High-temperature crack monitoring sensor and preparation method thereof

The insulating layer and sensitive grid are prepared in a high-temperature environment through anodization and screen printing technology, and a high-temperature ceramic glue protective layer is used to solve the problem of difficulty in applying traditional sensors under vibration and high-temperature conditions, and achieve accurate high-temperature crack monitoring. sex and stability.

CN118746601APending Publication Date: 2024-10-08华能(浙江)能源开发有限公司长兴分公司 +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410923340.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Traditional crack monitoring sensors cannot be effectively applied under harsh working conditions such as vibration and high temperature.

Method used

The anodizing method is used to prepare the insulating layer, screen printing is used to prepare the sensitive grid, and high-temperature ceramic glue is applied to prepare the protective layer to ensure that the sensor can work normally in a high temperature environment, isolate the sensitive grid from the metal matrix, and protect the sensitive grid from environmental influences.

Benefits of technology

It realizes crack monitoring under vibration and high temperature conditions, ensures accurate measurement of sensitive gate resistance changes and the structural integrity of the sensor, and extends the service life of the sensor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118746601A_ABST
    Figure CN118746601A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature crack monitoring sensor and a preparation method thereof, and belongs to the technical field of crack detection, an insulating layer is prepared by using an anodic oxidation method, a sensitive grid is prepared by silk-screen printing, a protective layer is prepared by brushing high-temperature ceramic adhesive, and the sensor needs to be insulated from a metal matrix during normal work, so that the insulating layer needs to be prepared; the effect of isolating the sensitive grid from a metal matrix material is achieved, and it is guaranteed that the resistance change of the sensitive grid can be accurately measured; the sensitive grid plays a role in converting strain and crack information of the substrate into resistance change and transmitting the resistance change to an external circuit; the protective layer plays a role in protecting the sensor, especially the sensitive grid structure, so that the sensitive grid is prevented from being corroded, damaged, polluted and the like due to environmental influence of non-mechanical structure change.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of crack monitoring, and in particular relates to a high-temperature crack monitoring sensor and a preparation method thereof. Background Art

[0002] Crack monitoring is a common means of monitoring the health of metal structures and is widely used in aerospace, automobile, shipbuilding, military and other fields. At present, the commonly used crack monitoring methods mainly include visual detection, eddy current detection, X-ray detection, ultrasonic detection, acoustic emission detection, and potential drop method. Among them, the potential drop method has the advantages of simple equipment, easy operation, and wide applicability. Therefore, crack monitoring based on the principle of potential drop method has become a research hotspot. The potential drop method is to prepare a sensing layer on the test piece. The resistance of the sensing layer is constant. When the crack passes through different positions of the sensing layer, the resistance of the sensing layer changes, which is manifested as a change in the measured potential drop. The sensing layer is connected to a constant current source, and the potential drop between two given points of the sensing layer is measured. Since the potential drop between two given points of the sensing layer is a related function of the crack size, the length of the crack can be inferred by the potential drop. The crack monitoring sensor usually includes a metal substrate, an insulating layer, a sensitive grid and a protective layer. The existing crack monitoring sensor preparation technologies mainly include: preparing the insulating layer by anodizing; preparing the sensitive grid by magnetron sputtering or ion plating; preparing the protective layer by brushing polymer. In addition, there is also a preparation method based on screen printing technology, the main difference of which is that the sensitive grid is prepared by screen printing conductive ink.

[0003] Crack monitoring sensors based on traditional technology are limited by the preparation materials and process conditions and cannot be used under harsh working conditions such as vibration and high temperature, such as vibrating high-temperature pipes and aircraft wings. Summary of the invention

[0004] The present invention provides a high-temperature crack monitoring sensor and a preparation method thereof, which solves the problem that traditional crack monitoring sensors cannot be used under harsh working conditions such as vibration and high temperature.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing a high temperature crack monitoring sensor, comprising:

[0007] An insulating layer, a sensitive gate and a protective layer are sequentially prepared on the metal structure to be tested;

[0008] The preparation of the insulating layer specifically includes: grinding the metal structure to be tested, polishing after grinding, cleaning after polishing, and performing anodizing operation on the surface of the metal structure to be tested after cleaning to generate the insulating layer;

[0009] The preparation of the sensitive grid is specifically as follows: treating the surface of the insulating layer, selecting and treating the printing ink, drawing a pattern using the printing ink and making a screen, printing after the production is completed, performing an ink curing operation after the printing is completed, and performing a lead-in operation after the operation is completed, and arranging an artificial electrode;

[0010] The preparation of the protective layer is specifically as follows: mixing ceramic glue, and evenly coating the mixed ceramic glue on the surface of the sensitive grid.

[0011] Preferably, the metal structure to be tested is polished by selecting 100#, 400#, 800#, 1000#, and 2000# sandpaper in sequence from coarse to fine to polish the double sides of the sample.

[0012] Preferably, polishing is performed after grinding, specifically, 1.0 μm diamond polishing agent is selected, and a polishing machine is used to polish the sample, and polishing is stopped when the sandpaper marks are basically removed.

[0013] Preferably, the cleaning after polishing is specifically to use acetone, anhydrous ethanol and deionized water to ultrasonically clean the polished sample in sequence.

[0014] Preferably, the concentration of 8g / L is required to prepare the anodic oxidation solution, and ensure that the Al 3+ The concentration is lower than 5.5 g / L, the experimental temperature is 20-25°C, the power supply is selected in constant voltage mode, the DC voltage is 10-20 V, the current density is 0.4-2.5 A / dm, and the time is 30-60 min.

[0015] Preferably, the printing ink is selected and processed, specifically, a resistivity of 10 -8 ~10 -7 Ω·m, and the temperature is greater than 650℃ silver paste printed sensing circuit, using a resistivity of 10 -5 ~10 -3 Ω·m, carbon paste printed sensing resistor with temperature greater than 650℃, adding diluent to adjust viscosity to ensure that screen printing can deposit ink patterned onto the metal substrate to be tested.

[0016] Preferably, a pattern is drawn using printing ink and a screen is produced. After the production is completed, printing is performed as follows: first, a pattern is drawn using printing ink, and the drawn pattern is used to determine the printing position and the relative positions of different printed parts. Then, the printing speed, scraper angle and scraper pressure are determined according to the determined printing position and the relative positions of different printed parts, and printing is performed according to the determined printing speed, scraper angle and scraper pressure.

[0017] Preferably, the ink curing operation is performed after printing is completed, specifically, the ink is heated to evaporate the solvent in the ink, thereby achieving ink curing.

[0018] Preferably, the mixed ceramic glue is prepared by mixing white powder of ceramic glue SX-8318 and translucent liquid of ceramic glue SX-8318 in a weight ratio of 1:1.

[0019] A high temperature crack monitoring sensor is prepared based on a high temperature crack monitoring sensor preparation method, wherein a lead is connected to an external measurement system.

[0020] Compared with the prior art, the present invention has the following beneficial effects: the present invention provides a method for preparing a high-temperature crack monitoring sensor, which uses anodizing to prepare an insulating layer, screen printing to prepare a sensitive grid, and brushing high-temperature ceramic glue to prepare a protective layer. The sensor needs to be insulated from the metal substrate for normal operation, so it is necessary to prepare an insulating layer to isolate the sensitive grid from the metal substrate material and ensure that the resistance change of the sensitive grid can be accurately measured; the sensitive grid converts the strain and crack information of the substrate into resistance changes and transmits it to an external circuit; the protective layer protects the sensor, especially the sensitive grid structure, to prevent the sensitive grid from being corroded, damaged, polluted, etc. by environmental influences of non-mechanical structural changes. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a schematic diagram of the structure of a high temperature crack monitoring sensor of the present invention;

[0022] Figure 2 This is the working principle of a high temperature crack monitoring sensor of the present invention;

[0023] Figure 3 A sensitive grid structure of a high temperature crack monitoring sensor of the present invention;

[0024] Figure 4 The present invention is a process for preparing a screen-printed sensitive grid;

[0025] Figure 5 The screen printing screen pattern of the present invention;

[0026] Figure 6 It is a schematic diagram of the screen printing principle of the present invention. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0028] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0030] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.

[0031] In addition, if the term "horizontal" appears, it does not mean that the component must be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.

[0032] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.

[0034] The present invention provides a method for preparing a high temperature crack monitoring sensor, comprising:

[0035] An insulating layer, a sensitive gate and a protective layer are sequentially prepared on the metal structure to be tested;

[0036] The preparation of the insulating layer specifically includes: grinding the metal structure to be tested, polishing after grinding, cleaning after polishing, and performing anodizing operation on the surface of the metal structure to be tested after cleaning to generate the insulating layer;

[0037] The preparation of the sensitive grid is specifically as follows: treating the surface of the insulating layer, selecting and treating the printing ink, drawing a pattern using the printing ink and making a screen, printing after the production is completed, performing an ink curing operation after the printing is completed, and performing a lead-in operation after the operation is completed, and arranging an artificial electrode;

[0038] The preparation of the protective layer is specifically as follows: mixing ceramic glue, and evenly coating the mixed ceramic glue on the surface of the sensitive grid.

[0039] The detailed preparation steps are as follows:

[0040] (1) Preparation of insulation layer:

[0041] The insulating layer in this technical solution is prepared by anodizing, and the preparation process includes two major steps: surface pretreatment and anodizing. Taking aluminum alloy metal structure as an example, pollutants such as grease and naturally formed oxide film on the base material will hinder the formation of oxide film during anodizing, and will cause problems such as uneven oxide film or even damage after film formation. Therefore, the surface of the material must be pretreated before officially starting anodizing treatment of the base material to be tested. The specific steps of the insulating layer preparation are as follows: sandpaper polishing → mechanical polishing → cleaning → anodizing.

[0042] 1) Sandpaper polishing: In the experiment, 100#, 400#, 800#, 1000#, and 2000# sandpapers were used in sequence from coarse to fine to polish the double-sided surfaces of the specimens.

[0043] 2) Mechanical polishing: Use 1.0 μm diamond polishing agent and polish the sample using a polishing machine. Stop polishing when the sandpaper marks are basically removed and quickly enter the cleaning step.

[0044] 3) Cleaning: Use acetone, anhydrous ethanol and deionized water to ultrasonically clean the polished samples in turn to wash away organic matter on the surface of the substrate, particles generated by grinding and polishing, etc.

[0045] 4) Anodizing: Prepare the anodizing solution according to the concentration requirements of 40g / L 98% concentrated sulfuric acid and 8g / L boric acid, and ensure that the Al content in the solution is 3+ The concentration is lower than 5.5g / L, and the experimental temperature is 20℃~25℃. The power supply is selected in constant voltage mode, with a DC voltage of 10~20V, a current density of 0.4~2.5A / dm, and a time of 30~60min.

[0046] (2) Sensitive gate preparation

[0047] The preparation process of screen-printed sensitive gate is mainly divided into five steps, namely, surface treatment of insulating layer, selection and treatment of functional ink, screen printing preparation, functional ink curing and lead. Figure 4 shown.

[0048] 1) Surface treatment of the insulating layer: Use acetone, anhydrous ethanol and deionized water to ultrasonically clean the metal structure to be tested after anodization to remove stains, dust, etc. on the surface, so that the ink adhesion on the surface of the structure is improved, thereby ensuring the printing quality of the sensitive grid.

[0049] 2) Functional ink selection and processing: Select resistivity 10 -8 ~10 -7 Ω·m, the temperature is greater than 650℃ silver paste printed sensor circuit, use resistivity 10 -5 ~10 -3 Ω·m, carbon paste printed sensing resistor at a temperature greater than 650°C. Add diluent to adjust the viscosity to ensure that screen printing can deposit the ink pattern onto the metal substrate to be tested to form a sensitive grid.

[0050] 3) Screen printing preparation: Since the sensitive gate structure is divided into two parts, the sensing circuit and the sensing resistor, the screen printing is also carried out in two steps. The screen pattern is as follows: Figure 5 The horizontal lines above the pattern are positioning parallel lines, which are used to determine the printing position of the entire sensitive grid on the substrate, as well as the relative positions of different printed parts in the sensitive grid. Figure 6 As shown, the key process parameters include: printing speed, squeegee angle, and squeegee pressure.

[0051] 4) Functional ink curing: Functional ink curing mainly uses high temperature to evaporate the solvent in the slurry, solidify the resin, and bond the conductive particles to each other.

[0052] 5) Lead wire: Artificially apply some high-temperature platinum paste and adhere platinum wire to perform lead wire operation. In order to protect the lead wire from falling off, use high-temperature ceramic glue to encapsulate the lead wire pad.

[0053] (3) Preparation of protective layer

[0054] Use high-temperature ceramic glue to coat the sensor surface to prepare a protective layer. Before coating, mix ceramic glue SX-8318 (component A, white powder) and ceramic glue SX-8318 (component B, translucent liquid) in proportion, stir evenly, and use a fine brush to coat the high-temperature ceramic glue on the sample surface where the sensitive grid is prepared.

[0055] Embodiment 1:

[0056] The present invention provides a method for preparing a high temperature crack monitoring sensor, comprising:

[0057] An insulating layer, a sensitive gate and a protective layer are sequentially prepared on the metal structure to be tested;

[0058] (1) Preparation of insulation layer:

[0059] The insulating layer in this technical solution is prepared by anodizing, and the preparation process includes two major steps: surface pretreatment and anodizing. Taking aluminum alloy metal structure as an example, pollutants such as grease and naturally formed oxide film on the base material will hinder the formation of oxide film during anodizing, and will cause problems such as uneven oxide film or even damage after film formation. Therefore, the surface of the material must be pretreated before officially starting anodizing treatment of the base material to be tested. The specific steps of the insulating layer preparation are as follows: sandpaper polishing → mechanical polishing → cleaning → anodizing.

[0060] 1) Sandpaper polishing: In the experiment, 100#, 400#, 800#, 1000#, and 2000# sandpapers were used in sequence from coarse to fine to polish the double-sided surfaces of the specimens.

[0061] 2) Mechanical polishing: Use 1.0 μm diamond polishing agent and polish the sample using a polishing machine. Stop polishing when the sandpaper marks are basically removed and quickly enter the cleaning step.

[0062] 3) Cleaning: Use acetone, anhydrous ethanol and deionized water to ultrasonically clean the polished samples in turn to wash away organic matter on the surface of the substrate, particles generated by grinding and polishing, etc.

[0063] 4) Anodizing: Prepare the anodizing solution according to the concentration requirements of 40g / L 98% concentrated sulfuric acid and 8g / L boric acid, and ensure that the Al content in the solution is 3+ The concentration was lower than 5.5 g / L, and the experimental temperature was 20°C. The power supply was selected in constant voltage mode, with a DC voltage of 10 V, a current density of 0.4 A / dm, and a time of 30 min.

[0064] (2) Sensitive gate preparation

[0065] The preparation process of screen-printed sensitive gate is mainly divided into five steps, namely, surface treatment of insulating layer, selection and treatment of functional ink, screen printing preparation, functional ink curing and lead. Figure 4 shown.

[0066] 1) Surface treatment of the insulating layer: Use acetone, anhydrous ethanol and deionized water to ultrasonically clean the metal structure to be tested after anodization to remove stains, dust, etc. on the surface, so that the ink adhesion on the surface of the structure is improved, thereby ensuring the printing quality of the sensitive grid.

[0067] 2) Functional ink selection and processing: Select resistivity 10 -8Ω·m, the temperature is greater than 650℃ silver paste printed sensor circuit, use resistivity 10 -5 Ω·m, carbon paste printed sensing resistor at a temperature greater than 650°C. Add diluent to adjust the viscosity to ensure that screen printing can deposit the ink pattern onto the metal substrate to be tested to form a sensitive grid.

[0068] 3) Screen printing preparation: Since the sensitive gate structure is divided into two parts, the sensing circuit and the sensing resistor, the screen printing is also carried out in two steps. The screen pattern is as follows: Figure 5 The horizontal lines above the pattern are positioning parallel lines, which are used to determine the printing position of the entire sensitive grid on the substrate, as well as the relative positions of different printed parts in the sensitive grid. Figure 6 As shown, the key process parameters include: printing speed, squeegee angle, and squeegee pressure.

[0069] 4) Functional ink curing: Functional ink curing mainly uses high temperature to evaporate the solvent in the slurry, solidify the resin, and bond the conductive particles to each other.

[0070] 5) Lead wire: Artificially apply some high-temperature platinum paste and adhere platinum wire to perform lead wire operation. In order to protect the lead wire from falling off, use high-temperature ceramic glue to encapsulate the lead wire pad.

[0071] (3) Preparation of protective layer

[0072] Use high-temperature ceramic glue to coat the sensor surface to prepare a protective layer. Before coating, mix ceramic glue SX-8318 (component A, white powder) and ceramic glue SX-8318 (component B, translucent liquid) in proportion, stir evenly, and use a fine brush to coat the high-temperature ceramic glue on the sample surface where the sensitive grid is prepared.

[0073] Embodiment 2:

[0074] The present invention provides a method for preparing a high temperature crack monitoring sensor, comprising:

[0075] An insulating layer, a sensitive gate and a protective layer are sequentially prepared on the metal structure to be tested;

[0076] (1) Preparation of insulation layer:

[0077] The insulating layer in this technical solution is prepared by anodizing, and the preparation process includes two major steps: surface pretreatment and anodizing. Taking aluminum alloy metal structure as an example, pollutants such as grease and naturally formed oxide film on the base material will hinder the formation of oxide film during anodizing, and will cause problems such as uneven oxide film or even damage after film formation. Therefore, the surface of the material must be pretreated before officially starting anodizing treatment of the base material to be tested. The specific steps of the insulating layer preparation are as follows: sandpaper polishing → mechanical polishing → cleaning → anodizing.

[0078] 1) Sandpaper polishing: In the experiment, 100#, 400#, 800#, 1000#, and 2000# sandpapers were used in sequence from coarse to fine to polish the double-sided surfaces of the specimens.

[0079] 2) Mechanical polishing: Use 1.0 μm diamond polishing agent and polish the sample using a polishing machine. Stop polishing when the sandpaper marks are basically removed and quickly enter the cleaning step.

[0080] 3) Cleaning: Use acetone, anhydrous ethanol and deionized water to ultrasonically clean the polished samples in turn to wash away organic matter on the surface of the substrate, particles generated by grinding and polishing, etc.

[0081] 4) Anodizing: Prepare the anodizing solution according to the concentration requirements of 40g / L 98% concentrated sulfuric acid and 8g / L boric acid, and ensure that the Al content in the solution is 3+ The concentration was lower than 5.5 g / L, and the experimental temperature was 23°C. The power supply was set to constant voltage mode, with a DC voltage of 14 V, a current density of 1.3 A / dm, and a time of 42 min.

[0082] (2) Sensitive gate preparation

[0083] The preparation process of screen-printed sensitive gate is mainly divided into five steps, namely, surface treatment of insulating layer, selection and treatment of functional ink, screen printing preparation, functional ink curing and lead. Figure 4 shown.

[0084] 1) Surface treatment of the insulating layer: Use acetone, anhydrous ethanol and deionized water to ultrasonically clean the metal structure to be tested after anodization to remove stains, dust, etc. on the surface, so that the ink adhesion on the surface of the structure is improved, thereby ensuring the printing quality of the sensitive grid.

[0085] 2) Functional ink selection and processing: Select resistivity 10 -7 Ω·m, the temperature is greater than 650℃ silver paste printed sensor circuit, use resistivity 10 -3 Ω·m, carbon paste printed sensing resistor at a temperature greater than 650°C. Add diluent to adjust the viscosity to ensure that screen printing can deposit the ink pattern onto the metal substrate to be tested to form a sensitive grid.

[0086] The viscosity is adjusted by adding diluent to ensure that the screen printing can deposit the ink pattern onto the metal substrate to be tested to form a sensitive grid.

[0087] 3) Screen printing preparation: Since the sensitive gate structure is divided into two parts, the sensing circuit and the sensing resistor, the screen printing is also carried out in two steps. The screen pattern is as follows: Figure 5The horizontal lines above the pattern are positioning parallel lines, which are used to determine the printing position of the entire sensitive grid on the substrate, as well as the relative positions of different printed parts in the sensitive grid. Figure 6 As shown, the key process parameters include: printing speed, squeegee angle, and squeegee pressure.

[0088] 4) Functional ink curing: Functional ink curing mainly uses high temperature to evaporate the solvent in the slurry, solidify the resin, and bond the conductive particles to each other.

[0089] 5) Lead wire: Artificially apply some high-temperature platinum paste and adhere platinum wire to perform lead wire operation. In order to protect the lead wire from falling off, use high-temperature ceramic glue to encapsulate the lead wire pad.

[0090] (3) Preparation of protective layer

[0091] Use high-temperature ceramic glue to coat the sensor surface to prepare a protective layer. Before coating, mix ceramic glue SX-8318 (component A, white powder) and ceramic glue SX-8318 (component B, translucent liquid) in proportion, stir evenly, and use a fine brush to coat the high-temperature ceramic glue on the sample surface where the sensitive grid is prepared.

[0092] Embodiment 3:

[0093] The present invention provides a method for preparing a high temperature crack monitoring sensor, comprising:

[0094] An insulating layer, a sensitive gate and a protective layer are sequentially prepared on the metal structure to be tested;

[0095] (1) Preparation of insulation layer:

[0096] The insulating layer in this technical solution is prepared by anodizing, and the preparation process includes two major steps: surface pretreatment and anodizing. Taking aluminum alloy metal structure as an example, pollutants such as grease and naturally formed oxide film on the base material will hinder the formation of oxide film during anodizing, and will cause problems such as uneven oxide film or even damage after film formation. Therefore, the surface of the material must be pretreated before officially starting anodizing treatment of the base material to be tested. The specific steps of the insulating layer preparation are as follows: sandpaper polishing → mechanical polishing → cleaning → anodizing.

[0097] 1) Sandpaper polishing: In the experiment, 100#, 400#, 800#, 1000#, and 2000# sandpapers were used in sequence from coarse to fine to polish the double-sided surfaces of the specimens.

[0098] 2) Mechanical polishing: Use 1.0 μm diamond polishing agent and polish the sample using a polishing machine. Stop polishing when the sandpaper marks are basically removed and quickly enter the cleaning step.

[0099] 3) Cleaning: Use acetone, anhydrous ethanol and deionized water to ultrasonically clean the polished samples in turn to wash away organic matter on the surface of the substrate, particles generated by grinding and polishing, etc.

[0100] 4) Anodizing: Prepare the anodizing solution according to the concentration requirements of 40g / L 98% concentrated sulfuric acid and 8g / L boric acid, and ensure that the Al content in the solution is 3+ The concentration was lower than 5.5 g / L, and the experimental temperature was 25°C. The power supply was set to constant voltage mode, with a DC voltage of 20 V, a current density of 0.25 A / dm, and a time of 60 min.

[0101] (2) Sensitive gate preparation

[0102] The preparation process of screen-printed sensitive gate is mainly divided into five steps, namely, surface treatment of insulating layer, selection and treatment of functional ink, screen printing preparation, functional ink curing and lead. Figure 4 shown.

[0103] 1) Surface treatment of the insulating layer: Use acetone, anhydrous ethanol and deionized water to ultrasonically clean the metal structure to be tested after anodization to remove stains, dust, etc. on the surface, so that the ink adhesion on the surface of the structure is improved, thereby ensuring the printing quality of the sensitive grid.

[0104] 2) Functional ink selection and processing: Select resistivity 10 -8 Ω·m, the temperature is greater than 650℃ silver paste printed sensor circuit, use resistivity 10 -4 Ω·m, carbon paste printed sensing resistor at a temperature greater than 650°C. Add diluent to adjust the viscosity to ensure that screen printing can deposit the ink pattern onto the metal substrate to be tested to form a sensitive grid.

[0105] 3) Screen printing preparation: Since the sensitive gate structure is divided into two parts, the sensing circuit and the sensing resistor, the screen printing is also carried out in two steps. The screen pattern is as follows: Figure 5 The horizontal lines above the pattern are positioning parallel lines, which are used to determine the printing position of the entire sensitive grid on the substrate, as well as the relative positions of different printed parts in the sensitive grid. Figure 6 As shown, the key process parameters include: printing speed, squeegee angle, and squeegee pressure.

[0106] 4) Functional ink curing: Functional ink curing mainly uses high temperature to evaporate the solvent in the slurry, solidify the resin, and bond the conductive particles to each other.

[0107] 5) Lead wire: Artificially apply some high-temperature platinum paste and adhere platinum wire to perform lead wire operation. In order to protect the lead wire from falling off, use high-temperature ceramic glue to encapsulate the lead wire pad.

[0108] (3) Preparation of protective layer

[0109] Use high-temperature ceramic glue to coat the sensor surface to prepare a protective layer. Before coating, mix ceramic glue SX-8318 (component A) and ceramic glue SX-8318 (component B) in proportion, stir evenly, and use a fine brush to coat the high-temperature ceramic glue on the sample surface where the sensitive grid is prepared.

[0110] Based on the above method, the present invention also provides a high-temperature crack monitoring sensor, which is developed to be highly integrated with the metal structure, does not affect the structural integrity and can be used under harsh working conditions such as vibration and high temperature.

[0111] The sensor is mainly composed of three parts: insulating layer, sensitive grid and protective layer. The sensor structure model is as follows: Figure 1 As shown. Since the sensor is directly generated on the metal substrate, the sensor needs to be insulated from the metal substrate for normal operation, so an insulating layer needs to be prepared to isolate the sensitive gate from the metal substrate material to ensure that the resistance change of the sensitive gate can be accurately measured; the sensitive gate plays a role in converting the strain and crack information of the substrate into resistance changes and transmitting them to the external circuit; the protective layer plays a role in protecting the sensor, especially the sensitive gate structure, to prevent the sensitive gate from being corroded, damaged, and contaminated by environmental influences such as non-mechanical structural changes. In addition to the three major components, the crack monitoring sensor also includes leads to connect to the external measurement system. In the crack monitoring sensor, the matrix material, as part of the measured structure, plays the role of providing a manufacturing plane for the sensor and inputting the measured strain, crack and other information. The leads connect the sensitive gate to the measurement circuit and output the electrical signal of the sensor to the external circuit of the measurement system.

[0112] The monitoring of metal structures by crack monitoring sensors mainly depends on the damage consistency between the crack monitoring sensors and the substrate structure. Figure 2 As shown in the figure, when fatigue damage occurs to the substrate structure, cracks also appear in the sensitive gate sensing layer that is closely bonded to the substrate at the same location. The cracks on the sensor continue to expand along with the substrate cracks, causing changes in the sensor resistance, which is manifested as changes in the sensor output voltage. Therefore, by monitoring and analyzing the changes in the sensor output voltage, the crack damage of the substrate structure can be reflected.

[0113] The sensitive gate determines the output characteristics of the sensor. Figure 3As shown, the sensitive grid has a parallel circuit configuration and is divided into two parts: the sensing circuit and the sensing resistor. During the test, the sensitive grid is perpendicular to the principal strain direction of the metal structure to be tested. When a crack is generated in the substrate to be tested and expands, the corresponding branch of the sensitive grid will be broken, and its overall resistance will then undergo a large step change. When tested with a constant current source, it will be manifested as a change in the output voltage. Since the resistance of the sensing resistors in series in each branch is different, the voltage change is also different when the branch is broken. The correlation curve between the sensor output voltage and the crack length of the substrate to be tested is drawn. With this as a reference, the crack length information can be inferred. Adjusting the number of branches and the branch length L can control the monitoring range, and adjusting the branch spacing S and width W can control the crack monitoring accuracy. The scheme is simple in design and easy to prepare, and only uses one constant current source, so the test equipment is simple and the cost is low.

[0114] Considering that the crack monitoring sensor developed is used in harsh working conditions such as high temperature and vibration, and in order to minimize the impact of sensor installation on the safe operation of the structure, this technical solution directly prepares the sensor on the metal structure to be tested. The main processes include: preparing the insulating layer by anodizing, preparing the sensitive grid by screen printing, and preparing the protective layer by brushing high-temperature ceramic glue. This technology has the advantages of fast preparation, strong adaptability of the substrate structure, and large-area preparation. Taking the common aluminum alloy metal structure as an example, a dense Al2O3 insulating layer will be generated on the surface of the aluminum alloy structure through anodizing. The maximum usable temperature of Al2O3 is 1200℃, and it can still maintain good mechanical strength and thermal stability in high temperature environment. In addition, high-temperature silver paste with low resistivity and high-temperature carbon paste with high resistivity are used to print the sensor circuit and sensor resistor respectively, ultimately ensuring that the crack monitoring sensor developed can be applied to high-temperature working conditions.

[0115] Although the embodiments of the present invention are described above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific embodiments and application fields, and the above-mentioned specific embodiments are only illustrative and instructive, rather than restrictive. Under the guidance of the specification, a person skilled in the art can also make many forms without departing from the scope of protection of the claims of the present invention, all of which belong to the scope of protection of the present invention.

Claims

1. A method for preparing a high temperature crack monitoring sensor, It is characterized in that include: An insulating layer, a sensitive gate and a protective layer are sequentially prepared on the metal structure to be tested; The preparation of the insulating layer specifically includes: grinding the metal structure to be tested, polishing after grinding, cleaning after polishing, and performing anodizing operation on the surface of the metal structure to be tested after cleaning to generate the insulating layer; The preparation of the sensitive grid is specifically as follows: treating the surface of the insulating layer, selecting and treating the printing ink, drawing a pattern using the printing ink and making a screen, printing after the production is completed, performing an ink curing operation after the printing is completed, and performing a lead-in operation after the operation is completed, and arranging an artificial electrode; The preparation of the protective layer is specifically as follows: mixing ceramic glue, and evenly coating the mixed ceramic glue on the surface of the sensitive grid.

2. A method for preparing a high temperature crack monitoring sensor according to claim 1, It is characterized in that Specifically, the metal structure to be tested is polished by selecting 100#, 400#, 800#, 1000#, and 2000# sandpaper in sequence from coarse to fine to polish the double-sided surface of the sample.

3. A method for preparing a high temperature crack monitoring sensor according to claim 1, It is characterized in that Polishing is performed after grinding. Specifically, 1.0 μm diamond polishing agent is selected and the sample is polished using a polishing machine. Polishing is stopped when the sandpaper marks are basically removed.

4. A method for preparing a high temperature crack monitoring sensor according to claim 1, It is characterized in that The cleaning after polishing is specifically to use acetone, anhydrous ethanol and deionized water to ultrasonically clean the polished sample in sequence.

5. A method for preparing a high temperature crack monitoring sensor according to claim 1, It is characterized in that The specific steps of anodizing the surface of the metal structure to be tested are as follows: prepare anodizing solution according to the concentration requirements of 40 g / L 98% concentrated sulfuric acid and 8 g / L boric acid, and ensure that Al in the solution is 3+ The concentration is lower than 5.5 g / L, the experimental temperature is 20-25°C, the power supply is selected in constant voltage mode, the DC voltage is 10-20 V, the current density is 0.4-2.5 A / dm, and the time is 30-60 min.

6. A method for preparing a high temperature crack monitoring sensor according to claim 1, It is characterized in that Select printing ink and process it. Specifically, select a resistivity of 10 -8 ~10 -7 Ω·m, and the temperature is greater than 650℃ silver paste printed sensing circuit, using a resistivity of 10 -5 ~10 -3 Ω·m, carbon paste printed sensing resistor with temperature greater than 650℃, adding diluent to adjust viscosity to ensure that screen printing can deposit ink patterned onto the metal substrate to be tested.

7. A method for preparing a high temperature crack monitoring sensor according to claim 1, It is characterized in that Use printing ink to draw a pattern and make a screen. After the production is completed, printing is carried out. Specifically, first use printing ink to draw a pattern, use the drawn pattern to determine the printing position and the relative positions of different printing parts, then determine the printing speed, scraper angle and scraper pressure according to the determined printing position and the relative positions of different printing parts, and print according to the determined printing speed, scraper angle and scraper pressure.

8. A method for preparing a high temperature crack monitoring sensor according to claim 1, It is characterized in that After printing, the ink curing operation is performed by heating the ink to evaporate the solvent in the ink to achieve ink curing.

9. A method for preparing a high temperature crack monitoring sensor according to claim 1, It is characterized in that Specifically, the mixed ceramic glue is prepared by mixing the white powder of ceramic glue SX-8318 and the translucent liquid of ceramic glue SX-8318 in a weight ratio of 1:

1.

10. A high temperature crack monitoring sensor, It is characterized in that A high-temperature crack monitoring sensor is prepared based on the preparation method of any one of claims 1-9, wherein the lead is connected to an external measurement system.

Citation Information

Cited By

  • High-temperature co-sintered multilayer special-shaped ceramic high-temperature sensor and preparation method thereof

    CN120213091A