Directional preparation method of diamond NV color center ensemble
By doping N atoms and annealing the diamond (111) film, the directional preparation of the NV color center ensemble is achieved, which solves the problem of random color center distribution, improves the magnetic field readout contrast and alignment rate, and is suitable for micromagnetic applications. measurement field.
Patent Information
- Application Number
- CN202410750510.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-08
AI Technical Summary
The existing technology cannot orientate the NV color center ensemble [111] on the diamond (111) surface, resulting in random distribution of color centers and reducing the alignment rate and magnetic field readout contrast.
Through the steps of ultrasonic cleaning, microwave plasma chemical vapor deposition, hydrofluoric acid stripping treatment and step flow growth, a diamond (111) film is prepared, doped with N atoms, and passed through a vacuum/atmosphere tube annealing furnace Form an NV color center ensemble [111] to achieve directional preparation.
The formation rate and alignment rate of the NV color center ensemble on the near surface of the diamond (111) film are improved, the magnetic field readout contrast is enhanced, and the application performance of the device is improved.
Smart Images

Figure CN118745595A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of diamond color centers, and in particular to a method for oriented preparation of a diamond NV color center ensemble. Background Art
[0002] An optical detection magnetic resonance device (ODMR) is a device that uses optical technology to detect and measure magnetic resonance signals. It usually includes an optical laser system, an optical detector, and a data processing system. By combining optical technology with magnetic resonance technology, high-sensitivity detection and measurement of weak magnetic resonance signals in biological tissues or material samples can be achieved, thus playing an important role in medical diagnosis, biomedicine, and materials science. Diamond NV color centers have won the favor of countless scholars and have conducted a large number of related studies due to their ultra-long coherence time and high magnetic sensitivity, and can be laser polarized and read at room temperature.
[0003] However, when using the existing technology to form the NV color center ensemble
[111] on the diamond film, there is a problem that the NV color center ensemble
[111] can only be randomly distributed on any one of the four surfaces of the diamond film, and the NV color center ensemble
[111] cannot be formed in a directionally manner on the diamond (111) surface (the diamond (111) surface is one of the surfaces on the diamond film). Summary of the invention
[0004] In view of this, an object of the present invention is to provide a method for oriented preparation of diamond NV color center ensemble, so as to solve the problem that the prior art cannot orient the NV color center ensemble
[111] on the diamond (111) plane.
[0005] The present invention discloses a method for directional preparation of a diamond NV color center ensemble, comprising the following steps:
[0006] S1, preliminary preparation: cleaning the silicon substrate by an ultrasonic cleaning machine; after taking out the silicon substrate, planting diamonds on the silicon substrate by diamond planting liquid; after taking out the silicon substrate, drying it with hot air.
[0007] S2, diamond substrate preparation: using microwave plasma chemical vapor deposition equipment, grow a diamond film with a thickness of about 2000nm-4000nm on the silicon substrate in step 1 as a diamond substrate.
[0008] S3, diamond film stripping treatment: using hydrofluoric acid, immersing the diamond film and silicon substrate prepared in step 2 in hydrofluoric acid, and heating the hydrofluoric acid to remove the silicon substrate and obtain a complete diamond film.
[0009] S4, step-flow growth of diamond (111) film: flip the diamond film in step 3 to obtain a diamond (111) substrate with the diamond (111) surface facing upward, and continue deposition to obtain a step-flow diamond (111) film.
[0010] S5, Directed preparation of diamond NV color centers
[0011] Preparation of N-doped diamond (111) film: The diamond (111) in step 4 is continued to grow in a step flow manner on the film, and N atoms are doped during the growth process. A microwave plasma chemical vapor deposition device is used to grow a N-containing diamond (111) film with a thickness of about 228nm-286nm on the diamond (111) substrate in step 4.
[0012] Formation of NV color center ensemble
[111] in diamond (111) film: Place the N-containing diamond (111) film grown in step 5 in a vacuum / atmosphere tubular annealing furnace for annealing to promote the formation of NV color center ensemble
[111] on the diamond (111) film and achieve directional preparation of diamond NV color center.
[0013] Specifically, the silicon substrate in S1 is a Φ50 mm×0.5 mm single-polished 111-surface silicon wafer.
[0014] Specifically, the temperature of ultrasonic cleaning in S1 is 25° C., the ultrasonic frequency is 800 Hz, the ultrasonic cleaning time is 10 min, and the cleaning liquid is anhydrous ethanol.
[0015] Specifically, CH4 in S2 is 2 sccm, H2 is 200 sccm, microwave power is 1200 W, temperature is 900°C, pressure is 4219 Pa, and duration is 60 h.
[0016] Specifically, in S3, the hydrofluoric acid is 30 ml and the relative molecular mass is 20%, the hydrofluoric acid heating temperature is 98° C., and the heating time is 15 min.
[0017] Specifically, CH4 in S4 is 2 sccm, H2 is 200 sccm, microwave power is 1200 W, temperature is 1050° C., pressure is 4219 Pa, duration is 14 h, and the thickness of the diamond (111) film is about 800 nm-1000 nm.
[0018] Specifically, in S5, CH4 is 0.2 sccm, H2 is 200 sccm, NH3 is 4 sccm, the microwave power is 1200 W, the temperature is 1050° C., the pressure is 4400 Pa, and the duration is 4 h.
[0019] Specifically, the heating temperature in S5 is 690° C. and the annealing time is 10 min.
[0020] The beneficial effects of the present invention are:
[0021] The present invention can directionally form the NV color center ensemble
[111] on the near surface of the diamond (111) film, thereby reducing the random distribution of the color centers in four directions and improving the alignment rate. Since the diamond NV color center ensemble near the surface is more easily excited, it is more beneficial for application in devices. On the other hand, compared with the other three surfaces of the diamond film, the NV color center ensemble
[111] is easier to form on the near surface of the diamond (111) film. Through the directional operation of the present invention, the formation rate of the NV color center ensemble
[111] on the diamond (111) film is indirectly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the NV color center model in four directions.
[0023] Figure 2 This is a point-line diagram of the formation energy of diamond NV color centers in different directions.
[0024] Figure 3 Schematic diagram of the step-flow growth mode of diamond.
[0025] Figure 4 Schematic diagram of the principle of preparing diamond (111) surface.
[0026] Figure 5 The following are SEM images of the front and back sides of the removed film.
[0027] Figure 6 This is the AFM detection image of diamond (111) film.
[0028] Figure 7 This is the Gaussian fitting Raman peak diagram of diamond (111) film.
[0029] Figure 8 This is the XRD detection diagram of diamond (111) film.
[0030] Fig. 9 This is the SEM image of the step-flow growth of diamond (111) film.
[0031] Fig.10 This is the fluorescence detection diagram of the diamond NV color center ensemble.
[0032] Fig.11 This is the Rabi oscillation spectrum of the diamond NV color center ensemble.
[0033] Fig.12 This is the ODMR diagram of the diamond NV color center ensemble. DETAILED DESCRIPTION
[0034] In order to clearly understand the technical solution of the present application, a method for oriented preparation of a diamond NV color center ensemble provided by the present application will be described in detail below with reference to specific embodiments and drawings.
[0035] The terms used in the following embodiments are only for the purpose of describing specific embodiments, and are not intended to be used as limitations to the present application. As used in the specification and claims of the present application, the singular expressions "one", "a kind of", "above", "the" and "this" are intended to also include expressions such as "one or more", unless there is a clear indication to the contrary in the context. It should also be understood that in the following embodiments of the present application, "at least one", "one or more" refer to one, two or more than two.
[0036] References to "one embodiment" or "some embodiments" etc. described in this specification mean that a particular feature, structure or characteristic described in conjunction with the embodiment is included in one or more embodiments of the present application. Thus, the phrases "one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. appearing in different places in this specification do not necessarily all refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized in other ways.
[0037] Example 1
[0038] This embodiment provides a method for oriented preparation of a diamond NV color center ensemble, comprising the following steps:
[0039] Step 1, preliminary preparation: clean the silicon substrate (for example, the silicon substrate can be a Φ50mm×0.5mm single-polished 111-surface silicon wafer) by using an ultrasonic cleaning machine (using an existing product on the market, which will not be described here); specifically, the ultrasonic cleaning temperature is 25°C, the ultrasonic frequency is 800Hz, the cleaning ultrasonic time is 10min each, and the cleaning liquid can directly select anhydrous ethanol. After taking out the above silicon substrate, blow dry it with hot air.
[0040] Step 2, preparation of diamond substrate: using microwave plasma chemical vapor deposition equipment, with specific parameters of CH4 2sccm, H2 200sccm, microwave power 1200W, temperature 900℃, pressure 4219Pa, and duration 60h, a diamond film with a thickness of about 2000nm-4000nm is grown on the silicon substrate in step 1 as a diamond substrate.
[0041] Step 3, diamond film stripping treatment: using hydrofluoric acid, the diamond film and silicon substrate prepared in step 2 are immersed in 30 ml of hydrofluoric acid with a relative molecular mass of 20%, and the hydrofluoric acid is heated at 98°C for 15 minutes to remove the silicon substrate and obtain a complete diamond film. Due to the presence of silicon oxide between the diamond and the silicon substrate, the silicon oxide can be decomposed by hydrofluoric acid to separate the diamond film from the silicon substrate, thereby achieving the removal of the silicon substrate.
[0042] Step 4, step flow growth of diamond (111) film: turn over the diamond film in step 3 to obtain a diamond (111) substrate with the diamond (111) facing upward, and continue deposition. The step flow growth chemical vapor deposition parameters of the diamond (111) film are: CH4 is 2sccm, H2 is 200sccm, microwave power is 1200W, temperature is 1050℃, pressure is 4219Pa, duration is 14h, and the thickness of the diamond (111) film is about 800nm-1000nm. When the diamond film grows on the diamond (111) substrate, it is based on the diamond deposition principle. The diamond deposition principle is: H atoms in H2 are ionized by plasma, so that the H atoms in H2 are decomposed and form H2 with H atoms in CH4, so that only C atoms fall.
[0043] In diamond crystals, the four valence electrons of each carbon atom form four completely identical atomic orbitals in sp3 hybridization, forming covalent bonds with the four most adjacent carbon atoms; the angles between these four covalent bonds are equal, about 109°28', and silicon crystals have the same lattice as diamonds, which is why the two can grow coherently. When silicon crystals are naturally exposed to air, oxygen atoms will be incorporated into the crystal gaps of silicon atoms to form silicon oxide. This incorporation does not change the crystal lattice of silicon atoms, which allows silicon-silicon oxide-diamond to grow coherently, which is the principle of diamond (111) substrate formation.
[0044] On a diamond (111) substrate, the process of growing a diamond (111) film layer by layer on the diamond (111) substrate by controlling parameters such as temperature and methane concentration during the MPCVD deposition process is also a type of homoepitaxial growth, namely, the step flow growth principle of the diamond (111) film.
[0010] Step 5: Directed preparation of diamond NV color centers
[0045] (1) Preparation of N-doped diamond (111) film: The diamond (111) in step 4 is continued to grow on the film in a step flow manner, and N atoms are doped during the growth process. A microwave plasma chemical vapor deposition device is used. The specific parameters are CH 4 is 0.2sccm, H2 200sccm, NH 3 The microwave power is 4 sccm, the microwave power is 1200 W, the temperature is 1050° C., the pressure is 4400 Pa, and the duration is 4 hours. A N-containing diamond (111) film with a thickness of about 228 nm to 286 nm is grown on the diamond (111) substrate in step 4.
[0046] (2) Formation of NV color center ensemble
[111] in diamond (111) film: The N-containing diamond (111) film grown in step 5 (1) is annealed in a vacuum / atmosphere tubular annealing furnace at a heating temperature of 690°C for 10 min to promote the formation of NV color center ensemble
[111] on the diamond (111) film and achieve directional preparation of diamond NV color centers.
[0047] The H atoms in H2 are ionized by plasma, so that the H atoms in H2 decompose and form H2 with the H atoms in NH3, making it easier for N atoms to fall, which is the principle of diamond NV color center ensemble deposition.
[0048] The present invention can directionally form the NV color center ensemble
[111] on the near surface of the diamond (111) film, thereby reducing the random distribution of the color centers in four directions and improving the alignment rate. Since the diamond NV color center ensemble near the surface is more easily excited, it is more beneficial for application in devices. On the other hand, compared with the other three surfaces of the diamond film, the NV color center ensemble
[111] is easier to form on the near surface of the diamond (111) film. Through the directional operation of the present invention, the formation rate of the NV color center ensemble
[111] on the diamond (111) film is indirectly improved.
[0049] In summary, the present invention breaks through the barriers of low magnetic field readout contrast and random distribution of color center directions (low alignment rate); the present invention realizes the directional preparation of NV color center ensemble by step-flow growth of NV color centers in diamond (111) thin film, reduces the random distribution of color centers in four directions, has low cost and high efficiency, and increases the magnetic field readout contrast characteristics, which has guiding significance for micromagnetic measurement and quantum sensing; and has an important impact on improving the sensitivity in the field of micromagnetic detection.
[0050] Compared with the diamond NV vacancy color center in the prior art, the directional preparation of the diamond NV color center system in the present invention can effectively solve the problem of low alignment rate and contrast of the diamond NV vacancy color center. Due to the principle that silicon-silicon oxide-diamond can achieve coherent growth, the surface of the diamond (111) film grown by step flow is very flat and smooth, and the crystal plane orientation is consistent with the (111) plane. Ammonia can be easily decomposed during the deposition process of the diamond film and enter the interior of the diamond film to form an NV color center system, which also provides basic conditions for the directional preparation of the NV color center system. Since nitrogen atoms and vacancies are more easily formed on the
[111] of the diamond (111) surface during the MPCVD deposition process, the alignment rate and contrast of the diamond NV color center are increased, and the magnetic measurement sensitivity of the diamond NV color center is greatly improved. Based on this, the directional preparation of the diamond NV color center system provides a new means for the field of weak magnetic measurement and opens a new chapter in weak magnetic measurement.
[0051] The experiment is as follows:
[0052] from Figure 1 It can be seen that the color centers located in four different directions are
[111] , from Figure 2 It can be seen that when the vacancy is at the
[111] point, the formation energy of the diamond NV color center is the smallest, with an energy of 7.23 eV. Figure 1 , Figure 2 It is proved that NV color center is more likely to form in the
[111] direction on the diamond (111) plane. Figure 1 is the NV color center model in four directions, Figure 2 This is a point-line diagram of the formation energy of diamond NV color centers in different directions.
[0053] from Figure 3 It can be seen from the figure that step flow growth will cause the diamond surface to grow in a planar trend; Figure 4 It can be seen that after the film is turned over, a flat, smooth and uniformly oriented diamond film can be obtained; Figure 3 , Figure 4 It is proved that the step flow growth has the same orientation of diamond surface; among them, Figure 3 Schematic diagram of diamond step-flow growth mode. Figure 4 Schematic diagram of the principle of preparing diamond (111) surface.
[0054] from Figure 5 As can be seen in (a), the entire diamond film is composed of diamond particles of about 2 μm in size squeezed together; Figure 5 It can be seen from (b) that although there are still gaps between these single crystal particles, it does not affect their combination into a plane; Figure 5(c) shows the boundary between each single crystal diamond; Figure 5 As can be seen in (d), there are almost no bumps or other crystals on the flipped surface; Figure 6 As shown in the figure, gaps between different grain boundaries can be observed, with a maximum peak height Rmax = 3.1nm, an average roughness Ra = 0.301nm, and a root mean square roughness Rq = 0.392nm. Figure 5 , Figure 6 The quality and smoothness of the diamond film surface were demonstrated; Figure 5 The SEM images of the front and back sides of the removed film, (a) front side, (b) front side magnified, (c) back side, (d) back side magnified, Figure 6 This is the AFM detection image of diamond (111) film.
[0055] from Figure 7 It can be seen that the diamond peak can be found at 1332 cm -1 The peak at 1200cm-1 is related to the vibration mode of trans-polyacetylene (TPA), which is attributed to the CH in-plane bending mode and CC, C=C stretching vibration mode. -1 The D peak near 1540 cm is due to the ring-shaped “breathing” vibration mode of the carbon sp2 phase, while the -1 and 1630cm -1 The G peak nearby is generated by the mixed vibration mode of the sp2 phase. As can be seen from Figure 8, the crystal plane orientation of the entire film is almost completely covered by the (111) orientation at 43.9°. Figure 7 , Figure 8 High-quality and highly oriented diamond (111) films were demonstrated; wherein, Figure 7 This is the Gaussian fitting Raman peak diagram of diamond (111) film. Figure 8 This is the XRD detection diagram of diamond (111) film.
[0056] As can be seen from Figure 9, the growth of diamond film is basically step-by-step growth, the grains are small and invisible, and the surface of each step is relatively smooth; as can be seen from Figure 10, its fluorescence intensity is higher, the zero phonon line of the NV color center is narrower, and the phonon sideband is more concentrated; Fig. 9 , Fig.10 The high fluorescence intensity of the step-flow generation on the surface of diamond (111) film and the ensemble orientation of diamond NV color centers was demonstrated; Fig. 9 This is the SEM image of diamond (111) film step flow growth. Fig.10 This is the fluorescence detection diagram of the diamond NV color center ensemble.
[0057] from Fig.11It can be seen from the figure that the NV color center exhibits a gradually decaying cosine characteristic spectrum; Fig.12 As can be seen in (a), the diamond NV color center has symmetrical peaks in four random directions. The contrast of the ordinary diamond NV color center along the
[111] direction reaches 0.8%, accounting for about 14% of the total contrast. Fig.12 As can be seen in (b), the diamond NV color center has only two symmetrical peaks in the orientation direction, while the contrast of the diamond NV color center prepared by step flow growth along the
[111] direction reaches 4.5%, accounting for about 45% of the total contrast. Fig.11 , Fig.12 It is proved that diamond NV color centers exist in the form of an ensemble. It is found that the random distribution direction of diamond NV color centers prepared by step flow growth is reduced, and the contrast of diamond NV color centers along the
[111] direction is improved, realizing the controllable preparation of diamond NV color center orientation. Fig.11 This is the Rabi oscillation spectrum of the diamond NV color center ensemble. Fig.12 This is the ODMR diagram of the diamond NV color center ensemble.
Claims
1. A method for directional preparation of a diamond NV color center ensemble, characterized in that: The steps include: S1, preliminary preparation: clean the silicon substrate with an ultrasonic cleaner; after taking out the silicon substrate, plant the diamond on the silicon substrate with diamond planting liquid; after taking out the silicon substrate, dry it with hot air S2, diamond substrate preparation: using microwave plasma chemical vapor deposition equipment, grow a diamond film with a thickness of about 2000nm-4000nm on the silicon substrate in step 1 as a diamond substrate S3, diamond film stripping treatment: using hydrofluoric acid, immersing the diamond film and silicon substrate prepared in step 2 in hydrofluoric acid, and heating the hydrofluoric acid to remove the silicon substrate to obtain a complete diamond film S4, step-flow growth of diamond (111) film: flip the diamond film in step 3 to obtain a diamond (111) substrate with the diamond (111) surface facing upward, and continue deposition to obtain a step-flow diamond (111) film. S5, Directed preparation of diamond NV color centers Preparation of N-doped diamond (111) film: Continue step flow growth of the diamond (111) in step 4 onto the film, and dope N atoms during the growth process, and use microwave plasma chemical vapor deposition equipment to grow a N-containing diamond (111) film with a thickness of about 228nm-286nm on the diamond (111) substrate in step 4 Formation of NV color center ensemble [111] in diamond (111) film: Place the N-containing diamond (111) film grown in step 5 in a vacuum / atmosphere tubular annealing furnace for annealing to promote the formation of NV color center ensemble [111] on the diamond (111) film and achieve directional preparation of diamond NV color centers.
2. The method for oriented preparation of diamond NV color center ensemble according to claim 1, characterized in that: The silicon substrate in S1 uses a Φ50 mm×0.5 mm single-polished 111-face silicon wafer.
3. The method for oriented preparation of diamond NV color center ensemble according to claim 1, characterized in that: The temperature of ultrasonic cleaning in S1 is 25°C, the ultrasonic frequency is 800 Hz, the ultrasonic cleaning time is 10 min, and the cleaning liquid is anhydrous ethanol.
4. The method for oriented preparation of diamond NV color center ensemble according to claim 1, characterized in that: The CH4 in S2 is 2 sccm, the H2 is 200 sccm, the microwave power is 1200 W, the temperature is 900 ° C, the pressure is 4219 Pa, and the duration is 60 h.
5. The method for oriented preparation of diamond NV color center ensemble according to claim 1, characterized in that: In S3, the hydrofluoric acid is 30 ml and the relative molecular mass is 20%, the hydrofluoric acid heating temperature is 98°C, and the heating time is 15 minutes.
6. The method for oriented preparation of diamond NV color center ensemble according to claim 1, characterized in that: In S4, CH4 is 2 sccm, H2 is 200 sccm, microwave power is 1200 W, temperature is 1050 °C, pressure is 4219 Pa, duration is 14 h, and the thickness of the diamond (111) film is about 800nm-1000nm.
7. The method for oriented preparation of diamond NV color center ensemble according to claim 1, characterized in that: In S5, CH4 is 0.2 sccm, H2 is 200 sccm, NH3 is 4 sccm, microwave power is 1200 W, temperature is 1050 °C, pressure is 4400 Pa, and duration is 4 h.
8. The method for oriented preparation of diamond NV color center ensemble according to claim 1, characterized in that: In S5, the heating temperature is 690°C and the annealing time is 10 min.
Citation Information
Cited By
Preparation method of MPCVD diamond film with high NV color center strength
CN119372619A
Preparation method and application of oriented NV color center diamond layer for vector magnetic field measurement
CN121137794A