Titanium alloy propeller hub laser repairing material and repairing method
Using titanium alloy propeller hub laser repair materials and repair methods, laser deposition technology is used to repair the helicopter propeller hub under the protection of argon gas, which solves the problem of complex propeller hub structure and easy damage, achieves efficient repair effects, reduces costs and improves The quality and stability of the repair layer are improved.
Patent Information
- Application Number
- CN202410978330.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-08
AI Technical Summary
Due to its complex structure and easy damage, the helicopter propeller hub component lacks effective repair methods, resulting in the failure and scrapping of key moving parts, and high manufacturing and use costs.
Titanium alloy propeller hub laser repair materials and repair methods are used to obtain alloy powder through vacuum smelting. The spherical particle size is 45-100 μm. Laser deposition technology is used to repair under argon protection, combined with adaptive material reduction and efficient processing to ensure repair. Mechanical properties and dimensional accuracy of the parts.
It achieves effective repair of the propeller hub, restores its use value, avoids the scrapping of the helicopter, reduces economic losses, and provides a crack-free repair layer through metallurgical fusion. The combined interface is simple to operate, has low equipment and environmental requirements, and is suitable for engineering. application.
Smart Images

Figure CN118745537A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of helicopter hub maintenance, and in particular to a titanium alloy hub laser repair material and a repair method. Background Art
[0002] The helicopter's key component hub system mainly includes three parts: the main hub, the tail hub and the automatic inclinometer. At present, most of the mainstream helicopters in the world use the third-generation flexible hub technology. The main load-bearing material of this hub has been replaced by high-strength Ti-10V-2Fe-3Al titanium alloy instead of the high-quality alloy steel commonly used in the past. Ti-10V-2Fe-3Al titanium alloy has high specific strength, good fracture toughness and strong corrosion resistance, and is widely used in various types of helicopters in service and under development. Due to the complex structure of the hub component and the easy damage during use, there is no effective repair method for these, resulting in the failure and scrapping of key moving parts, long replacement cycle and high manufacturing and use costs.
[0003] Laser deposition repair technology can overcome the shortcomings of traditional welding continuous repair, such as the accumulation of thermal effects and the large heat-affected zone, and ensure the mechanical properties and dimensional accuracy of the repaired parts and surrounding areas. Based on laser deposition technology, combined with adaptive material reduction and efficient processing, the damaged titanium alloy key components of the helicopter hub are remanufactured and repaired to meet the comprehensive mechanical properties. Summary of the invention
[0004] The purpose of the present invention is to propose a titanium alloy hub laser repair material and repair method to address the problem that hub components are complex in structure and easily damaged during use, and there is no effective repair method, which causes key moving parts to fail and be scrapped.
[0005] The technical solution implemented by the present invention is as follows: A titanium alloy propeller hub laser repair material, comprising, by weight percentage, 9.0-11.0% V, 1.6-2.2% Fe, 2.6-3.4% Al, 0-0.05% C, 0-0.05% N, 0-0.015% H, 0-0.005% Y, 0-0.005% O, and a remainder of Ti.
[0006] A method for laser repairing a titanium alloy propeller hub, the steps are as follows: (1) The alloy of the required composition is obtained by vacuum melting, in which, by weight percentage, V: 9.0-11.0%, Fe: 1.6-2.2%, Al: 2.6-3.4%, C: 0-0.05%, N: 0-0.05%, H: 0-0.015%, Y: 0-0.005%, O: 0-0.13%, and the balance is Ti; (2) Atomizing the alloy into powder, the spherical powder particle size is 45-100 mm; (3) Grind the hub to be repaired to remove the surface oxide layer and surface crack defects, and use anhydrous ethanol to clean the repair surface; (4) Use laser deposition technology to clad the area that needs to be repaired: (5) The repair process is carried out under argon protection, and a sealed bag is used to provide all-round sealed argon protection for the entire repair process; (6) After the repair is completed, the repair area is subjected to penetrant testing to ensure that no cracks or holes are found; (7) Grind the cladding residue in the repair area to ensure that the surface quality of the repair area meets the use requirements.
[0007] The process parameters of the laser deposition repair are as follows: The laser power is 6.5-7.5kW, the scanning rate is 1.0-1.2 m / min, the powder feeding rate is 1.2-1.4 Kg / h, the powder feeding gas flow rate is 7.0-1.0 L / min, the optical path air pressure value is 0.5 MPa, the scanning spacing is 5-6 mm, the spot diameter is 8 mm, and the light-to-powder distance is 15 mm.
[0008] The hub is ground at the position to be repaired by using a grinder and by hand; the grinder is used to grind the cladding excess in the repaired area.
[0009] The beneficial effect of the present invention is that the present invention can realize the repair of the propeller hub, restore the use value of the propeller hub, avoid the scrapping of the helicopter, and reduce economic losses. The present invention provides a new repair material and repair process for the surface defect repair of titanium alloy propeller hubs. The repair layer has no cracks, and the bonding interface between the repair layer and the substrate is metallurgical fusion with uniform structure, which provides a new solution for laser repair of titanium alloy propeller hubs. The present invention is simple to operate, and the selected process parameters have very low requirements on equipment and environment, which is close to actual engineering applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 This is a flowchart of the laser repair method for titanium alloy hub of the present invention; Figure 2 The tensile strength and elongation after break values in Examples 1-6. DETAILED DESCRIPTION
[0011] This embodiment provides a titanium alloy propeller hub laser repair material and repair method, and the repair method steps are as follows: Figure 1 shown.
[0012] In this embodiment, the repair material is composed of the following components in weight percentage: V: 9.0-11.0%, Fe: 1.6-2.2%, Al: 2.6-3.4%, C: 0-0.05%, N: 0-0.05%, H: 0-0.015%, Y: 0-0.005%, O: 0-0.13%, and Ti as the balance.
[0013] The above repair materials are atomized into 45-100 mm powders, and the area to be repaired is clad by laser deposition technology. The laser power is 6.5-7.5 kW, the scanning rate is 1.0-1.2 m / min, the powder feeding rate is 1.2-1.4 Kg / h, the powder feeding gas flow rate is 7.0-1.0 L / min, the optical path pressure value is 0.5 MPa, the scanning spacing is 5-6 mm, the spot diameter is 8 mm, and the light-powder distance is 15 mm. The processing process is carried out under argon protection. After the processing is completed, the repair position is inspected, polished and flawed to ensure that the repair layer has no cracks and defects and is well fused.
[0014] Example 1 In this embodiment, the laser deposition repair material is composed of the following components by weight percentage: V: 9.0%, Fe: 1.6%, Al: 3.4%, C: 0.05%, N: 0.05%, H: 0.01%, Y: 0.005%, O: 0.13%, and Ti as the balance.
[0015] The above repair materials were atomized into powders of 45-100 mm, and the areas to be repaired were clad using laser deposition technology. The laser power was 6.5 kW, the scanning rate was 1.1 m / min, the powder feeding rate was 1.3 Kg / h, the powder feeding gas flow rate was 9.0 L / min, the optical path pressure was 0.5 MPa, the scanning spacing was 5.5 mm, the spot diameter was 8 mm, and the light-powder distance was 15 mm. The processing was carried out under argon protection. After the processing was completed, the repair position was inspected, polished and inspected to ensure that the repair layer was free of cracks and defects and well fused. After inspection, the tensile strength was 869.94 MPa, the elongation after fracture was 16.39%, and the impact toughness was 62.3J; the tensile strength and elongation after fracture were as follows Figure 2 shown.
[0016] Example 2 In this embodiment, the laser deposition repair material is composed of the following components by weight percentage: V: 11.0%, Fe: 2.2%, Al: 2.6%, C: 0.03%, N: 0.04%, H: 0.012%, Y: 0.003%, O: 0.11%, and the remainder is Ti.
[0017] The above repair materials were atomized into powders of 45-100 mm, and the areas to be repaired were clad using laser deposition technology. The laser power was 6.7 kW, the scanning rate was 1.2 m / min, the powder feeding rate was 1.2 Kg / h, the powder feeding gas flow rate was 8.0 L / min, the optical path pressure was 0.5 MPa, the scanning spacing was 5.5 mm, the spot diameter was 8 mm, and the light-powder distance was 15 mm. The processing was carried out under argon protection. After the processing was completed, the repair position was inspected, polished and inspected to ensure that the repair layer was free of cracks and defects and well fused. After inspection, the tensile strength was 860.74 MPa, the elongation after fracture was 15.82%, and the impact toughness was 66.3 J; the tensile strength and elongation after fracture were as follows Figure 2 shown.
[0018] Example 3 In this embodiment, the laser deposition repair material is composed of the following components by weight percentage: V: 10.5%, Fe: 2.0%, Al: 2.8%, C: 0.01%, N: 0.02%, H: 0.011%, Y: 0.002%, O: 0.11%, and Ti as the balance.
[0019] The above repair materials were atomized into 45-100mm powders, and the areas to be repaired were clad using laser deposition technology. The laser power was 6.9 kW, the scanning rate was 1.1 m / min, the powder feeding rate was 1.2 Kg / h, the powder feeding gas flow rate was 7.0L / min, the optical path pressure was 0.5 MPa, the scanning spacing was 5.5 mm, the spot diameter was 8 mm, and the light-to-powder distance was 15 mm. The processing was carried out under argon protection. After the processing was completed, the repair position was inspected, polished and inspected to ensure that the repair layer was free of cracks and defects and well fused. After inspection, the tensile strength was 852.70 MPa, the elongation after fracture was 15.60%, and the impact toughness was 62.3J; the tensile strength and elongation after fracture were as follows Figure 2 shown.
[0020] Example 4 In this embodiment, the laser deposition repair material is composed of the following components by weight percentage: V: 9.5%, Fe: 1.8%, Al: 3.2%, C: 0.05%, N: 0.01%, H: 0.005%, Y: 0.005%, O: 0.08%, and the remainder is Ti.
[0021] The above repair materials were atomized into 45-100mm powders, and the areas to be repaired were clad using laser deposition technology. The laser power was 7.1 kW, the scanning rate was 1.2 m / min, the powder feeding rate was 1.4 Kg / h, the powder feeding gas flow rate was 9.0 L / min, the optical path pressure was 0.5 MPa, the scanning spacing was 6 mm, the spot diameter was 8 mm, and the light-to-powder distance was 15 mm. The processing was carried out under argon protection. After the processing was completed, the repair position was inspected, polished and inspected to ensure that the repair layer was free of cracks and defects and well fused. After inspection, the tensile strength was 831.83 MPa, the elongation after fracture was 21.41%, and the impact toughness was 71.7 J; the tensile strength and elongation after fracture were as follows Figure 2 shown.
[0022] Example 5 In this embodiment, the laser deposition repair material is composed of the following components by weight percentage: V: 9.8%, Fe: 1.9%, Al: 3.0%, C: 0.01%, N: 0.04%, H: 0.015%, Y: 0.002%, O: 0.10%, and the remainder is Ti.
[0023] The above repair materials were atomized into powders of 45-100 mm, and the areas to be repaired were clad using laser deposition technology. The laser power was 7.3 kW, the scanning rate was 1.1 m / min, the powder feeding rate was 1.3 Kg / h, the powder feeding gas flow rate was 10L / min, the optical path pressure was 0.5 MPa, the scanning spacing was 5.5 mm, the spot diameter was 8 mm, and the light-to-powder distance was 15 mm. The processing was carried out under argon protection. After the processing was completed, the repair position was inspected, polished and inspected to ensure that the repair layer was free of cracks and defects and well fused. After inspection, the tensile strength was 839.35 MPa, the elongation after fracture was 22.19%, and the impact toughness was 90.6J; the tensile strength and elongation after fracture were as follows Figure 2 shown.
[0024] Example 6 In this embodiment, the laser deposition repair material is composed of the following components by weight percentage: V: 9.2%, Fe: 1.7%, Al: 3.4%, C: 0.02%, N: 0.04%, H: 0.012%, Y: 0.004%, O: 0.11%, and the remainder is Ti.
[0025] The above repair materials were atomized into powders of 45-100 mm, and the areas to be repaired were clad using laser deposition technology. The laser power was 7.5 kW, the scanning rate was 1.1 m / min, the powder feeding rate was 1.2 Kg / h, the powder feeding gas flow rate was 8.0 L / min, the optical path pressure was 0.5 MPa, the scanning spacing was 5 mm, the spot diameter was 8 mm, and the light-to-powder distance was 15 mm. The processing was carried out under argon protection. After the processing was completed, the repair position was inspected, polished and inspected to ensure that the repair layer was free of cracks and defects and well fused. After inspection, the tensile strength was 849.16 MPa, the elongation after fracture was 25.18%, and the impact toughness was 73.2 J; the tensile strength and elongation after fracture were as follows Figure 2 shown.
Claims
1. A titanium alloy propeller hub laser repair material, It is characterized in that The materials are calculated by weight percentage: V: 9.0-11.0%, Fe: 1.6-2.2%, Al: 2.6-3.4%, C: 0-0.05%, N: 0-0.05%, H: 0-0.015%, Y: 0-0.005%, O: 0-0.13%, and the balance is Ti.
2. A method for laser repair of titanium alloy propeller hub, It is characterized in that The method steps are as follows: (1) The alloy of the required composition is obtained by vacuum melting, in which, by weight percentage, V: 9.0-11.0%, Fe: 1.6-2.2%, Al: 2.6-3.4%, C: 0-0.05%, N: 0-0.05%, H: 0-0.015%, Y: 0-0.005%, O: 0-0.13%, and the balance is Ti; (2) Atomizing the alloy into powder, the spherical powder particle size is 45-100 mm; (3) Grind the hub to be repaired to remove the surface oxide layer and surface crack defects, and use anhydrous ethanol to clean the repair surface; (4) Use laser deposition technology to clad the area that needs to be repaired: (5) The repair process is carried out under argon protection, and a sealed bag is used to provide all-round sealed argon protection for the entire repair process; (6) After the repair is completed, the repair area is subjected to penetrant testing to ensure that no cracks or holes are found; (7) Grind the cladding residue in the repair area to ensure that the surface quality of the repair area meets the use requirements.
3. The method for laser repairing a titanium alloy propeller hub according to claim 2, It is characterized in that The process parameters of the laser deposition repair are as follows: The laser power is 6.5-7.5kW, the scanning rate is 1.0-1.2 m / min, the powder feeding rate is 1.2-1.4 Kg / h, the powder feeding gas flow rate is 7.0-1.0 L / min, the optical path air pressure value is 0.5 MPa, the scanning spacing is 5-6 mm, the spot diameter is 8 mm, and the light-to-powder distance is 15 mm.
4. The method for laser repairing a titanium alloy propeller hub according to claim 2, It is characterized in that The hub is ground at the position to be repaired by a grinder and manually; the grinder is used to grind the cladding residue in the repaired area.