Preparation method of hybrid insulator

By introducing mud inspection and structural inspection steps in insulator production, screening and repairing unqualified porcelain insulators, the problem of low hybrid insulator yield and production efficiency is solved, and efficient hybrid insulator preparation is achieved.

CN118748110AActive Publication Date: 2024-10-08GUANGDONG POWER GRID CO LTD +1

Patent Information

Application Number
CN202410905055.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-08
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

Existing insulator production technology cannot meet the accuracy requirements of high-temperature vulcanized silicone rubber coating on the surface of hybrid insulators, resulting in low yield and production efficiency. When production capacity is tight, porcelain insulators need to be re-produced, causing economic losses.

Method used

Adopt the mud blank inspection and structure inspection steps, through weight measurement and shed structure inspection, screen out the mud blanks that meet the standards and repair the unqualified porcelain insulators to ensure that they meet the accuracy requirements of the coating mold, improve the yield and production efficiency.

Benefits of technology

It improves the yield and production efficiency of hybrid insulators, reduces losses during the production process, and ensures the consistency and accuracy of product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748110A_ABST
    Figure CN118748110A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a hybrid insulator, and belongs to the technical field of insulators. In the preparation process of the mixed insulator, firstly, the mud blank meeting the production standard is screened out through mud blank detection, secondly, the produced porcelain insulators are classified through the umbrella skirt detection plate comprising the marking device according to the requirement of a mixed insulator coating mold, and then the mixed insulator coating mold is obtained. And the marking area of the surface of the umbrella skirt structure of the porcelain insulator is repaired to be less than or equal to 10%, so that the requirement of a coating mold is met, the yield of the mixed insulator is ensured, the production efficiency of the mixed insulator is improved, and the loss in the production process of the mixed insulator is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of insulators, and in particular to a method for preparing a hybrid insulator. Background Art

[0002] The new hybrid insulator for transmission lines is a new type of insulator that uses a high-temperature injection process to coat a layer of high-temperature vulcanized silicone rubber (HTV) on a traditional porcelain insulator or glass insulator. It has the advantages of long life and high mechanical strength of traditional porcelain insulators or glass insulators and pollution flashover resistance of HTV composite insulators. It has broad application prospects in heavily polluted areas in my country.

[0003] The coating of the new hybrid insulator adopts the three-dimensional measurement method of insulation parts based on structured light scanning and precise alignment to model and make the coating mold. Since the porcelain insulator or glass insulator structure in the core body has a complete umbrella skirt and the thickness of the coated HTV is about 3mm, the process has very high requirements on the structural accuracy of the mold, porcelain insulator and glass insulator.

[0004] In order to improve the consistency of the structure of mass-produced porcelain insulators or glass insulators, patent CN113921208B proposed a fully automated production line for ceramic suspension insulators, and set up two types of embryo repair mechanisms, rough repair and fine repair, in the production process of porcelain insulators, which improved the consistency of porcelain insulator products; although the existing insulator production technology adopts automated molding, the entire production process from mud making, molding, glazing and sanding, drying and firing, and gluing is basically mechanized, standardized, and automated, which improves the stability and consistency of product quality. However, for hybrid insulators, the existing production technology still cannot fully meet the precision requirements of surface HTV coating. For example, under the condition of tight production capacity, some of the produced porcelain insulator structures do not meet the precision requirements of the coating mold (such as the umbrella skirt diameter exceeds the 2mm required by the coating mold), resulting in the need to re-produce porcelain insulators, delaying the construction period and causing huge economic losses. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a method for preparing a hybrid insulator. The method can improve the yield and production efficiency of the hybrid insulator and reduce the loss in the production process of the hybrid insulator.

[0006] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a hybrid insulator, comprising the following steps: mud blank detection and structure detection;

[0007] The clay blank detection step includes: placing the clay blank on a weight measuring device for weighing, obtaining the weight measurement result of the clay blank to be tested, comparing the weight measurement results, and the qualified products proceed to the next step;

[0008] The structural detection step is: using a shed structure detection device to detect the shed structure of the fired porcelain insulator, the shed detection device includes a shed detection plate, the shed detection plate includes a detection surface matching the shed structure of the porcelain insulator, and the detection surface is provided with a marking device to obtain the marking result of the surface of the porcelain insulator to be tested; taking the surface area of ​​the shed structure of the porcelain insulator as 100%, if the marked area of ​​the surface of the shed structure of the porcelain insulator is 0, then proceed to the next step; if the marked area of ​​the surface of the shed structure of the porcelain insulator is ≤10%, then repair the marked area of ​​the porcelain insulator until the marked area of ​​the surface of the shed structure of the porcelain insulator is 0; if the marked area of ​​the surface of the shed structure of the porcelain insulator is >10%, it is marked as unqualified.

[0009] In some embodiments, a gap is provided between the detection surface and the shed structure of the porcelain insulator.

[0010] In some embodiments, the umbrella skirt detection board includes a first detection board, a second detection board and a third detection board, wherein the third detection board is connected to the first detection board and the second detection board respectively.

[0011] In some embodiments, the shed detection board further includes a driving device, and the driving device is connected to the first detection board.

[0012] In some embodiments, the shed structure detection device further includes a base, and the base is used to fix the porcelain insulator.

[0013] In some embodiments, the marking means is a color marking means.

[0014] In some embodiments, the weight measurement results are compared by weight comparison or weight percentage deviation comparison.

[0015] In some embodiments, the weight measurement comparison is performed in measurement software.

[0016] In some embodiments, the method for preparing the hybrid insulator further includes the following steps: kneading clay, molding, trimming, drying, glazing, firing, and vulcanization coating.

[0017] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention adds a clay blank detection step and a structure detection step to the prior art of preparing hybrid insulators. First, the clay blanks that meet the production standards are screened out through the clay blank detection. Secondly, the produced porcelain insulators are classified according to the requirements of the hybrid insulator coating mold through the shed detection plate including the marking device, and the marking area ≤10% of the surface of the shed structure of the porcelain insulator is repaired to meet the requirements of the coating mold. While ensuring the yield of the hybrid insulators, the production efficiency of the hybrid insulators is improved and the loss in the production process of the hybrid insulators is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A process flow chart for preparing hybrid insulators for the present disclosure;

[0019] Figure 2 This is a flow chart of the porcelain insulator structure detection disclosed in the present invention; wherein, 3-1, porcelain insulator head; 3-2, upper umbrella shape; 3-3, lower umbrella shape; 5, base; 6-1, upper plate; 6-2, lower plate; 6-3, middle plate; 7, drive shaft;

[0020] Figure 3 A classification diagram of the results of the structural inspection of the porcelain insulator disclosed in the present invention;

[0021] Figure 4 It is a schematic diagram of the structure of a double umbrella-shaped porcelain insulator; 1, steel cap; 2-1 and 2-2, adhesive; 3-1, porcelain insulator head; 3-2, upper umbrella; 3-3, lower umbrella; 4, steel foot. DETAILED DESCRIPTION

[0022] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.

[0023] In the description of the present disclosure, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present disclosure.

[0024] In the description of the present disclosure, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection or a detachable connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to specific circumstances.

[0025] The invention aims to solve the problems of low yield rate and production efficiency of hybrid insulators in the production process of hybrid insulators in the prior art.

[0026] Based on the existing technology of preparing hybrid insulators, the present invention adds mud blank detection and structure detection steps, such as Figure 1 As shown, the present disclosure provides a method for preparing a hybrid insulator, comprising the following steps:

[0027] S1: Material preparation: weigh the required raw materials according to the requirements of porcelain insulators;

[0028] S2: Vacuum mud kneading: Use vacuum mud kneading machine to knead the raw materials into mud segments and output;

[0029] The function of vacuum clay kneading is to eliminate the minimum gas content in the clay, eliminate the air, knead and extrude the clay, improve the plasticity, density and uniformity of the clay, thereby improving the plasticity and strength of the clay blank; in addition, it can also destroy the directional arrangement of the clay, improve the qualified rate of the clay blank, and thus improve the finished product rate of porcelain insulators.

[0030] Specifically, before the vacuum mud kneading step, those skilled in the art may perform at least one of the following steps according to actual needs: mixing, screening, iron removal, mud pressing and aging;

[0031] Screening the mixed slurry can control the fineness of the blank and keep the slurry uniform, remove harmful impurities, further purify the slurry, and remove coarse particles, hard mud blocks, sawdust, cotton cloth, oil residue and other residues; it is conducive to molding and firing, and improves the strength of porcelain insulators;

[0032] The purpose of iron removal is to remove iron spots from products and improve product purity and electromechanical properties; iron removal and screening are complementary process operations and are one of the methods for purifying sludge;

[0033] Mud squeezing is to remove the water from the mud. The mud can be used for plastic molding only after dehydration.

[0034] Aging is the process of sending the squeezed and dehydrated mud cake into a closed room of appropriate size (i.e. mud storage) and storing it for one to two weeks; this is used to improve the plasticity and formability of the mud, make the moisture in the mud cake uniform, and improve the electromechanical properties of the green body.

[0035] S3: Molding, air-drying, and trimming: the clay after vacuum kneading is molded according to the product size requirements to obtain a porcelain insulator blank; the porcelain insulator blank is naturally air-dried until the surface of the porcelain body turns white, and then trimmed to meet the product's precision requirements.

[0036] S4: Clay blank inspection: Place the clay blank on a weight measuring device for weighing, obtain the weight measurement result of the clay blank to be tested, compare the weight measurement results, and the qualified products proceed to the next step;

[0037] Specifically, the present disclosure can measure the weight of the unfired clay billets through a weight measuring device, and screen out the unfired clay billets with unqualified weights through an identification device. The unqualified unfired clay billets can be used as raw materials for other standard parts, or can be transported to the stock preparation step through a cleaning device for reuse, so as to improve the yield rate of porcelain insulators and reduce the production cost of porcelain insulators.

[0038] The weight of the unfired clay billets can be evaluated whether it meets the standard by the weight value or the weight percentage change rate. The weight standards of porcelain insulators with different standards are different. Those skilled in the art can, according to the actual situation, design different weight values or weight percentage change rates that meet the standards to evaluate the qualification rate of porcelain insulators.

[0039] Taking the standard weight of the unfired clay billets as 10 kg, according to calculations, when the weight deviation of the unfired clay billets is within the range of ±0.5 kg or the weight percentage change rate is ±5%, the unfired clay billets meet the requirements. Therefore, a weight sensing device can be installed on the robotic arm for transferring the unfired clay billets, and the designed weight values are 10 kg and 10.5 kg. When the weight m ≤ 10.0 kg, the robotic arm transfers the unfired clay billets to the Class A partition, recorded as excellent products. When the weight 10.0 kg < m ≤ 10.5 kg, the robotic arm transfers the unfired clay billets to the Class B partition, recorded as qualified products. When the weight m > 10.5 kg, the robotic arm transfers the unfired clay billets to the Class C partition. Assuming that the unfired clay billets in the Class C partition meet the requirements of porcelain insulators with other standards, they can be used as raw materials for porcelain insulators with other standards and enter the next process of preparing porcelain insulators with other standards; assuming that the unfired clay billets in the Class C partition do not meet the requirements of porcelain insulators with other standards, or there is no production demand for porcelain insulators with other standards, the unfired clay billets in the Class C partition return to the stock preparation step and are used as raw materials to produce porcelain insulators again; the unfired clay billets in the Class A partition and the Class B partition directly proceed to the next step.

[0040] S5: Drying, glazing and firing: The qualified unfired clay billets measured by the weight measuring device are dried. The drying method is not particularly limited, as long as the green body can be dried to a moisture content of less than 0.05%. The drying method can be drying by baking or microwave drying.

[0041] The glazing method is not specifically limited. Those skilled in the art can select a suitable method for glazing according to actual needs. For example, it can be dip coating or spraying.

[0042] Before firing after glazing, there is also a sanding step. The above purpose is to lay a foundation for cementing to increase the stability and firmness of the cementing accessories. The sand can be obtained by drying, crushing and screening the waste materials from坯 body making, and its components are the same as those of the坯 body material.

[0043] The firing temperature, time and number of firings are not specifically limited. Those skilled in the art can select suitable firing temperature, firing time and number of firings according to actual needs.

[0044] For example, the firing is carried out in stages, including a preheating period, an oxidation period, a reduction period, a heat preservation period and a cooling period.

[0045] The preheating temperature is 250-400°C and the time is 10-15h. The preheating period is mainly to preheat the insulator green embryo to remove residual water and a small amount of crystal water.

[0046] The temperature of the oxidation period is 700-900°C and the time is 25-30h. During the oxidation period, most of the crystal water is discharged and organic matter, carbonates and part of sulfates are decomposed.

[0047] The temperature of the reduction period is 1000-1250° C. and the time is 25-30 hours. During the reduction period, most oxides are reduced, sulfates are decomposed, and carbon and carbon are oxidized, thereby forming a ceramic material.

[0048] The holding period is to slowly reduce the temperature from 1000-1250°C in the reduction period to 600°C, with a cooling rate of 50-80°C / h; during the holding period, the green embryo is completely calcined into ceramics to prevent the quality of the insulator from being reduced due to incomplete calcination.

[0049] The cooling period is 4-6 hours; the kiln is cooled to room temperature to prevent the ceramic from bursting due to rapid cooling and damaging the insulator structure.

[0050] S6: Structural inspection: The fired porcelain insulator is inspected for shed structure by an shed structure inspection device, wherein the shed inspection device comprises an shed inspection plate, the shed inspection plate comprises an inspection surface matching the shed structure of the porcelain insulator, and the inspection surface is provided with a marking device to obtain the marking result of the surface of the porcelain insulator to be inspected; taking the surface area of ​​the shed structure of the porcelain insulator as 100%, if the marking area of ​​the shed structure surface of the porcelain insulator is 0, proceed to the next step; if the marking area of ​​the shed structure surface of the porcelain insulator is ≤10%, the marking area of ​​the porcelain insulator is repaired until the structural inspection is passed; if the marking area of ​​the shed structure surface of the porcelain insulator is >10%, it is marked as unqualified.

[0051] The present invention performs structural inspection on fired porcelain insulators through an shed inspection plate with a specific structure. When the outer contours of the tested porcelain insulator samples are smaller than the size deviation, the marking device cannot mark the surface of the porcelain insulator; when the outer contours of the tested porcelain insulator samples are larger than the size deviation, the marking device marks the unqualified area. For porcelain insulators whose size deviations are within the standard range, a grinder can be used to grind the marked position of the porcelain insulator until the surface of the porcelain insulator is free of marks after inspection, and then proceed to the next step.

[0052] The shed structure detection device disclosed in the present invention can judge whether the shed structure of the porcelain insulator meets the standards through the marking of the porcelain insulator. The detection is convenient and the detection result is intuitive. The porcelain insulators that do not meet the standards can also be marked to provide an accurate marking area for the grinding and repair steps. In the production process of the porcelain insulator, not only the yield of the porcelain insulator can be guaranteed, but also the production efficiency of the porcelain insulator can be improved and the loss of the production process can be reduced.

[0053] In some embodiments, a gap is provided between the detection surface and the shed structure of the porcelain insulator, and the gap is designed according to the requirement of coating accuracy. For example, assuming that the shed diameter is required not to exceed 2 mm of the coating mold, the width of the gap is 1-2 mm.

[0054] like Figure 2 As shown, according to the data obtained by measuring the porcelain insulator standard parts through three-dimensional laser scanning, a shed detection plate is produced by 3D printing. The structure of the shed detection plate is completely consistent with the structure of the injection vulcanization mold of the hybrid insulator, and the shed detection plate has a detection surface that matches the shed structure of the porcelain insulator. Then, the shed detection plate is processed into a multi-piece assembly type. The shed detection plate disclosed in the present invention has three pieces, which are divided into a lower plate 6-1, an upper plate 6-2 and a middle plate 6-3. Then, according to the requirements of the coating accuracy, a marking device is installed on the detection surface. The marking device can be a color marking device, but the present disclosure is not limited to this.

[0055] If the shed detection plate is one-piece, when the shed structure is more complicated, such as a three-shed structure and the height difference of the outer edge of the shed is much greater than the height difference of the middle part, the insulator will be difficult to install into the shed detection plate.

[0056] The specific methods of structural detection are:

[0057] S61: Figure 2 As shown in a, the lower plate 6-1 of the shed detection plate is installed on the horizontal part of the base 5.

[0058] S62: Figure 2 As shown in b, the interior of the porcelain insulator head 3-1 is mounted on the vertical portion of the base 5, and the lower umbrella 3-3 of the porcelain insulator umbrella skirt structure is placed on the lower plate 6-1 of the umbrella skirt detection plate;

[0059] S63: Figure 2 As shown in c, the upper plate 6-2 of the shed detection plate connected to the drive shaft 7 is fixed to the head of the porcelain insulator;

[0060] S64: Figure 2 As shown in d, the middle plate 6-3 of the shed detection plate is fixed between the upper plate 6-1 of the shed detection plate and the upper plate 6-2 of the shed detection plate. If the installation of the shed detection plate fails, the tested porcelain insulator does not meet the requirements of the porcelain insulator standard parts and is marked as unqualified;

[0061] S65: Figure 2 As shown in Figure 5, the porcelain insulator is fixed, and the motor is started to drive the driving shaft 7 to make the shed detection plate 6 rotate at a constant speed for one circle to obtain the marking result of the surface of the porcelain insulator to be tested; the surface area of ​​the shed structure of the porcelain insulator is 100%, if the marking area of ​​the shed structure of the porcelain insulator is 0 (such as Figure 3 a), then proceed to the next step. If the marking area on the surface of the porcelain insulator shed structure is ≤10% (such as Figure 3 b), the marked area of ​​the porcelain insulator is repaired until it passes the structural inspection; if the marked area on the surface of the porcelain insulator shed structure is greater than 10% (such as Figure 3 c), marked as unqualified.

[0062] For the porcelain insulator that needs to be repaired, it is necessary to fix the porcelain insulator on the grinding base, use a grinder to grind the marked area, and select the appropriate grinding intensity and number of times according to the depth of the color of the marked area until the umbrella-shaped detection result of the polished porcelain insulator is as follows: Figure 3 As shown in a, the vulcanization coating step is entered.

[0063] The structure of the shed detection plate used for the structural detection of the present invention is completely consistent with the structure of the injection vulcanization mold of the hybrid insulator, which improves the accuracy of the detection result of the porcelain insulator. In addition, the shed detection plate of the present invention is a self-rotating structure, and there is no need to install the porcelain insulator into the detection structure. It is only necessary to place the porcelain insulator on the base and rely on the motor to drive the shed detection plate to rotate at a constant speed for one circle to obtain the detection result. The detection result is intuitive, and the detection process is simple, convenient, time-saving and energy-saving.

[0064] S7: Surface treatment, vulcanization coating:

[0065] The qualified products that have passed the structural inspection will be subjected to surface treatment, including but not limited to surface cleaning, degreasing treatment and silane coupling agent to change the hydrophilicity of the porcelain insulator glaze layer into hydrophobicity.

[0066] The surface treated porcelain insulator is placed in a coating mold and coated with a high temperature sulfide silicon umbrella sleeve under set temperature, pressure and time parameters.

[0067] Take out the vulcanized overmolded hybrid insulators, trim the coating, and then install the iron caps and steel feet. After passing the routine mechanical and electrical inspections, they are packaged and put into storage.

[0068] Example 1

[0069] like Figure 1 As shown, this embodiment provides a method for preparing a hybrid insulator, comprising the following steps:

[0070] To produce Figure 4Taking the double-umbrella hybrid insulator shown as an example, the double-umbrella hybrid insulator mainly consists of a steel cap 1, an adhesive 2, a porcelain insulator, and a steel foot 4. The porcelain insulator includes a porcelain insulator head 3-1, an upper umbrella 3-2, and a lower umbrella 3-3. The top of the porcelain insulator is connected to the steel cap 1 through the adhesive 2-1, and the inner top of the porcelain insulator is connected to the steel foot 4 through the adhesive 2-2. The standard weight of the clay blank used to prepare the porcelain insulator is 10 kg. According to calculations, when the weight deviation of the clay blank is ±0.5 kg or the weight percentage change rate is within the range of ±5%, the clay blank meets the requirements.

[0071] S1: Preparation of materials: Weigh the required raw materials according to the requirements of the porcelain insulator.

[0072] S2: Vacuum pugging: Use a vacuum pugging machine to pug the raw materials into clay segments and output them.

[0073] S3: Spin forming, air drying, and trimming: Shape the clay material after vacuum pugging according to the requirements of the product size to obtain the initial blank of the porcelain insulator. Let the initial blank of the porcelain insulator air dry naturally. It can be air dried naturally until the surface of the porcelain body looks white visually, and then trim it to meet the accuracy requirements of the product.

[0074] S4: Inspection of clay blanks: Install a weight sensing device on the robotic arm for transferring the clay blanks. Set the designed weight values as 10 kg and 10.5 kg. When the weight m ≤ 10.0 kg, the robotic arm transfers the clay blank to Zone A and records it as a high-quality product. When the weight 10.0 kg < m ≤ 10.5 kg, the robotic arm transfers the clay blank to Zone B and records it as a qualified product. When the weight m > 10.5 kg, the robotic arm transfers the clay blank to Zone C. Assume that the clay blanks in Zone C meet the requirements of porcelain insulators of other standards and can be used as raw materials for porcelain insulators of other standards and enter the next process of preparing porcelain insulators of other standards. Assume that the clay blanks in Zone C do not meet the requirements of porcelain insulators of other standards, or there is no production demand for porcelain insulators of other standards. The clay blanks in Zone C return to the material preparation step and are used as raw materials to produce porcelain insulators again. The clay blanks in Zone A and Zone B directly proceed to the next step.

[0075] S5: Drying, glazing, and firing: Dry the qualified clay blanks measured by the weight measuring device. The drying method is not particularly limited as long as the blank can be dried to a moisture content of less than 0.05%. The drying method can be drying in an oven or microwave drying.

[0076] The glazing method is not specifically limited, and those skilled in the art can select a suitable method for glazing according to actual needs. For example, it can be dip coating or spraying.

[0077] After glazing and before firing, there is also a sanding step. The purpose is to lay the foundation for binding to increase the stability and firmness of the binding accessories. The sand can be obtained by drying, crushing and screening the leftover materials from blank making, and its composition is the same as that of the blank.

[0078] The firing temperature, time and number of firings are not specifically limited, and those skilled in the art can select appropriate firing temperature, firing time and number of firings according to actual needs.

[0079] For example, the firing is carried out in stages, including a preheating period, an oxidation period, a reduction period, a heat preservation period and a cooling period.

[0080] The preheating temperature is 250-400°C and the time is 10-15h. The preheating period is mainly to preheat the insulator green embryo to remove residual water and a small amount of crystal water.

[0081] The temperature of the oxidation period is 700-900°C and the time is 25-30h. During the oxidation period, most of the crystal water is discharged and organic matter, carbonates and part of sulfates are decomposed.

[0082] The temperature of the reduction period is 1000-1250° C. and the time is 25-30 hours. During the reduction period, most oxides are reduced, sulfates are decomposed, and carbon and carbon are oxidized, thereby forming a ceramic material.

[0083] The holding period is to slowly reduce the temperature from 1000-1250°C in the reduction period to 600°C, with a cooling rate of 50-80°C / h; during the holding period, the green embryo is completely calcined into ceramics to prevent the quality of the insulator from being reduced due to incomplete calcination.

[0084] The cooling period is 4-6 hours; the kiln is cooled to room temperature to prevent the ceramic from bursting due to rapid cooling and damaging the insulator structure.

[0085] S6: Structural detection: Figure 2 As shown, according to the data obtained by measuring the porcelain insulator standard parts through three-dimensional laser scanning, a shed detection plate is produced by 3D printing. The structure of the shed detection plate is completely consistent with the structure of the injection vulcanization mold of the hybrid insulator, and the shed detection plate has a detection surface that matches the shed structure of the porcelain insulator. Then, the shed detection plate is processed into a multi-piece assembly. The shed detection plate disclosed in the present invention has three pieces, which are divided into a lower plate 6-1, an upper plate 6-2 and a middle plate 6-3. According to the requirements of the coating accuracy, the gap width between the detection surface and the shed structure of the porcelain insulator is 1 mm, and a color marking device is installed on the detection surface.

[0086] The specific methods of structural detection are:

[0087] S61: Figure 2 As shown in a, the lower plate 6-1 of the shed detection plate is installed on the horizontal part of the base 5.

[0088] S62: Figure 2 As shown in b, the interior of the porcelain insulator head 3-1 is mounted on the vertical portion of the base 5, and the lower umbrella 3-3 of the porcelain insulator umbrella skirt structure is placed on the lower plate 6-1 of the umbrella skirt detection plate;

[0089] S63: Figure 2 As shown in c, the upper plate 6-2 of the shed detection plate connected to the drive shaft 7 is fixed to the head of the porcelain insulator;

[0090] S64: Figure 2 As shown in d, the middle plate 6-3 of the shed detection plate is fixed between the upper plate 6-1 of the shed detection plate and the upper plate 6-2 of the shed detection plate. If the installation of the shed detection plate fails, the tested porcelain insulator does not meet the requirements of the porcelain insulator standard parts and is marked as unqualified;

[0091] S65: Figure 2 As shown in Figure 5, the porcelain insulator is fixed, and the motor is started to drive the driving shaft 7 to make the shed detection plate 6 rotate at a constant speed for one circle to obtain the marking result of the surface of the porcelain insulator to be tested; the surface area of ​​the shed structure of the porcelain insulator is 100%, if the marking area of ​​the shed structure of the porcelain insulator is 0 (such as Figure 3 a), then proceed to the next step. If the marking area on the surface of the porcelain insulator shed structure is ≤10% (such as Figure 3 b), the marked area of ​​the porcelain insulator is repaired until it passes the structural inspection; if the marked area on the surface of the porcelain insulator shed structure is greater than 10% (such as Figure 3 c), marked as unqualified.

[0092] For the porcelain insulator that needs to be repaired, it is necessary to fix the porcelain insulator on the grinding base, use a grinder to grind the marked area, and select the appropriate grinding intensity and number of times according to the depth of the color of the marked area until the umbrella-shaped detection result of the polished porcelain insulator is as follows: Figure 3 As shown in a, the vulcanization coating step is entered.

[0093] The structure of the shed detection plate used for the structural detection of the present invention is completely consistent with the structure of the injection vulcanization mold of the hybrid insulator, which improves the accuracy of the detection result of the porcelain insulator. In addition, the shed detection plate of the present invention is a self-rotating structure, and there is no need to install the porcelain insulator into the detection structure. It is only necessary to place the porcelain insulator on the base and rely on the motor to drive the shed detection plate to rotate at a constant speed for one circle to obtain the detection result. The detection result is intuitive, and the detection process is simple, convenient, time-saving and energy-saving.

[0094] S7: Surface treatment, vulcanization coating:

[0095] The qualified products that have passed the structural inspection are subjected to surface cleaning and degreasing treatment, and then a silane coupling agent is used to change the hydrophilicity of the porcelain insulator glaze layer into hydrophobicity;

[0096] The surface treated porcelain insulator is placed in a coating mold and coated with a high temperature sulfide silicon umbrella sleeve under set temperature, pressure and time parameters.

[0097] Take out the vulcanized overmolded hybrid insulators, trim the coating, and then install the iron caps and steel feet. After passing the routine mechanical and electrical inspections, they are packaged and put into storage.

[0098] Finally, it should be noted that the above embodiments are used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a hybrid insulator, characterized in that: The following steps are involved: Mud testing and structure testing; The clay blank detection step includes: placing the clay blank on a weight measuring device for weighing, obtaining the weight measurement result of the clay blank to be tested, comparing the weight measurement results, and the qualified products proceed to the next step; The structural detection step is: using a shed structure detection device to detect the shed structure of the fired porcelain insulator, the shed detection device includes a shed detection plate, the shed detection plate includes a detection surface matching the shed structure of the porcelain insulator, and the detection surface is provided with a marking device to obtain the marking result of the surface of the porcelain insulator to be tested; taking the surface area of ​​the shed structure of the porcelain insulator as 100%, if the marking area of ​​the shed structure surface of the porcelain insulator is 0, then proceed to the next step, if the marking area of ​​the shed structure surface of the porcelain insulator is ≤10%, then repair the marked area of ​​the porcelain insulator until it passes the structural detection; if the marking area of ​​the shed structure surface of the porcelain insulator is >10%, it is marked as unqualified.

2. The preparation method according to claim 1, characterized in that A gap is provided between the detection surface and the umbrella skirt structure of the porcelain insulator.

3. The preparation method according to claim 1, characterized in that: The umbrella skirt detection board includes a first detection board, a second detection board and a third detection board, wherein the third detection board is connected to the first detection board and the second detection board respectively.

4. The preparation method according to claim 3, characterized in that: The shed detection board also includes a driving device, and the driving device is connected to the first detection board.

5. The preparation method according to claim 1, characterized in that: The umbrella skirt structure detection device also includes a base, and the base is used to fix the porcelain insulator.

6. The preparation method according to claim 1, characterized in that: The marking device is a color marking device.

7. The preparation method according to claim 1, characterized in that: The weight measurement result comparison method is one of weight comparison and weight percentage deviation comparison.

8. The preparation method according to claim 1, characterized in that: The comparison of the weight measurement results is done in the measurement software.

9. The preparation method according to claim 1, characterized in that: The following steps are also included: Kneading the clay, shaping, trimming, drying, glazing, firing and vulcanization coating.

Citation Information

Patent Citations

  • Mud blank supply line for manufacturing porcelain insulator

    CN111015922A

  • Method for measuring surface deviation of core disc of disc insulator

    CN115585751A

  • Method for detecting interface state of high-temperature vulcanized silicone rubber coated insulator

    CN117949449A

  • Insulator form and location tolerance measuring device

    CN212133536U

  • Detection tool of disc-shaped suspension type porcelain insulator core body for mixed insulator

    CN219347618U

Cited By

  • Hybrid insulator preparation method

    WO2026011695A1