Preparation method of bonding type blue light polymer fiber
By using green and environmentally friendly zinc ion and electrospinning technology, bonded blue light polymer fibers are prepared, which solves the problems of difficulty in preparing blue light fibers and low luminous efficiency, and achieves high-efficiency blue light luminescence performance and excellent anti-counterfeiting effect. Expanding its application in the field of anti-counterfeiting.
Patent Information
- Application Number
- CN202411089244.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-08
AI Technical Summary
The existing blue light anti-counterfeiting fiber technology lags behind in development, is difficult to prepare, and has low luminous efficiency. Commonly used raw materials such as beryllium have toxicity problems, and rare earth ion doping limits the luminous efficiency, limiting its application in daily life and medical fields.
Using green and environmentally friendly zinc ions, we first prepare an environmentally friendly and low-toxic blue reactive zinc complex, and then prepare bonded blue light polymer fibers through electrospinning technology, using Zn(BTZ)(UA) phosphor and polymethylmethacrylate Based on methyl acrylate-zinc phosphor, it forms an inorganic-organic dual material to improve the luminous efficiency and fiber morphology.
It achieves high-efficiency blue light luminescence performance, uniform fiber diameter, excellent anti-counterfeiting effect, reduces the risk of raw material toxicity, and expands the application potential of blue light fiber in the anti-counterfeiting field.
Smart Images

Figure CN118745602A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fluorescent fiber preparation, in particular to a method for preparing a bonded blue light polymer fiber. Background Art
[0002] Under the background of booming market economy, the phenomenon of commodity counterfeiting and counterfeiting is becoming more and more serious, which undoubtedly poses a threat to the legitimate rights and interests of enterprises, damages the brand image, and deprives consumers of their legitimate rights and interests. Therefore, the market demand for efficient anti-counterfeiting technology is becoming increasingly urgent. In order to maintain market order and protect the interests of all parties, the importance of anti-counterfeiting technology is self-evident. As an anti-counterfeiting technology, anti-counterfeiting fiber can improve the advancement and effectiveness of anti-counterfeiting means, cope with the constantly upgraded counterfeiting technology, make anti-counterfeiting means more sophisticated and complex, and increase the difficulty of counterfeiting.
[0003] Rare earth metal ion Eu 3 + It is often used as an activator or as an activator doped to construct red light anti-counterfeiting fiber. In the prior art, Zheng Zaiyong et al. used europium nitrate reagent and RE 3+ The hybrid phosphor was synthesized by coordination, which can be used in red light-emitting diodes and anti-counterfeiting fibers. Zang et al. prepared submicron-scale europium complex / PMMA red light ultrafine fibers with uniform fiber diameter and good concealment, which have good application prospects in the field of red light anti-counterfeiting. Li Zhen et al. prepared Eu by electrospinning technology. 3+ Doped LaPO 4 Red light micro-nano fiber. In the research of green light anti-counterfeiting fiber, the rare earth element Tb 3+ It is highly favored for its strong luminous intensity and high quantum efficiency. Shi Rui et al. used the solvent thermal method to prepare a special multi-layer six-petal-shaped green light micron crystal. The composite material has excellent fluorescence properties and can emit rare earth Tb 3+ The green fluorescence has a long fluorescence lifetime and has good application prospects in microscale fluorescence anti-counterfeiting. Liao Jinsheng et al. successfully synthesized terbium-doped CaF 2 :Tb 3+ Green light phosphor, this phosphor shows great application potential in the preparation of green light nano anti-counterfeiting fibers.
[0004] In the current research field of fluorescent anti-counterfeiting fibers, the research on red and green fibers is relatively mature and has been widely used in anti-counterfeiting fields such as banknotes and certificates. As a key component of tri-color fluorescent fibers, blue fiber has unique properties that enable it to be combined with other luminescent media to produce a diverse visible light spectrum, thus showing great potential in practical applications. Therefore, the innovation and development of blue fiber has vital research value in promoting the practical application of fluorescent anti-counterfeiting fibers.
[0005] However, the blue light anti-counterfeiting fiber technology still has the following problems: 1) Red light and green light anti-counterfeiting fibers have been widely studied and the preparation technology is relatively mature, but there are few reports on blue light metal organic anti-counterfeiting fibers; 2) The development of blue light anti-counterfeiting fibers is relatively lagging. Not only is the synthesis difficult, but the luminous efficiency also needs to be improved; commonly used preparation raw materials such as beryllium (Be) have toxicity problems, which limits their widespread application in daily life (such as anti-counterfeiting and medical fields); 3) Rare earth ions are currently often doped into polymer matrices to prepare blue light fibers. This method will limit the concentration of rare earth complexes, thereby affecting the luminous efficiency of the product and limiting its actual production application. Summary of the invention
[0006] The purpose of the present invention is to solve the problems existing in the above-mentioned prior art and to provide a method for preparing a bonded blue light polymer fiber.
[0007] The present invention is achieved through the following technical solutions: A method for preparing a bonded blue light polymer fiber comprises the following steps: 1) Preparation of Zn(BTZ)(UA) phosphor Weigh ZnCl 2 , 2-(2-hydroxyphenyl)benzothiazole (BTZ), and undecylenic acid (UAH), each of which was added with methanol and stirred until fully dissolved to obtain ZnCl 2 Solution, 2-(2-hydroxyphenyl)benzothiazole (BTZ) solution, undecylenic acid (UAH) solution.
[0008] Under water bath conditions, undecylenic acid (UAH) solution was added to a three-necked flask, and then ZnCl was added dropwise. 2 solution and NaOH ethanol solution to react; then 2-(2-hydroxyphenyl)benzothiazole (BTZ) solution was added dropwise to react; after the system was uniform, NaOH solution was added dropwise until a large amount of white precipitate was generated, and the system was closed to react.
[0009] The precipitate obtained by filtering and washing three times with methanol is dried to obtain the Zn(BTZ)(UA) phosphor.
[0010] 2) Preparation of polymethyl methacrylate-zinc phosphor Zn(BTZ)(UA) phosphor, methyl methacrylate (MMA) and initiator azobisisobutyronitrile (AIBN) were weighed separately and added into dimethyl sulfoxide (DMSO) solution, and ultrasonically stirred until the system was uniform.
[0011] The mixed solution was transferred to a test tube with a support, and dimethyl sulfoxide (DMSO) solution was added. After nitrogen was passed to deoxygenate, the system was sealed and placed in a constant temperature water bath until the reaction was complete.
[0012] The product was washed alternately with methanol and dimethyl sulfoxide (DMSO) solvents for 6 times to remove impurities, and then dried to obtain the polymethyl methacrylate-zinc phosphor.
[0013] 3) Preparation of bonded blue light polymer fibers The polymethyl methacrylate-zinc phosphor is dissolved in N,N-dimethylformamide (DMF) to prepare a spinning solution; an electrostatic spinning method is used to prepare a bonded blue light polymer fiber membrane, and after drying in an oven, the bonded blue light polymer fiber is obtained.
[0014] As a preferred technical solution, in step 1), ZnCl 2 The molar ratio of 2-(2-hydroxyphenyl)benzothiazole (BTZ) and undecylenic acid (UAH) is 1:1:1, and ZnCl 2 The ratio of 2-(2-hydroxyphenyl)benzothiazole (BTZ), undecylenic acid (UAH) and methanol was 1 mol:20 mL; the water bath reaction conditions were 50 °C, 180 r / min; ZnCl 2 The ratio of NaOH ethanol solution is 1 mol:0.4 mL, and the concentration of NaOH ethanol solution is 1 mol / L; ZnCl is added 2 After adding the solution and NaOH ethanol solution, the reaction time is 30 minutes; after adding 2-(2-hydroxyphenyl)benzothiazole (BTZ) solution, the reaction time is 30 minutes; the closed system reaction time is 4 hours; the drying temperature is 75°C and the time is 8 hours.
[0015] As a preferred technical solution, in step 2), the mass ratio of Zn(BTZ)(UA) phosphor, methyl methacrylate (MMA), and initiator azobisisobutyronitrile (AIBN) is 9:150:1; the ratio of Zn(BTZ)(UA) phosphor to the first added dimethyl sulfoxide (DMSO) solution is 9g:350mL; the ratio of Zn(BTZ)(UA) phosphor to the second added dimethyl sulfoxide (DMSO) solution is 9g:150mL; the ultrasonic stirring time is 30min; the nitrogen deoxygenation time is 30min; the temperature of the constant temperature water bath is set to 75°C, the reaction time is 32h; the drying temperature is 60°C and the time is 12h.
[0016] As a preferred technical solution, in step 3), the concentration of the prepared spinning solution is 16%; the parameters of electrospinning are spinning voltage 18 kV, propulsion speed 2 mL / h, receiving distance 20 cm; the drying temperature of the oven is 65°C, and the drying time is 8 hours.
[0017] Compared with the prior art, the present invention has the following beneficial effects: 1) The method of the present invention takes green and environmentally friendly zinc ions as the research object, adopts the technical means of first complexing and then polymerizing, first prepares environmentally friendly and low-toxic blue reactive zinc complexes, and then polymerizes to prepare bonded zinc blue light polymers. The obtained metal organic material has the characteristics of both inorganic and organic materials.
[0018] 2) The method of the present invention adopts electrospinning technology to spin bonded blue light polymer fibers, which have good fiber morphology, uniform diameter, high luminous efficiency, and will not cause fluorescence quenching due to agglomeration.
[0019] 3) The bonded blue light polymer fiber prepared by the method of the present invention has good luminescence performance and excellent anti-counterfeiting effect, and plays an important role in the innovation and development of anti-counterfeiting technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments of the present invention are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0021] Figure 1 1 and 2. Infrared spectra of Zn(BTZ)(UA) phosphor, 2-(2-hydroxyphenyl)benzothiazole (BTZ), homopolymer PMMA, polymer PMZn, and fiber FPMZn in Example 1 of the present invention.
[0022] Figure 2 It is the ultraviolet absorption spectra of Zn(BTZ)(UA) phosphor, 2-(2-hydroxyphenyl)benzothiazole (BTZ), undecylenic acid (UAH), homopolymer PMMA, polymer PMZn, and fiber FPMZn in Example 1 of the present invention.
[0023] Figure 3 This is the microscopic morphology and elemental composition diagram of the bonded blue light polymer fiber (fiber FPMZn) in Example 1 of the present invention.
[0024] Figure 4 1 is the fluorescence spectrum of the polymer PMZn and fiber FPMZn in Example 1 of the present invention and the fluorescence enhancement mechanism diagram.
[0025] Figure 5 This is a fluorescence attenuation curve diagram of the polymer PMZn and fiber FPMZn at 365nm and 395nm in Example 1 of the present invention.
[0026] Figure 6This is a comparison chart of the blue light anti-counterfeiting paper made of the bonded blue light polymer fiber (fiber FPMZn) in Example 1 of the present invention under 365 nm ultraviolet light and sunlight. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention. Example 1
[0028] A method for preparing a bonded blue light polymer fiber comprises the following steps: 1) Preparation of Zn(BTZ)(UA) phosphor Weigh 0.5 mol of ZnCl 2 , 2-(2-hydroxyphenyl)benzothiazole (BTZ), and undecylenic acid (UAH), each of which was added with 10 mL of methanol and stirred until fully dissolved to obtain ZnCl 2 Solution, 2-(2-hydroxyphenyl)benzothiazole (BTZ) solution, undecylenic acid (UAH) solution.
[0029] Under the conditions of 50℃ and 180 r / min in a water bath, undecylenic acid (UAH) solution was added into a three-necked flask, and ZnCl was added dropwise. 2 The solution was added with 0.2 mL of 1 mol / L NaOH ethanol solution and reacted for 30 min. Then, 2-(2-hydroxyphenyl)benzothiazole (BTZ) solution was added dropwise and reacted for 30 min. After the system was uniform, NaOH solution was added dropwise until a large amount of white precipitate was produced, and the closed system was reacted for 4 h.
[0030] The precipitate obtained by filtering and washing three times with methanol was dried at 75° C. for 8 h to obtain the Zn(BTZ)(UA) phosphor.
[0031] 2) Preparation of polymethyl methacrylate-zinc phosphor 0.18 g of Zn(BTZ)(UA) phosphor, 3 g of methyl methacrylate (MMA), and 0.02 g of initiator azobisisobutyronitrile (AIBN) were weighed separately and added into 7 mL of dimethyl sulfoxide (DMSO) solution, and ultrasonically stirred for 30 min until the system was uniform.
[0032] The mixed solution was transferred to a test tube with a support, and 3 mL of dimethyl sulfoxide (DMSO) solution was added. After nitrogen was passed through the system for 30 min to deoxygenate, the system was sealed and polymerized in a constant temperature water bath at 75°C for 32 h until the reaction was complete.
[0033] The product was washed alternately with methanol and dimethyl sulfoxide (DMSO) solvents for 6 times to remove impurities, and the product was dried at 60° C. for 12 h to obtain the polymethyl methacrylate-zinc phosphor, which was recorded as polymer PMZn.
[0034] 3) Preparation of bonded blue light polymer fibers The polymethyl methacrylate-zinc phosphor was dissolved in N,N-dimethylformamide (DMF) to prepare a spinning solution with a concentration of 16%. The electrospinning method was used to obtain a bonded blue light polymer fiber membrane with spinning parameters of 18 kV, 2 mL / h, and a receiving distance of 20 cm. The membrane was dried at an oven temperature of 65°C for 8 hours to obtain the bonded blue light polymer fiber, which was recorded as fiber FPMZn.
[0035] Figure 1 The infrared spectra of Zn(BTZ)(UA) phosphor, 2-(2-hydroxyphenyl)benzothiazole (BTZ), homopolymer PMMA, polymer PMZn, and fiber FPMZn in Example 1 are shown in the figure. 2+ , BTZ and UAH were successfully combined, and the complex was successfully polymerized with methyl methacrylate (MMA).
[0036] Figure 2 The UV absorption spectra of Zn(BTZ)(UA) phosphor, 2-(2-hydroxyphenyl)benzothiazole (BTZ), undecylenic acid (UAH), homopolymer PMMA, polymer PMZn, and fiber FPMZn in Example 1 are shown in the figure. It can be seen from the figure that the complex monomer Zn(BTZ)(UA) phosphor and methyl methacrylate MMA are successfully polymerized, and the ultraviolet absorption range of fiber FPMZn is narrower than that of polymer PMZn.
[0037] Figure 3 This is the microscopic morphology and elemental composition diagram of the bonded blue light polymer fiber in Example 1.
[0038] Figure 4 The fluorescence spectra of polymer PMZn and fiber FPMZn and their fluorescence enhancement mechanism diagrams in Example 1. As shown in Figures (b) and (c), the emission peak of fiber FPMZn is blue-shifted and the emission spectrum is broadened compared with that of polymer PMZn. The fluorescence emission spectra excited by two wavelengths show that the luminescence intensity of the fiber is greater than that of the polymer, indicating that the polymer PMZn has a significant fluorescence enhancement effect after fiberization.
[0039] Figure 5The fluorescence decay curves of polymer PMZn and fiber FPMZn at 365nm and 395nm in Example 1 are shown. It can be seen from the figure that fiberization has little effect on the fluorescence lifetime of the polymer.
[0040] Figure 6 The following is a comparison chart of the blue light anti-counterfeiting paper made of the bonded blue light polymer fiber in Example 1 under 365 nm ultraviolet light and sunlight. As can be seen from the figure, under natural light, no traces of fibers are shown on the blue light anti-counterfeiting paper, which has good concealment. In a dark environment, when irradiated with 365 nm ultraviolet light, blue fluorescent fibers appear on the blue light anti-counterfeiting paper, indicating that the prepared bonded blue light polymer fiber has good application potential in anti-counterfeiting applications. The blue light anti-counterfeiting paper has excellent anti-counterfeiting effect, and is dispersed in the anti-counterfeiting object in the form of short fibers, which greatly reduces the cost. Compared with fluorescent powder, it will not pollute the anti-counterfeiting object on a large scale, is green and environmentally friendly, and has high practical value.
[0041] The method of the invention adopts green and environmentally friendly zinc ions, and adopts a technical route of first coordination and then polymerization to prepare metal organic complexes. The raw materials are environmentally friendly and the material performance is excellent. The method of the invention belongs to the preparation process of new anti-counterfeiting materials. The blue light fiber has good luminous performance and excellent anti-counterfeiting effect, and plays an important role in the innovation and development of anti-counterfeiting technology.
[0042] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a bonded blue light polymer fiber, characterized in that: The steps include: 1) Preparation of Zn(BTZ)(UA) phosphor Weigh ZnCl2, 2-(2-hydroxyphenyl)benzothiazole, and undecylenic acid respectively, add methanol to each and stir until fully dissolved, to obtain a ZnCl2 solution, a 2-(2-hydroxyphenyl)benzothiazole solution, and an undecylenic acid solution respectively; Under water bath conditions, undecylenic acid solution was added to a three-necked flask, and then ZnCl2 solution and NaOH ethanol solution were added dropwise to react; then 2-(2-hydroxyphenyl)benzothiazole solution was added dropwise to react; after the system was uniform, NaOH solution was added dropwise until a large amount of white precipitate was produced, and the system was closed to react; The precipitate obtained by filtering and washing with methanol three times is dried to obtain the Zn(BTZ)(UA) phosphor; 2) Preparation of polymethyl methacrylate-zinc phosphor Weigh Zn(BTZ)(UA) phosphor, methyl methacrylate and azobisisobutyronitrile respectively and add them into dimethyl sulfoxide solution, and stir ultrasonically until the system is uniform; The mixed solution was transferred to a test tube with a support, and dimethyl sulfoxide solution was added. After nitrogen was passed to deoxygenate, the system was sealed and placed in a constant temperature water bath until the reaction was complete; The product was washed 6 times with methanol and dimethyl sulfoxide solvents alternately to remove impurities, and then dried to obtain the polymethyl methacrylate-zinc phosphor; 3) Preparation of bonded blue light polymer fibers The polymethyl methacrylate-zinc phosphor is dissolved in N,N-dimethylformamide to prepare a spinning solution; an electrostatic spinning method is adopted to prepare a bonded blue light polymer fiber membrane, and after drying in an oven, the bonded blue light polymer fiber is obtained.
2. The method for preparing a bonded blue light polymer fiber according to claim 1, characterized in that: In step 1), the molar ratio of ZnCl2, 2-(2-hydroxyphenyl)benzothiazole and undecylenic acid is 1:1:1, and the ratio of ZnCl2, 2-(2-hydroxyphenyl)benzothiazole, undecylenic acid to methanol is 1 mol:20 mL; the conditions for the water bath reaction are 50 ° C, 180 r / min; the ratio of ZnCl2 to NaOH ethanol solution is 1 mol:0.4 mL, and the concentration of NaOH ethanol solution is 1 mol / L; after adding ZnCl2 solution and NaOH ethanol solution, the reaction time is 30 min; after adding 2-(2-hydroxyphenyl)benzothiazole solution, the reaction time is 30 min; the closed system reaction time is 4 h; the drying temperature is 75 ° C and the time is 8 h.
3. The method for preparing a bonded blue light polymer fiber according to claim 1, characterized in that: In step 2), the mass ratio of Zn(BTZ)(UA) phosphor, methyl methacrylate and azobisisobutyronitrile is 9:150:1; the ratio of Zn(BTZ)(UA) phosphor to the first added dimethyl sulfoxide solution is 9g:350mL; the ratio of Zn(BTZ)(UA) phosphor to the second added dimethyl sulfoxide solution is 9g:150mL; the ultrasonic stirring time is 30min; the nitrogen deoxygenation time is 30min; the temperature of the constant temperature water bath is set to 75°C, the reaction time is 32h; the drying temperature is 60°C and the time is 12h.
4. The method for preparing a bonded blue light polymer fiber according to claim 1, characterized in that: In step 3), the concentration of the prepared spinning solution is 16%; the parameters of electrospinning are spinning voltage 18 kV, propulsion speed 2 mL / h, receiving distance 20 cm; the drying temperature of the oven is 65°C, and the drying time is 8 hours.