[0043] Example 2
[0044] The following steps are included:
[0045] S1, heat treatment after forging;
[0046] S2. Performance heat treatment: After rough machining, the forgings that have been heat treated after forging are placed in a heat treatment furnace for performance heat treatment, wherein they are heated to 650°C at 70°C / h, kept at this temperature for 4h, then heated to 900°C at 90°C / h, kept at this temperature for 11h, taken out of the furnace, and water-cooled in a quenching pool to below 100°C, taken out of the quenching pool, and tempered in a heat treatment furnace, heated to 530°C at 80°C / h, kept at this temperature for 18.5h, and then air-cooled to room temperature.
[0047] In this embodiment, in step S1, the composition of the large low alloy steel Q460D forging is as follows, in terms of mass percentage:
[0048] C0.16%, Si0.28%, Mn0.98%, Cr0.63%, Ni0.41%, Mo0.26%, Nb0.030%, Ti0.015%, V0.090%, B0.0025%, Cu0.06%, P0.017%, S0.0050%, Al0.031%, N0.0055%, and the rest is Fe.
[0049] In this embodiment, in step S1, the specific steps of post-forging heat treatment are: first air-cool the large low-alloy steel Q460D forging to 360°C, then load it into a heat treatment furnace, and keep it at 320°C for 9 hours; heat it to 655°C at 90°C / h, and keep it for 3.5 hours; then heat it to 925°C at 80°C / h, keep it for 11 hours, and air-cool it to 325°C after it is taken out of the furnace; put it into a heat treatment furnace, heat it to 355°C, and keep it for 9 hours; heat it to 655°C at 80°C / h, and keep it for 23 hours; cool it to below 250°C at 85°C / h and take it out of the furnace.
[0050] In this embodiment, in step S2, the transfer time of the large low alloy steel Q460D forging from the furnace to the quenching pool is controlled within 2 minutes.
[0051] In this embodiment, the water temperature in the quenching tank is 18°C.
[0052] In this embodiment, a large low alloy steel Q460D forging is placed in a quenching pool. After being immersed in cooling water, the forging must move in the water along the axial direction for 9 minutes.
[0053] In this embodiment, after the large low-alloy steel Q460D forging is cooled in the quenching pool for 30 minutes, the temperature of the forging is measured after the water temperature stabilizes, and the water outlet temperature is controlled below 100°C. If the workpiece temperature exceeds 100°C, it is further cooled in water. If the workpiece temperature is lower than 100°C, the quenching is completed.
[0054] Example 3
[0055] The following steps are included:
[0056] S1, heat treatment after forging;
[0057] S2. Performance heat treatment: After rough machining, the forgings that have been heat treated after forging are placed in a heat treatment furnace for performance heat treatment, wherein the forgings are heated to 650°C at 90°C / h, kept at this temperature for 3h, then heated to 890°C at 120°C / h, kept at this temperature for 11h, taken out of the furnace, and water-cooled in a quenching pool to below 100°C, taken out of the quenching pool, and tempered in a heat treatment furnace, heated to 540°C at 70°C / h, kept at this temperature for 19h, and then taken out of the furnace and air-cooled to room temperature.
[0058] In this embodiment, in step S1, the composition of the large low alloy steel Q460D forging is as follows, in terms of mass percentage:
[0059] C0.16%, Si0.28%, Mn0.98%, Cr0.63%, Ni0.41%, Mo0.26%, Nb0.030%, Ti0.015%, V0.090%, B0.0025%, Cu0.06%, P0.017%, S0.0050%, Al0.031%, N0.0055%, and the rest is Fe.
[0060] Specifically, in step S1, the specific steps of post-forging heat treatment are: first air-cool the large low-alloy steel Q460D forging to 300°C, then load it into a heat treatment furnace, and keep it at 300°C for 10 hours; heat it to 650°C at 120°C / h, and keep it for 4 hours; then heat it to 930°C at 90°C / h, keep it for 10 hours, and air-cool it to 350°C after it is taken out of the furnace; put it into a heat treatment furnace, heat it at 350°C, and keep it for 8 hours; heat it to 660°C at 60°C / h, and keep it for 22 hours; cool it to below 250°C at 40°C / h before taking it out of the furnace.
[0061] In this embodiment, in step S2, the transfer time of the large low alloy steel Q460D forging from the furnace to the quenching pool is controlled within 2 minutes.
[0062] In this embodiment, the water temperature in the quenching tank is 25°C.
[0063] In this embodiment, a large low alloy steel Q460D forging is placed in a quenching pool. After being immersed in cooling water, the forging must move in the water along the axial direction for 10 minutes.
[0064] In this embodiment, after the large low-alloy steel Q460D forging is cooled in the quenching pool for 30 minutes, the temperature of the forging is measured after the water temperature stabilizes, and the water outlet temperature is controlled below 100°C. If the workpiece temperature exceeds 100°C, it is further cooled in water. If the workpiece temperature is lower than 100°C, the quenching is completed.
[0065] The forgings in Examples 1 to 3 were sampled respectively, and the data are as follows:
[0066]
[0067] The tensile and impact properties all meet the required values and are stable. Metallographic analysis is performed on each batch of impact specimens, such as Figures 1 to 9 The grain size is tested according to GB / T 6394, and the austenite grain size can reach 7.5-8 level; the organization is evenly distributed tempered bainite + ferrite, with good comprehensive performance, especially low-temperature impact resistance, which can fully meet customer requirements.
[0068] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. Heat treatment process of large low alloy steel Q460D forgings, characterized in that: The following steps are included: S1, heat treatment after forging; S2. Performance heat treatment: After rough machining of the forgings after post-forging heat treatment, put them into a heat treatment furnace for performance heat treatment, wherein they are heated to 650±10℃ at 50-100℃ / h, kept warm for 3-4h, then heated to 900±10℃ at 50-150℃ / h, kept warm for 10-11h, taken out of the furnace, water-cooled in a quenching pool to below 100℃, taken out of the quenching pool, tempered in a heat treatment furnace, heated to 520-540℃ at 50-100℃ / h, kept warm for 18-19h, and then air-cooled to room temperature.
2. The heat treatment process of large low alloy steel Q460D forgings according to claim 1, characterized in that: In step S1, the composition of the large low alloy steel Q460D forging is as follows, in terms of mass percentage: C 0.15%~0.18%, Si 0.25%~0.35%, Mn 0.8%~1.2%, Cr 0.5%~1.0%, Ni 0.25%~0.6%, Mo 0.25%~0.3%, Nb 0.025%~0.05%, Ti 0.01%~0.03%, V 0.08%~0.12%, B 0.002%~0.004%, Cu 0.03%~0.1%, P ≤ 0.020%, S ≤ 0.010%, Al 0.025%~0.035%, N 0.005%~0.015%, and the rest is Fe.
3. The heat treatment process of large low alloy steel Q460D forgings according to claim 2, characterized in that: In step S1, the specific steps of post-forging heat treatment are: first air-cool the large low-alloy steel Q460D forging to 350±50℃, then load it into a heat treatment furnace, and keep it at 300-350℃ for 8-10h; heat it to 650±10℃ at 50-150℃ / h, and keep it for 3-4h; then heat it to 920±10℃ at 50-100℃ / h, keep it for 10-12h, take it out of the furnace and air-cool it to 300±50℃; put it into a heat treatment furnace, heat it to 350±20℃, and keep it for 8-10h; heat it to 650±10℃ at 50-100℃ / h, and keep it for 22-24h; cool it to below 250℃ at 20-100℃ / h and take it out of the furnace.
4. The heat treatment process for large low alloy steel Q460D forgings according to claim 2, characterized in that: In step S2, the transfer time of the large low alloy steel Q460D forging from the furnace to the quenching pool is controlled within 2 minutes.
5. The heat treatment process for large low alloy steel Q460D forgings according to claim 1 or 4, characterized in that: The water temperature in the quenching pool is 18-25°C.
6. The heat treatment process for large low alloy steel Q460D forgings according to claim 5, characterized in that: The water temperature in the quenching tank is 20°C.
7. The heat treatment process for a large low alloy steel Q460D forging according to any one of claims 4 to 6, characterized in that: Place the large low alloy steel Q460D forging in the quenching pool. After being immersed in cooling water, the forging must move in the water along the axial direction for 8 to 10 minutes.
8. The heat treatment process for large low alloy steel Q460D forgings according to claim 7, characterized in that: After the large low alloy steel Q460D forgings are cooled in the quenching pool for 30 minutes, the temperature of the forgings is measured after the water temperature stabilizes.
9. The heat treatment process for large low alloy steel Q460D forgings according to claim 8, characterized in that: Control the water outlet temperature below 100℃. If the workpiece temperature exceeds 100℃, add water to continue cooling. If the workpiece temperature is below 100℃, quenching is completed.
Citation Information
Cited By
33CrNiMo steel and heat treatment process thereof
CN122013051A
33CrNiMo steel and heat treatment process thereof
CN122038909A