Method for improving impact toughness of aluminum alloy for automobile chassis forge piece
Through multi-directional isothermal thermal compression deformation, short-term insulation and aging heat treatment, combined with electromagnetic impact treatment, the microstructure of the aluminum alloy is controlled, which solves the problem of insufficient impact toughness of aluminum alloy for automobile chassis forgings and significantly improves its strength, toughness and service life. performance.
Patent Information
- Application Number
- CN202410797653.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-08
AI Technical Summary
It is difficult to effectively improve the impact toughness of aluminum alloys used for automotive chassis forgings with existing technology, causing them to be easily damaged and fatigued in harsh environments, affecting their service life and safety.
By optimizing multi-directional isothermal thermal compression deformation, short-term insulation and aging heat treatment, combined with electromagnetic impact treatment, the grains, intragranular precipitates and grain boundary microstructure of the aluminum alloy are controlled to significantly improve its strength, toughness and impact resistance.
It significantly improves the impact toughness and service performance of aluminum alloys, achieves high reliability and long life of aluminum alloy forgings, and improves its performance in automotive applications.
Smart Images

Figure CN118745561A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular relates to a method for improving the impact toughness of aluminum alloys used for automobile chassis forgings. Background Art
[0002] Aluminum alloy forgings are used more and more frequently in the manufacturing of automotive parts. In actual use, the environment in which they are used is relatively harsh. Various external effects, such as heat, mechanical and radiation, will affect the performance of metal forgings, easily leading to damage or even fatigue failure of forgings, thereby shortening the service life of forgings and reducing safety.
[0003] Impact toughness refers to the ability of metal materials to resist damage (the ability to absorb plastic deformation work and fracture work) under impact load. Its size represents the ability of the sample to suppress the appearance of original cracks and is a key performance indicator that can indirectly reflect the fracture and fatigue properties of the alloy. The microstructure that affects the impact toughness of the alloy is mainly composed of grains, precipitation phases and grain boundary microstructures. The casting process is used to control the composition of the aluminum alloy and refine the cast aluminum alloy grains, and further large deformation or severe plastic deformation is used to greatly refine the aluminum alloy grains. Conventional heat treatment can optimize and control the distribution of precipitation phases in the grains, thereby ensuring the toughness of the aluminum alloy (patents CN 117758111 A, CN 115927936 A, CN 115927936 A, CN115707789 A) and impact resistance (CN 113462937 A). Existing studies have shown (International Journal of Fatigue, 2017, 94: 30-40; International Journal of Plasticity, 2018, 110: 38-56; Acta Materialia, 2021, 204: 116492) that the evolution of the metal alloy interface microstructure and the resulting changes in the interface stress state are one of the key factors affecting crack initiation and propagation and controlling the fracture and fatigue properties of aluminum alloys, which seriously restricts the high reliability and long service life of lightweight automotive alloy forgings.
[0004] In view of the fatigue cracking problem of aluminum alloys used in specific engineering applications (such as automobile chassis forgings), it is urgently necessary to develop a method to improve the impact toughness of aluminum alloys used in automobile chassis forgings, comprehensively regulate the grains, precipitation phase distribution and grain boundary microstructure in the microstructure, and further improve the impact toughness of aluminum alloys by purposefully preparing ultrafine grains, dispersing precipitation phase distribution within grains, and improving the distribution of aluminum alloy interface microstructure (width of grain boundary non-precipitation precipitation zone, grain boundary precipitation phase distribution and grain boundary bridging state). This is of great significance to improving the service performance of automobile aluminum alloy chassis forgings. Summary of the invention
[0005] The purpose of the present invention is to provide a method for improving the impact toughness of aluminum alloys for automobile chassis forgings, by optimizing the multi-directional isothermal hot compression deformation and aging heat treatment system, improving the distribution of aluminum alloy grains and intracrystalline precipitation phases, and on this basis matching the optimized electromagnetic impact treatment parameters, further optimizing and regulating the grain boundary precipitation phases and grain boundary morphology, so as to achieve the purpose of greatly improving the strength and toughness of aluminum alloys and improving the service performance of automobile aluminum alloy forgings.
[0006] In order to achieve the above purpose, the technical solutions adopted are as follows:
[0007] The method for improving the impact toughness of aluminum alloy for automobile chassis forgings comprises the following steps:
[0008] S1) subjecting the original extruded aluminum alloy bar to high temperature solid solution treatment and quenching to obtain an aluminum alloy billet;
[0009] S2) subjecting the obtained aluminum alloy billet to multi-directional isothermal hot compression deformation strengthening;
[0010] S3) short-term heat preservation of the aluminum alloy strengthened by multi-directional hot compression deformation; matching the corresponding heat preservation time and heat preservation temperature according to the distribution state of the precipitation phase in the aluminum alloy crystal after the multi-directional hot compression deformation;
[0011] S4) quenching the aluminum alloy after heat preservation and then performing aging heat treatment;
[0012] S5) performing electromagnetic shock treatment on the aluminum alloy subjected to aging heat treatment; matching corresponding electromagnetic shock treatment process methods and parameters according to the distribution state of precipitation phase at the grain boundaries of the aluminum alloy after aging heat treatment.
[0013] According to the above scheme, the original extruded aluminum alloy bar material used in step S1 is 6082 aluminum alloy, and its chemical composition is Mg: (0.8~1.0)%, Si: (0.9~1.2)%, Mn: (0.4~0.6)%, Fe: (0.3~0.4)%, Cu: (0.06~0.08)%, Cr: (0.05~0.08)%, Zn: (0.02~0.04)%, Ti: (0.03~0.04)%, and the rest is Al and unavoidable impurities.
[0014] According to the above scheme, the average grain size d of the extruded aluminum alloy bar material used in step S1 is ave ≤100μm.
[0015] According to the above scheme, the solution temperature used in step S1 is 535-545° C.; the solution time is 60-120 min.
[0016] According to the above scheme, the multi-directional isothermal hot compression deformation process used in step S2 includes:
[0017] First, compress (20-25)% along the extrusion direction (ED) of the extruded rod, and then compress (10-15)% along the cross-sectional direction (TD), and repeat 3 times; the deformation temperature is 400-440℃, and the deformation rate is 0.1-10s -1 , the cumulative deformation is 50 to 80%.
[0018] According to the above scheme, step S3 matches the corresponding holding time and holding temperature according to the distribution state of the precipitated phase in the aluminum alloy crystal after multi-directional hot compression deformation, including the following steps:
[0019] If there is basically no fine dispersed precipitate phase in the crystal, the holding temperature is 445-455°C and the holding time is 3-5 minutes;
[0020] If there are a small amount of fine dispersed precipitates in the crystal, the area fraction of the precipitates Then the holding temperature is 455-465°C and the holding temperature is 2-3min;
[0021] If there are a small amount of fine dispersed precipitates in the crystal, the area fraction of the precipitates The insulation temperature is 465-475°C, and the insulation temperature is 1-2 minutes.
[0022] According to the above scheme, the aging heat treatment temperature in step S4 is 175-185° C., and the aging heat treatment time is 5-8 hours.
[0023] According to the above scheme, step S5 matches the corresponding electromagnetic impact treatment process method and parameters according to the distribution state of the precipitation phase at the grain boundary of the aluminum alloy after aging heat treatment, including the following steps:
[0024] If there is no precipitation at the grain boundary, the average width w ave ≤20nm and the average spacing of the grain boundary precipitates l ave ≥100nm, the peak current density of the pulse current is in the range of 20~100A / mm 2 The pulse current frequency range is 20-50Hz, the pulse duty cycle is 25-40%, the pulse current action time is 0.12-0.48s, and the surface temperature rise of the sample during the treatment does not exceed 30℃. If it exceeds 30℃, the electromagnetic shock treatment is stopped and waited to cool to room temperature before the electromagnetic shock treatment is repeated.
[0025] According to the above scheme, step S5 matches the corresponding electromagnetic impact treatment process method and parameters according to the distribution state of the precipitation phase at the grain boundary of the aluminum alloy after aging heat treatment, including the following steps:
[0026] If there is no precipitation at the grain boundary, the average width w ave >20nm and the average spacing of the grain boundary precipitates is l ave <100nm, the electromagnetic shock treatment is carried out in two steps:
[0027] (1) The peak current density of the pulse current is in the range of 100 to 200 A / mm 2 , the pulse current frequency range is 30-100Hz, the pulse duty ratio is 10-15%, the pulse current action time is 0.48-1.2s, and the surface temperature rise of the sample during the treatment process does not exceed 60℃. If it exceeds 60℃, the electromagnetic shock treatment is stopped and waited to cool to room temperature before re-performing the electromagnetic shock treatment;
[0028] (2) The peak current density of the pulse current is in the range of 50 to 100 A / mm 2 The pulse current frequency range is 100-200Hz, the pulse duty cycle is 15-25%, the pulse current action time is 0.08-0.24s, and the surface temperature rise of the sample during the treatment process does not exceed 30℃. If it exceeds 30℃, the electromagnetic shock treatment is stopped and waited to cool to room temperature before the electromagnetic shock treatment is repeated.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present invention adopts high-temperature solid solution to ensure that the solute atoms of the extruded aluminum alloy original billet are completely dissolved; multi-directional isothermal hot compression and severe plastic deformation are used to perform deformation strengthening treatment on the aluminum alloy, and the grains are significantly refined; the aluminum alloy after multi-directional hot compression deformation strengthening is briefly heat-insulated to ensure that fine precipitated phases that may be precipitated during the multi-directional hot compression process are dissolved back, and the solute atoms are completely dissolved before aging treatment; after short-time heat insulation, the precipitation phase distribution is optimized by optimizing the heat treatment parameters; finally, based on the grain boundary state of the aluminum alloy after deformation heat treatment, appropriate electromagnetic shock treatment parameters are matched to further regulate the interface precipitation phase distribution and the interface bridging state.
[0031] The present invention adjusts the aluminum alloy grain distribution and the distribution state of the precipitation phase in the grain to the optimum through multi-directional isothermal hot compression deformation, short-time heat preservation and aging heat treatment system. On this basis, according to the grain boundary state of the aluminum alloy after aging heat treatment, the width of the grain boundary non-precipitation zone, the distribution of the precipitation phase at the grain boundary and the grain boundary connection state are further improved through electromagnetic impact treatment, so as to realize the ultra-high strength and toughness of the aluminum alloy for automobile chassis forgings and achieve the purpose of improving the service performance of automobile aluminum alloy chassis components. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 : Schematic diagram of the method for preparing the aluminum alloy raw material adopted in the present invention.
[0033] Figure 2 : A diagram of the electromagnetic impact treatment process of aluminum alloy prepared by the present invention.
[0034] Figure 3 : Tensile fracture morphology of aluminum alloy raw materials.
[0035] Figure 4 : The tensile fracture morphology of the aluminum alloy prepared by the present invention.
[0036] Figure 5 : Impact fracture morphology of aluminum alloy raw materials.
[0037] Figure 6 : Impact fracture morphology of the aluminum alloy prepared by the present invention. DETAILED DESCRIPTION
[0038] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.
[0039] The specific implementation method provides a method for improving the impact toughness of aluminum alloy for automobile chassis forgings:
[0040] S1) The original extruded aluminum alloy bar is subjected to high temperature solid solution and quenching to obtain an aluminum alloy billet; the solid solution temperature is 535-545°C; the solid solution time is 60-120min; the preparation method of the aluminum alloy raw material that can be used is as shown in the attached Figure 1 shown.
[0041] S2) The obtained aluminum alloy billet is subjected to multi-directional isothermal hot compression deformation strengthening; firstly, the aluminum alloy billet is compressed (20-25)% along the extrusion direction (ED) of the extruded rod, and then compressed (10-15)% along the cross-sectional direction (TD), and this is repeated 3 times; wherein the deformation temperature is 400-440°C, and the deformation rate is 0.1-10s -1 , the cumulative deformation is 50 to 80%.
[0042] S3) short-term heat preservation of the aluminum alloy strengthened by multi-directional hot compression deformation; matching the corresponding heat preservation time and heat preservation temperature according to the distribution state of the precipitation phase in the aluminum alloy crystal after the multi-directional hot compression deformation;
[0043] If there is basically no fine dispersed precipitate phase in the crystal, the holding temperature is 445-455°C and the holding time is 3-5 minutes;
[0044] If there are a small amount of fine dispersed precipitates in the crystal, the area fraction of the precipitates Then the holding temperature is 455-465°C and the holding temperature is 2-3min;
[0045] If there are a small amount of fine dispersed precipitates in the crystal, the area fraction of the precipitates The insulation temperature is 465-475°C, and the insulation temperature is 1-2 minutes.
[0046] S4) quenching the aluminum alloy after heat preservation and then performing aging heat treatment; the treatment temperature is 175-185° C. and the treatment time is 5-8 hours.
[0047] S5) performing electromagnetic impact treatment on the aluminum alloy subjected to aging heat treatment; matching corresponding electromagnetic impact treatment process methods and parameters according to the distribution state of the precipitation phase at the grain boundary of the aluminum alloy after aging heat treatment;
[0048] If there is no precipitation at the grain boundary, the average width w ave ≤20nm and the average spacing of the grain boundary precipitates l ave ≥100nm, the peak current density of the pulse current is in the range of 20~100A / mm 2 The pulse current frequency range is 20-50Hz, the pulse duty cycle is 25-40%, the pulse current action time is 0.12-0.48s, and the surface temperature rise of the sample during the treatment does not exceed 30℃. If it exceeds 30℃, the electromagnetic shock treatment is stopped and waited to cool to room temperature before the electromagnetic shock treatment is repeated.
[0049] If there is no precipitation at the grain boundary, the average width w ave >20nm and the average spacing of the grain boundary precipitates is l ave <100nm, the electromagnetic shock treatment is carried out in two steps:
[0050] (1) The peak current density of the pulse current is in the range of 100 to 200 A / mm 2 , the pulse current frequency range is 30-100Hz, the pulse duty ratio is 10-15%, the pulse current action time is 0.48-1.2s, and the surface temperature rise of the sample during the treatment process does not exceed 60℃. If it exceeds 60℃, the electromagnetic shock treatment is stopped and waited to cool to room temperature before re-performing the electromagnetic shock treatment;
[0051] (2) The peak current density of the pulse current is in the range of 50 to 100 A / mm 2 The pulse current frequency range is 100-200Hz, the pulse duty cycle is 15-25%, the pulse current action time is 0.08-0.24s, and the surface temperature rise of the sample during the treatment process does not exceed 30℃. If it exceeds 30℃, the electromagnetic shock treatment is stopped and waited to cool to room temperature before the electromagnetic shock treatment is repeated.
[0052] Specifically, the original extruded aluminum alloy bar material used in the specific embodiment is 6082 aluminum alloy with an average grain size of d ave ≤100μm; the chemical composition is Mg: (0.8~1.0)%, Si: (0.9~1.2)%, Mn: (0.4~0.6)%, Fe: (0.3~0.4)%, Cu: (0.06~0.08)%, Cr: (0.05~0.08)%, Zn: (0.02~0.04)%, Ti: (0.03~0.04)%, and the rest is Al and inevitable impurities.
[0053] The important technical parameters of the specific embodiment are shown in Table 1, Table 2 and Table 3. The characterization parameters of the aluminum alloy product obtained in the specific embodiment are shown in Table 3.
[0054] Table 1
[0055]
[0056] Table 2
[0057]
[0058] Table 3
[0059]
[0060]
[0061] Compared with Example 1, Comparative Example 1 did not undergo short-term heat preservation. Compared with the sample in Example 1, the strength of the sample in Comparative Example 1 was significantly reduced, the elongation was slightly increased, and the impact work was reduced. This is mainly because the strength of the aluminum alloy mainly depends on the distribution of the precipitated phase in the crystal. After the solid solution and quenching treatment, the alloy is in an oversaturated state. If short-term heat preservation is not performed, during the multi-directional hot compression and subsequent quenching process, the deformation energy storage may cause the supersaturated solid solution to precipitate. If the solid solution atoms nucleate and precipitate in large quantities in advance, they will continue to grow in the subsequent aging process, and eventually form a precipitate distribution with a coarse size and a small number density, which will significantly reduce the strength of the sample, thereby reducing the impact toughness. The main function of short-term heat preservation is to directly perform short-term heat preservation after the multi-directional hot compression is completed, so as to promote the complete dissolution of the fine precipitated phase precipitated during the deformation and quenching process, form a sufficient supersaturated solid solution, and ensure that the precipitated phase nucleates in large quantities and grows evenly during the subsequent aging process, forming a dispersed precipitate distribution with a small size and a large number density, thereby improving the strength and thus improving the impact toughness.
[0062] Compared with Example 1, Comparative Example 2 was not subjected to electromagnetic shock treatment. Compared with the sample in Example 1, the tensile strength of the sample in Comparative Example 2 was slightly decreased, the yield strength was significantly decreased, the elongation was slightly increased, and the impact work was reduced. This is mainly because grain bridging, as an external toughening method, can significantly improve the crack initiation work and crack propagation work of aluminum alloys, thereby increasing the energy absorbed by aluminum alloys during impact deformation. Through thermal deformation, short-term heat preservation, and aging heat treatment to refine the grains and regulate the distribution of precipitation phases within the crystals, and finally according to the distribution state of the interface precipitation phases, the electromagnetic shock treatment is used to specifically regulate the distribution of the interface precipitation phases and the interface connection state, promote grain boundary connection, and help improve the impact toughness of the aluminum alloy.
[0063] The mechanical properties of the 6082 aluminum alloy raw material and the 6082 aluminum alloy obtained in Example 1 were tested by room temperature tensile test. The test results showed that the average tensile strength, yield strength and elongation of the 6082 aluminum alloy raw material were 288MPa, 257MPa and 9.5%, respectively, while the average tensile strength, yield strength and elongation of the 6082 aluminum alloy obtained in Example 1 were 354MPa, 347MPa and 10.3%, respectively, with an increase of approximately 22.9%, 35.0% and 8.4%, respectively, and the mechanical properties of the aluminum alloy were significantly improved. See the attached tensile fracture morphology of the aluminum alloy raw material. Figure 3 The tensile fracture morphology of the aluminum alloy obtained in Example 1 is shown in the attached Figure 4 shown.
[0064] The impact toughness of the 6082 aluminum alloy raw material and the 6082 aluminum alloy obtained in Example 1 was tested by the Charpy impact test. The test results showed that the average impact energy of the 6082 aluminum alloy raw material was 61.5 J, while the average impact energy of the 6082 aluminum alloy obtained in Example 1 was 102.8 J, an increase of about 67%, achieving a significant improvement in the strength and toughness of the aluminum alloy. Figure 5 The impact fracture morphology of the aluminum alloy obtained in Example 1 is shown in the attached Figure 6 shown.
[0065] In summary, the present invention adopts high-temperature solid solution to ensure that its solute atoms are completely dissolved; multi-directional isothermal hot compression and severe plastic deformation are used to deform and strengthen the aluminum alloy, significantly refining the grains; the aluminum alloy after multi-directional hot compression deformation strengthening is kept warm for a short time to ensure that the fine precipitated phases that may precipitate during the multi-directional hot compression process are dissolved back, and the solute atoms are completely dissolved before aging treatment; after short-time insulation, the precipitate phase distribution is optimized by optimizing the heat treatment parameters; finally, based on the grain boundary state of the aluminum alloy after deformation heat treatment, the appropriate electromagnetic shock treatment parameters are matched to further regulate the interface precipitate phase distribution and the interface bridging state.
[0066] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.
Claims
1. A method for improving the impact toughness of aluminum alloy for automobile chassis forgings, characterized in that The following steps are involved: S1) subjecting the original extruded aluminum alloy bar to high temperature solid solution treatment and quenching to obtain an aluminum alloy billet; S2) subjecting the obtained aluminum alloy billet to multi-directional isothermal hot compression deformation strengthening; S3) short-term heat preservation of the aluminum alloy strengthened by multi-directional hot compression deformation; matching the corresponding heat preservation time and heat preservation temperature according to the distribution state of the precipitation phase in the aluminum alloy crystal after the multi-directional hot compression deformation; S4) quenching the aluminum alloy after heat preservation and then performing aging heat treatment; S5) performing electromagnetic shock treatment on the aluminum alloy subjected to aging heat treatment; matching corresponding electromagnetic shock treatment process methods and parameters according to the distribution state of precipitation phase at the grain boundaries of the aluminum alloy after aging heat treatment.
2. The method for improving the impact toughness of aluminum alloy for automobile chassis forgings according to claim 1, characterized in that The original extruded aluminum alloy bar material used in step S1 is 6082 aluminum alloy, and its chemical composition is Mg: (0.8-1.0)%, Si: (0.9-1.2)%, Mn: (0.4-0.6)%, Fe: (0.3-0.4)%, Cu: (0.06-0.08)%, Cr: (0.05-0.08)%, Zn: (0.02-0.04)%, Ti: (0.03-0.04)%, and the rest is Al and unavoidable impurities.
3. The method for improving the impact toughness of aluminum alloy for automobile chassis forgings according to claim 1, characterized in that The average grain size d of the extruded aluminum alloy bar used in step S1 is ave ≤100μm.
4. The method for improving the impact toughness of aluminum alloy for automobile chassis forgings according to claim 1, characterized in that The solution temperature used in step S1 is 535-545° C.; the solution time is 60-120 min.
5. The method for improving the impact toughness of aluminum alloy for automobile chassis forgings according to claim 1, characterized in that The multi-directional isothermal hot compression deformation process used in step S2 includes: First, compress the extruded rod by 20-25% along the extrusion direction, and then compress it by 10-15% along the cross-section direction. Repeat this process for 3 times; the deformation temperature is 400-440℃, and the deformation rate is 0.1-10s -1 , the cumulative deformation is 50 to 80%.
6. The method for improving the impact toughness of aluminum alloy for automobile chassis forgings according to claim 1, characterized in that Step S3 matches the corresponding holding time and holding temperature according to the distribution state of the precipitated phase in the aluminum alloy crystal after multi-directional hot compression deformation, including the following steps: If there is basically no fine dispersed precipitate phase in the crystal, the holding temperature is 445-455°C and the holding temperature is 3-5 minutes.
7. The method for improving the impact toughness of aluminum alloy for automobile chassis forgings according to claim 1, characterized in that Step S3 matches the corresponding holding time and holding temperature according to the distribution state of the precipitated phase in the aluminum alloy crystal after multi-directional hot compression deformation, including the following steps: If there are a small amount of fine dispersed precipitates in the crystal, the area fraction of the precipitates Then the holding temperature is 455-465°C and the holding temperature is 2-3min; If there are a small amount of fine dispersed precipitates in the crystal, the area fraction of the precipitates The insulation temperature is 465-475°C, and the insulation temperature is 1-2 minutes.
8. The method for improving the impact toughness of aluminum alloy for automobile chassis forgings according to claim 1, characterized in that In step S4, the aging heat treatment temperature is 175-185° C., and the aging heat treatment time is 5-8 hours.
9. The method for improving the impact toughness of aluminum alloy for automobile chassis forgings according to claim 1, characterized in that Step S5 matches the corresponding electromagnetic impact treatment process method and parameters according to the distribution state of the precipitation phase at the grain boundary of the aluminum alloy after the aging heat treatment, including the following steps: If there is no precipitation at the grain boundary, the average width w ave ≤20nm and the average spacing of the grain boundary precipitates l ave ≥100nm, the peak current density of the pulse current is in the range of 20~100A / mm 2 The pulse current frequency range is 20-50Hz, the pulse duty cycle is 25-40%, the pulse current action time is 0.12-0.48s, and the surface temperature rise of the sample during the treatment does not exceed 30℃. If it exceeds 30℃, the electromagnetic shock treatment is stopped and waited to cool to room temperature before the electromagnetic shock treatment is repeated.
10. The method for improving the impact toughness of aluminum alloy for automobile chassis forgings according to claim 1, characterized in that Step S5 matches the corresponding electromagnetic impact treatment process method and parameters according to the distribution state of the precipitation phase at the grain boundary of the aluminum alloy after the aging heat treatment, including the following steps: If there is no precipitation at the grain boundary, the average width w ave >20nm and the average spacing of the grain boundary precipitates is l ave <100nm, the electromagnetic shock treatment is carried out in two steps: (1) The peak current density of the pulse current is in the range of 100 to 200 A / mm 2 , the pulse current frequency range is 30-100Hz, the pulse duty ratio is 10-15%, the pulse current action time is 0.48-1.2s, and the surface temperature rise of the sample during the treatment process does not exceed 60℃. If it exceeds 60℃, the electromagnetic shock treatment is stopped and waited to cool to room temperature before re-performing the electromagnetic shock treatment; (2) The peak current density of the pulse current is in the range of 50 to 100 A / mm 2 The pulse current frequency range is 100-200Hz, the pulse duty cycle is 15-25%, the pulse current action time is 0.08-0.24s, and the surface temperature rise of the sample during the treatment process does not exceed 30℃. If it exceeds 30℃, the electromagnetic shock treatment is stopped and waited to cool to room temperature before the electromagnetic shock treatment is repeated.