Method for preparing high-quality sponge titanium raw material from ilmenite
By performing ball milling and batching, pre-oxidation, roasting reduction, grinding, magnetic separation and rust treatment on ilmenite, the problem of unremoved impurities in ilmenite is solved, the quality and production efficiency of titanium sponge raw materials are improved, and environmental pollution is reduced. .
Patent Information
- Application Number
- CN202410835922.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-08
AI Technical Summary
In the prior art, ilmenite is not subjected to titanium enrichment treatment and impurity purification, resulting in poor quality titanium tetrachloride, the raw material for titanium sponge, which increases preparation difficulty and energy consumption, causing environmental pollution.
Through ball milling and batching, pre-oxidation, roasting reduction, grinding and magnetic separation, rust and chlorination reactions, the ilmenite is titanium-enriched and impurities are removed to generate high-quality titanium sponge raw material titanium tetrachloride.
It improves the production efficiency and quality of titanium tetrachloride, the raw material of titanium sponge, reduces the difficulty of purification and energy consumption, and reduces environmental pollution.
Smart Images

Figure CN118745507A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nonferrous metallurgy, and in particular to a method for preparing high-quality titanium sponge by utilizing ilmenite. Background Art
[0002] Natural rutile and ilmenite are the main titanium resources in the world. The concentrate content of natural rutile can reach 95% to 96%, which is a high-quality raw material for the titanium industry, but the reserves are relatively small. With the gradual depletion of natural rutile resources, the rise in prices and the development of the titanium industry, abundant ilmenite has become the main production raw material for the titanium industry.
[0003] At present, the grade of ilmenite is low. In order to adapt to the development of the titanium industry, ilmenite must be enriched into high-grade titanium-rich materials. Ilmenite is mainly used as a raw material for the manufacture of titanium dioxide and sponge titanium. The proportion of ilmenite used in the manufacture of titanium dioxide exceeds 90%. The sulfuric acid process is simple and can directly use ilmenite as a raw material, but the quality of titanium dioxide in the product is low. A large-scale boiling chlorination process is required to generate an intermediate product of titanium tetrachloride, thereby improving the quality of titanium dioxide products prepared by ilmenite based on the sulfuric acid method.
[0004] In the prior art, Chinese patent CN112745699A discloses a method for preparing titanium sponge for spandex fiber matting, which specifically involves crushing titanium tetrachloride, introducing chlorine gas, and adding artificial rutile for chlorination to obtain crude titanium tetrachloride. However, this method does not purify the raw materials, which results in excessive calcium and iron impurities in the crude titanium tetrachloride, increasing the difficulty of preparing titanium sponge and also reducing the quality of titanium sponge.
[0005] Chinese patent CN115415291A discloses a method for treating chlorinated titanium dioxide chlorinated slag by the chloride process, specifically placing titanium chloride in a boiling chlorination furnace and chlorinating at a temperature of about 1000°C. General ilmenite or low-grade titanium-rich materials contain high-purity iron, calcium and magnesium impurities, and calcium chloride and magnesium chloride have high boiling points, while iron is highly oxidized. Under general chlorination conditions, calcium chloride and magnesium chloride are liquids, while iron is solid. If the concentration of molten calcium chloride and magnesium chloride is high enough, the viscosity of the fluidized bed will rise sharply, resulting in the bed not being fluidized, chloride settling, and iron element also settling, thereby increasing the difficulty of purifying titanium tetrachloride, causing more serious energy consumption and environmental pollution.
[0006] In the prior art CN112745699A and CN115415291A methods for preparing titanium tetrachloride as a raw material for sponge titanium, ilmenite is not treated to be titanium-enriched, and impurities therein are not removed for purification, so the quality of the prepared titanium tetrachloride as a raw material for sponge titanium is poor.
[0007] In view of this, it is of great significance to provide a method for preparing high-quality sponge titanium raw material using ilmenite. Summary of the invention
[0008] The present invention provides a method for preparing high-quality sponge titanium raw material by utilizing ilmenite, which solves the environmental pollution caused by the large amount of accumulation of low-grade ilmenite, carries out titanium-enriching treatment on the ilmenite and removes impurities therein, improves the production efficiency of titanium tetrachloride, a sponge titanium raw material, and the prepared sponge titanium raw material is of high quality.
[0009] A method for preparing high-quality sponge titanium raw material using ilmenite, comprising the following steps:
[0010] 1) Ball milling: ball milling ilmenite to obtain ilmenite powder, adding sodium hypochlorite, sodium humate, a binder and water to the ilmenite powder and mixing to obtain a mixture;
[0011] 2) Pre-oxidation: the mixture of the ball-milled ingredients in step 1) is subjected to ball-making, drying and pre-heating and pre-oxidation treatments in sequence to obtain pre-oxidized pellets;
[0012] 3) Calcination reduction: the pre-oxidized pellets pre-oxidized in step 2) are mixed with a reducing agent and a carbonaceous reducing agent, and calcined and reduced in a nitriding atmosphere and kept warm to obtain reduced ilmenite pellets;
[0013] 4) grinding and magnetic separation: grinding the reduced ilmenite pellets obtained by roasting and reduction in step 3), and then performing graded screening and graded magnetic separation to obtain metallic iron and nitrided tailings;
[0014] 5) Corrosion: adding a corrosion agent to the nitriding tailings screened and magnetically separated in step 4) to carry out corrosion reaction and leaching separation to obtain iron removal tailings and corrosion waste liquid;
[0015] 6) Chlorination reaction: After the corroded iron removal tailings from step 5) are mixed with petroleum coke, a chlorinating agent is introduced to carry out a chlorination reaction to obtain a high-quality sponge titanium raw material.
[0016] In a specific embodiment of the present invention, step 1) ball milling ingredients, the TiO2 content in the ilmenite powder is greater than 48.5wt%, and the TFe content is 31-37%; the particle size of the ilmenite powder is -0.084mm, accounting for greater than or equal to 90%; the amount of the adhesive added is 0.5-2wt% of the ilmenite powder.
[0017] In a specific embodiment of the present invention, the mass ratio of the sodium chlorate, sodium humate and adhesive is 20-30:25-35:30-60.
[0018] In a specific embodiment of the present invention, the adhesive is made of carboxymethyl cellulose, starch, polyvinyl alcohol, polyvinyl acetal and sodium alginate.
[0019] In a specific embodiment of the present invention, the mass ratio of the carboxymethyl cellulose, starch, polyvinyl alcohol, polyvinyl acetal and sodium alginate is 8-12:2-5:2-5:1-3:2-6.
[0020] In a specific embodiment of the present invention, step 2) pre-oxidation, the particle size of the pelletizing is 10-15 mm; the blast temperature of the drying and preheating is 600-750°C, the blast time is 3-4 min, and the blast wind speed is 0.5-1.5 m / s; the pre-oxidation temperature is 750-850°C, the time is 30-60 min, and the wind speed is 2.0-2.8 m / s.
[0021] In a specific embodiment of the present invention, the pelletizing is performed using a pelletizing machine.
[0022] In a specific embodiment of the present invention, the drying and preheating is performed using a chain grate.
[0023] In a specific embodiment of the present invention, an oxidizing gas is introduced during the pre-oxidation process.
[0024] In a specific embodiment of the present invention, the oxidizing gas is air and / or oxygen.
[0025] In a specific embodiment of the present invention, in step 3) roasting reduction, the amount of the reducing agent added is 12-18wt% of the pre-oxidized pellets, and the mass ratio of the reducing agent to the carbonaceous reducing agent is 12-16:3-5.
[0026] In a specific embodiment of the present invention, the reducing agent is at least one of ethoxymagnesium, sodium carbonate, sodium borate, and alkoxysilane.
[0027] In a specific embodiment of the present invention, the carbonaceous reducing agent is lignite and / or anthracite.
[0028] In a specific embodiment of the present invention, step 3) calcination reduction, the calcination reduction temperature is 900-1100°C, and the time is 0.5-8h; the nitriding atmosphere is any one or any combination of NH3-N2, NH3-H2, and NH3-N2-H2; the insulation temperature is 220-280°C, and the time is 5-8h.
[0029] In a specific embodiment of the present invention, step 4) grinding and magnetic separation, the grinding adopts a disc ball mill; the mesh size of the graded screening is 220-280 mesh; the magnetic field strength of the graded magnetic separation is 1500-2500 Gs.
[0030] In a specific embodiment of the present invention, in step 5) corrosion, the corrosion agent consists of NH4Cl and HCl.
[0031] In a specific embodiment of the present invention, the mass ratio of NH4Cl and HCl to nitriding tailings in the corrosion agent is 0.5-1.5:1.5-2.5:100.
[0032] In a specific embodiment of the present invention, in step 5) corrosion, the temperature of the corrosion reaction is 65-85°C, the concentration of the corrosion agent is 0.5-3wt%, the solid-liquid ratio is 4-8, the stirring rate is 150-300r / min, and the air flow rate is 1-2.6L·min -1 ·m -3 , time is 3 to 4 hours; the temperature of the leaching separation is 250 to 320°C, and the time is 2 hours.
[0033] In a specific embodiment of the present invention, in step 6) chlorination reaction, the amount of petroleum coke added is 12-17wt% of the iron removal tailings; the temperature of the chlorination reaction is 800-1050°C, the reaction time is 8-10.5h, and the amount of chlorinating agent introduced is 0.2L / min.
[0034] In a specific embodiment of the present invention, the chlorinating agent is chlorine gas.
[0035] The beneficial effects of adopting the above further scheme are:
[0036] 1. The present invention generates an intermediate product, titanium carbonitride, to replace the titanium-rich material in the chlorination reaction, which can effectively reduce the temperature of the chlorination reaction and avoid the chlorination of metal elements such as calcium and magnesium, thereby achieving the selective chlorination of the titanium element. The chlorination rate of the chlorination reaction is high, and the difficulty of purifying titanium tetrachloride is reduced. The titanium tetrachloride product prepared by the chlorination reaction can be used as a raw material for preparing high-quality sponge titanium;
[0037] 2. The present invention can remove most of the metallic iron impurities based on the combination of magnetic separation and corrosion, improve the purity of titanium carbonitride, and at the same time improve the chlorination rate of the chlorination reaction, reduce the difficulty of purifying titanium tetrachloride, and provide high-quality raw materials for the production of high-quality sponge titanium;
[0038] 3. The present invention can prepare the intermediate product titanium carbonitride by roasting and reducing with a gas containing nitrogen and hydrogen elements. The temperature of reduction and nitridation is low, which saves energy consumption, and the purity of the intermediate product titanium carbonitride is high;
[0039] 4. The present invention promotes the growth of iron crystal nuclei in the reduced pellets by heat preservation after reduction roasting, which is beneficial to improving the reduction rate of iron compounds.
[0040] 5. The present invention performs pre-oxidation treatment on the mixed material, which can remove impurities such as phosphorus and sulfur in the ilmenite, and is beneficial to the subsequent reduction roasting step. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is a flowchart of the method for preparing high-quality sponge titanium raw material using ilmenite in the present invention;
[0042] Figure 2 The present invention is a flow chart showing the principle of the method for preparing high-quality sponge titanium raw material using ilmenite. DETAILED DESCRIPTION
[0043] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0044] Based on the attached Figure 1 and 2 A method for preparing high-quality sponge titanium raw material using ilmenite comprises the following steps:
[0045] 1) Ball milling: ball milling ilmenite to obtain ilmenite powder, adding sodium hypochlorite, sodium humate, a binder and water to the ilmenite powder and mixing to obtain a mixture;
[0046] 2) Pre-oxidation: the mixture of the ball-milled ingredients in step 1) is subjected to ball-making, drying and pre-heating and pre-oxidation treatments in sequence to obtain pre-oxidized pellets;
[0047] 3) Calcination reduction: the pre-oxidized pellets pre-oxidized in step 2) are mixed with a reducing agent and a carbonaceous reducing agent, and calcined and reduced in a nitriding atmosphere and kept warm to obtain reduced ilmenite pellets;
[0048] 4) grinding and magnetic separation: grinding the reduced ilmenite pellets obtained by roasting and reduction in step 3), and then performing graded screening and graded magnetic separation to obtain metallic iron and nitrided tailings;
[0049] 5) Corrosion: adding a corrosion agent to the nitriding tailings screened and magnetically separated in step 4) to carry out corrosion reaction and leaching separation to obtain iron removal tailings and corrosion waste liquid;
[0050] 6) Chlorination reaction: After the corroded iron removal tailings from step 5) are mixed with petroleum coke, a chlorinating agent is introduced to carry out a chlorination reaction to obtain a high-quality sponge titanium raw material.
[0051] In some examples, step 1) ball milling ingredients, the TiO2 content in the ilmenite powder is greater than 48.5wt%, and the TFe content is 31-37%; the particle size of the ilmenite powder is -0.084mm, accounting for greater than or equal to 90wt%; the amount of the adhesive added is 0.5-2wt% of the ilmenite powder.
[0052] In some examples, the mass ratio of sodium chlorate, sodium humate and binder is 20-30:25-35:30-60.
[0053] In some examples, the adhesive is made of carboxymethyl cellulose, starch, polyvinyl alcohol, polyvinyl acetal, and sodium alginate.
[0054] In some examples, the mass ratio of carboxymethyl cellulose, starch, polyvinyl alcohol, polyvinyl acetal and sodium alginate is 8-12:2-5:2-5:1-3:2-6.
[0055] In some examples, in step 2) pre-oxidation, the particle size of the pelletizing is 10-15 mm; the blast temperature of the drying and preheating is 600-750°C, the blast time is 3-4 min, and the blast wind speed is 0.5-1.5 m / s; the pre-oxidation temperature is 750-850°C, the time is 30-60 min, and the wind speed is 2.0-2.8 m / s.
[0056] In some instances, pelletizing uses a pelletizing machine;
[0057] In some instances, dry preheating uses a chain grate;
[0058] In some embodiments, an oxidizing gas is introduced during the pre-oxidation process;
[0059] In some examples, the oxidizing gas is air and / or oxygen.
[0060] In some examples, in step 3) roasting reduction, the amount of reducing agent added is 12-18wt% of the pre-oxidized pellets, and the mass ratio of reducing agent to carbonaceous reducing agent is 12-16:3-5.
[0061] In some examples, the reducing agent is at least one of ethoxymagnesium, sodium carbonate, sodium borate, and alkoxysilane;
[0062] In some examples, the carbonaceous reductant is lignite and / or anthracite.
[0063] In some examples, step 3) is calcined and reduced, the temperature of the calcination and reduction is 900-1100°C, and the time is 0.5-8h; the nitriding atmosphere is any one or any combination of NH3-N2, NH3-H2, and NH3-N2-H2; the insulation temperature is 220-280°C, and the time is 5-8h.
[0064] In some examples, step 4) grinding and magnetic separation is performed using a disc ball mill; the mesh size of the graded screening is 220-280 meshes; and the magnetic field strength of the graded magnetic separation is 1500-2500 Gs.
[0065] In some embodiments, step 5) is corrosion, and the corrosion agent consists of NH4Cl and HCl.
[0066] In some examples, the mass ratio of NH4Cl and HCl to nitriding tailings in the rusting agent is 0.5-1.5:1.5-2.5:100.
[0067] In some examples, in step 5) corrosion, the temperature of the corrosion reaction is 65-85°C, the concentration of the corrosion agent is 0.5-3wt%, the solid-liquid ratio is 4-8, the stirring rate is 150-300r / min, and the air flow rate is 1-2.6L·min -1 ·m -3 , time is 3 to 4 hours; the temperature of the leaching separation is 250 to 320°C.
[0068] In some examples, in step 6) chlorination reaction, the amount of petroleum coke added is 12-17wt% of the iron removal tailings; the temperature of the chlorination reaction is 800-1050°C, the reaction time is 8-10.5h, and the amount of chlorinating agent introduced is 0.2L / min.
[0069] In some examples, the chlorinating agent is chlorine gas.
[0070] The method for preparing high-quality sponge titanium raw material by using ilmenite of the present invention has the advantages of simple process, high removal rate of impure iron, high grade of sponge titanium raw material, green and environmental protection, etc.
[0071] In the present invention, ilmenite is crushed and ground, and then mixed with sodium hypochlorite, sodium humate and a binder to obtain a mixed material; the mixed material is successively subjected to balling, drying and preheating and preoxidation treatment, and then mixed with a carbonaceous reducing agent and a reducing agent for nitriding reduction to obtain reduced ilmenite pellets; the reduced ilmenite pellets are subjected to grinding and crushing, graded screening and graded magnetic separation to obtain metallic iron and nitrided tailings respectively; oxygen is passed through the nitrided tailings, and a rusting agent is added to perform rust treatment and separation to obtain iron oxide and nitrided ilmenite respectively; the nitrided ilmenite is subjected to boiling chlorination treatment to finally obtain high-quality sponge titanium raw material.
[0072] The following examples further illustrate the use of ilmenite to prepare high-quality titanium sponge raw materials in the present invention:
[0073] Example 1
[0074] This embodiment provides a method for preparing high-quality sponge titanium raw material using ilmenite, comprising the following steps:
[0075] 1. Grind 120g of Panxi ilmenite containing 49wt% TiO2 and 31wt% TFe with a ball mill until the particle size of the ilmenite powder is -0.084mm accounting for 91wt%, and add 2.1g of sodium chlorate, 2.5g of sodium humate, 3.2g of carboxymethyl cellulose, 0.8g of starch, 0.8g of polyvinyl alcohol, 0.4g of polyvinyl acetal and 0.8g of sodium alginate to the ilmenite powder;
[0076] 2. The mixed material is pelletized by a ball forming machine to obtain ilmenite pellets, and the ilmenite pellets are dried, preheated and preoxidized in a chain grate to obtain preoxidized pellets; wherein the air temperature in the preheating section of the drying and preheating is 600°C, the drying and preheating time is 3 minutes, and the wind speed is 0.5 m / s; the temperature of the preoxidation treatment is 750°C, the time is 30 minutes, and the wind speed is 2.0 m / s;
[0077] A total of 119.3 g of pre-oxidized pellets were obtained, with a particle size of 10 mm, a drop strength of 9 times / 0.5 m, a burst temperature of 155 ° C, and a compressive strength of 1700 N.
[0078] 3. 119.3 g of pre-oxidized pellets, 13 g of anthracite, 1.2 g of anhydrous sodium carbonate and 1.1 g of sodium borate were mixed evenly, placed in a rotary kiln under a nitriding atmosphere of NH3-N2 and NH3-H2-N2, calcined and reduced at 900°C for 1.5 h, and then heat-treated at 220°C for 5 h to obtain reduced ilmenite pellets;
[0079] The drop strength of the reduced ilmenite pellets is 5 times / 0.5m, the burst temperature is 180℃, and the iron core growth rate is 95%;
[0080] 4. The reduced ilmenite pellets are crushed and ground with a disc ball mill, and then graded and screened with a 220-mesh screen, and then graded magnetic separation is performed to obtain metallic iron and nitrided tailings; wherein the magnetic field intensity of the graded magnetic separation is 1500 Gs;
[0081] 5. Add the corrosion liquid (solid-liquid ratio of 4) to the nitriding tailings, perform corrosion treatment at 65°C for 3 hours, filter and dry to obtain the iron removal tailings and corrosion waste liquid; wherein the corrosion liquid is a mixture of 0.5wt% NH4Cl and 1.5wt% HCl;
[0082] 6. Take 90g of iron removal tailings and 10.2g of petroleum coke, mix them, place them in a boiling chlorination furnace, and carry out chlorination reaction at 800°C and a chlorine gas introduction rate of 0.2L / min for 8h to obtain high-quality sponge titanium raw material.
[0083] In this embodiment, the iron recovery rate of the whole process is 88.45%, and the purity of titanium tetrachloride in the high-quality sponge titanium raw material is 90.2%.
[0084] Example 2
[0085] This embodiment provides a method for preparing high-quality sponge titanium raw material using ilmenite, comprising the following steps:
[0086] 1. Grind 120g of Panxi ilmenite containing 49.5wt% TiO2 and 32wt% TFe with a ball mill until the particle size of the ilmenite powder is -0.084mm accounting for 90wt%, and add 2.2g of sodium chlorate, 2.7g of sodium humate, 3.1g of carboxymethyl cellulose, 0.8g of starch, 0.9g of polyvinyl alcohol, 0.9g of polyvinyl acetal and 0.8g of sodium alginate to the ilmenite powder;
[0087] 2. The mixed material is pelletized by a ball forming machine to obtain ilmenite pellets, and the ilmenite pellets are dried, preheated and preoxidized in a chain grate to obtain preoxidized pellets; wherein the air temperature of the preheating section of the drying preheating is 620°C, the drying preheating time is 3.5 minutes, and the wind speed is 0.5 m / s; the preoxidation temperature is 760°C, the time is 33 minutes, and the wind speed is 2.0 m / s;
[0088] The obtained pre-oxidized pellets weigh 120.4 g, have a particle size of 10 mm, a drop strength of 8 times / 0.5 m, a burst temperature of 140° C., and a compressive strength of 1700N.
[0089] 3. Take 120.4g of pre-oxidized pellets, 13.8g of anthracite, 1.3g of anhydrous sodium carbonate and 1.2g of sodium borate and mix them evenly, put them into a rotary kiln under a nitriding atmosphere of NH3-N2 and NH3-H2-N2, roast and reduce them at 950°C for 1.5h, and then keep them at 250°C for 5h to obtain reduced ilmenite pellets;
[0090] The drop strength of the reduced ilmenite pellets is >5 times / 0.5m, the burst temperature is >180℃, and the iron core growth rate is 90%;
[0091] 4. The reduced ilmenite pellets are crushed and ground with a disc ball mill, and then graded and screened with a 230-mesh screen, and then graded magnetic separation is performed to obtain metallic iron and nitrided tailings; wherein the magnetic field intensity of the graded magnetic separation is 2050 Gs;
[0092] 5. Add the corrosion liquid (solid-liquid ratio of 5) to the nitriding tailings, perform corrosion treatment at 68°C for 3.5 hours, filter and dry to obtain the iron removal tailings and corrosion waste liquid; wherein the corrosion liquid is a mixture of 0.7wt% NH4Cl and 1.7wt% HCl;
[0093] 6. Take 90g of iron removal tailings and 12.2g of petroleum coke, mix them, place them in a boiling chlorination furnace, and carry out chlorination reaction at 850°C and a chlorine gas introduction rate of 0.2L / min for 8h to obtain high-quality sponge titanium raw material.
[0094] In this embodiment, the iron recovery rate of the whole process is 90.02%, and the purity of titanium tetrachloride in the high-quality sponge titanium raw material is 92.12%.
[0095] Example 3
[0096] This embodiment provides a method for preparing high-quality sponge titanium raw material using ilmenite, comprising the following steps:
[0097] 1. Grind 120g of Panxi ilmenite containing 51.5wt% TiO2 and 31wt% TFe with a ball mill until the particle size of the ilmenite powder is -0.084mm accounting for 90wt%, add 2.1g of sodium chlorate, 2.7g of sodium humate, and 6.5g of adhesive to the ilmenite powder to obtain a mixture; wherein the adhesive is made of 3.3g of carboxymethyl cellulose, 0.7g of starch, 0.9g of polyvinyl alcohol, 0.9g of polyvinyl acetal and 0.7g of sodium alginate;
[0098] 2. The mixed material is pelletized by a ball forming machine to obtain ilmenite pellets, and the ilmenite pellets are dried, preheated and preoxidized in a chain grate to obtain preoxidized pellets; wherein the air temperature in the preheating section of the drying and preheating is 640°C, the drying and preheating time is 3 minutes, and the wind speed is 0.5 m / s; the preoxidation temperature is 780°C, the time is 30 minutes, and the wind speed is 2.0 m / s;
[0099] A total of 120.8 g of pre-oxidized pellets were obtained, the particle size of the pre-oxidized pellets was 10 mm, the drop strength was 8 times / 0.5 m, the burst temperature was 1450° C., and the compressive strength was 1600N.
[0100] 3. Take 120.8g of pre-oxidized pellets, mix them evenly with 13.9g of anthracite, 1.4g of anhydrous sodium carbonate and 1.3g of sodium borate, put them into a rotary kiln under a nitriding atmosphere of NH3-N2 and NH3-H2-N2, roast and reduce them at 950°C for 5h, and then keep them at 250°C for 6h to obtain reduced ilmenite pellets;
[0101] The drop strength of the reduced ilmenite pellets is >5 times / 0.5m, the burst temperature is >180℃, and the iron core growth rate is 80%;
[0102] 4. The reduced ilmenite pellets are crushed and ground with a disc ball mill, and then graded and screened with a 230-mesh screen, and then graded magnetic separation is performed to obtain metallic iron and nitrided tailings; wherein the magnetic field intensity of the graded magnetic separation is 2500 Gs;
[0103] 5. Add the corrosion liquid (solid-liquid ratio of 4) to the nitriding tailings, perform corrosion treatment at 68°C for 4 hours, filter and dry to obtain the iron removal tailings and corrosion waste liquid; wherein the corrosion liquid is a mixture of 0.5wt% NH4Cl and 1.5wt% HCl;
[0104] 6. Take 90g of iron removal tailings and 13.2g of petroleum coke, mix them, place them in a boiling chlorination furnace, and carry out chlorination reaction at 950°C and a chlorine gas introduction rate of 0.2L / min for 8.5h to obtain high-quality sponge titanium raw material.
[0105] In this embodiment, the iron recovery rate of the whole process is 92.47%, and the purity of titanium tetrachloride in the high-quality sponge titanium raw material is 93.9%.
Claims
1. A method for preparing high-quality sponge titanium raw material using ilmenite, characterized in that: The following steps are involved: 1) Ball milling: ball milling ilmenite to obtain ilmenite powder, adding sodium hypochlorite, sodium humate, a binder and water to the ilmenite powder and mixing to obtain a mixture; 2) Pre-oxidation: the mixture of the ball-milled ingredients in step 1) is subjected to ball-making, drying and pre-heating and pre-oxidation treatments in sequence to obtain pre-oxidized pellets; 3) Calcination reduction: the pre-oxidized pellets pre-oxidized in step 2) are mixed with a reducing agent and a carbonaceous reducing agent, and calcined and reduced in a nitriding atmosphere and kept warm to obtain reduced ilmenite pellets; 4) grinding and magnetic separation: grinding the reduced ilmenite pellets obtained by roasting and reduction in step 3), and then performing graded screening and graded magnetic separation to obtain metallic iron and nitrided tailings; 5) Corrosion: adding a corrosion agent to the nitriding tailings screened and magnetically separated in step 4) to carry out corrosion reaction and leaching separation to obtain iron removal tailings and corrosion waste liquid; 6) Chlorination reaction: After the corroded iron removal tailings from step 5) are mixed with petroleum coke, a chlorinating agent is introduced to carry out a chlorination reaction to obtain a high-quality sponge titanium raw material.
2. The method for preparing high-quality sponge titanium raw material using ilmenite according to claim 1, characterized in that: Step 1) ball milling ingredients, the TiO2 content in the ilmenite powder is greater than 48.5wt%, and the TFe content is 31-37%; the particle size of the ilmenite powder is greater than or equal to -0.084mm; the amount of the adhesive added is 0.5-2wt% of the ilmenite powder.
3. The method for preparing high-quality sponge titanium raw material using ilmenite according to claim 1 or 2, characterized in that: The mass ratio of the sodium chlorate, sodium humate and adhesive is 20-30:25-35:30-60; Preferably, the adhesive is made of carboxymethyl cellulose, starch, polyvinyl alcohol, polyvinyl acetal and sodium alginate; More preferably, the mass ratio of the carboxymethyl cellulose, starch, polyvinyl alcohol, polyvinyl acetal and sodium alginate is 8-12:2-5:2-5:1-3:2-6.
4. The method for preparing high-quality sponge titanium raw material using ilmenite according to claim 1, characterized in that: Step 2) pre-oxidation, the particle size of the pelletizing is 10-15 mm; the blast temperature of the drying and preheating is 600-750° C., the blast time is 3-4 min, and the blast wind speed is 0.5-1.5 m / s; the pre-oxidation temperature is 750-850° C., the time is 30-60 min, and the wind speed is 2.0-2.8 m / s; Preferably, the pelletizing is carried out using a spherical machine; Preferably, the drying and preheating is performed using a chain grate; Preferably, an oxidizing gas is introduced during the pre-oxidation process; More preferably, the oxidizing gas is air and / or oxygen.
5. The method for preparing high-quality sponge titanium raw material using ilmenite according to claim 1, characterized in that: Step 3) calcination reduction, the amount of the reducing agent added is 12-18wt% of the pre-oxidized pellets, and the mass ratio of the reducing agent to the carbonaceous reducing agent is 12-16:3-5; Preferably, the reducing agent is at least one of ethoxymagnesium, sodium carbonate, sodium borate, and alkoxysilane; Preferably, the carbonaceous reducing agent is lignite and / or anthracite.
6. The method for preparing high-quality sponge titanium raw material using ilmenite according to claim 1, characterized in that: Step 3) calcination reduction, the calcination reduction temperature is 900-1100°C, and the time is 0.5-8h; the nitriding atmosphere is any one or any combination of NH3-N2, NH3-H2, and NH3-N2-H2; the insulation temperature is 220-280°C, and the time is 5-8h.
7. The method for preparing high-quality sponge titanium raw material using ilmenite according to claim 1, characterized in that: Step 4) grinding and magnetic separation, the grinding adopts a disc ball mill; the mesh size of the graded screening is 220-280 mesh; the magnetic field strength of the graded magnetic separation is 1500-2500 Gs.
8. The method for preparing high-quality sponge titanium raw material using ilmenite according to claim 1, characterized in that: Step 5) rusting, wherein the rusting agent consists of NH4Cl and HCl; Preferably, the mass ratio of NH4Cl and HCl to nitriding tailings in the corrosion agent is 0.5-1.5:1.5-2.5:
100.
9. The method for preparing high-quality sponge titanium raw material using ilmenite according to claim 1, characterized in that: Step 5) corrosion, the temperature of the corrosion reaction is 65-85°C, the concentration of the corrosion agent is 0.5-3wt%, the solid-liquid ratio is 4-8, the stirring rate is 150-300r / min, and the air flow rate is 1-2.6L·min -1 ·m -3 , time is 3 to 4 hours; the temperature of the leaching separation is 250 to 320°C, and the time is 2 hours.
10. The method for preparing high-quality sponge titanium raw material using ilmenite according to claim 1, characterized in that: Step 6) chlorination reaction, the amount of petroleum coke added is 12-17wt% of the iron removal tailings; the temperature of the chlorination reaction is 800-1050°C, the reaction time is 8-10.5h, and the amount of chlorinating agent introduced is 0.2L / min; Preferably, the chlorinating agent is chlorine gas.
Citation Information
Cited By
Preparation method of high-carbon, high-nitrogen and high-oxygen sponge titanium
CN121518827A