Semiconductor laser with high base film output power and preparation method thereof
By forming a high-resistance region and a low-refractive index dielectric column inside the P-type DBR layer of the semiconductor laser, the problems of low output power and difficult production of the base film in the existing technology are solved, and efficient laser output and simplified preparation processes are achieved. .
Patent Information
- Application Number
- CN202410673510.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-10-08
AI Technical Summary
Existing semiconductor lasers have problems such as low output power and high device manufacturing difficulty when increasing the output power of the base film. In particular, the base mode output efficiency of the oxidation-limited structure decreases when the aperture is less than 3 μm, and the etching of the photonic crystal structure is difficult.
A circular hole is formed inside the P-type DBR layer, and ions are implanted in the lower half of the hole to form a high-resistance area. A dielectric pillar is grown in the upper half of the hole. The material of the dielectric pillar is BN, AlN or GaN. The dielectric pillar The conductivity is greater than 5e3S/m and the refractive index is less than 2.5. It is prepared by chemical vapor deposition of metal organic compounds and magnetron sputtering technology.
It improves the basic mode output efficiency, filters high-order laser modes, optimizes light field characteristics and current distribution, reduces etching difficulty and threshold current, and simplifies the preparation process.
Smart Images

Figure CN118748353A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor lasers, and in particular relates to a semiconductor laser with high base film output power and a preparation method thereof. Background Art
[0002] Semiconductor lasers have the advantages of high photoelectric conversion efficiency, small size, light weight, and low cost, and have become a research hotspot in the field of optoelectronic technology. The electrically pumped vertical cavity surface emitting semiconductor laser has a very short resonant cavity and has the excellent characteristics of natural single longitudinal mode operation. However, the large lateral size will lead to multi-transverse mode output of the laser, reducing the beam quality. Single transverse mode lasers have the advantages of low loss and high beam quality, and have been widely used in optical communications, laser printing, laser mouse, atomic clock light sources and other fields.
[0003] With the popularization of smart devices and the rapid development of fields such as communications, higher demands are placed on laser light sources, and improving the fundamental mode output efficiency of lasers has become a research hotspot. The commonly used method is usually the oxidation confinement structure. When the aperture of the oxidation hole is less than 3μm, the output laser mode is the fundamental transverse mode. However, this will cause the fundamental mode output efficiency of the device to decrease and affect the output power. The photonic crystal structure can suppress high-order modes, but the etching difficulty is relatively high. Summary of the invention
[0004] In view of this, the present invention aims to provide a semiconductor laser with high base film output power and a preparation method thereof, so as to solve the technical problems of low output power and high difficulty in device manufacturing in the existing process of improving the base film output power.
[0005] To achieve the above object, the technical solution created by the present invention is implemented as follows: A semiconductor laser with high base film output power comprises, from bottom to top, an N-side electrode, a substrate, an N-type DBR layer, an oxidation restriction layer, an active layer, a P-type DBR layer and a P-side electrode. A circular hole is formed inside the P-type DBR layer at a position corresponding to a light output hole. The lower half of the hole is converted into a high resistance region by ion implantation. A dielectric column is prepared in the upper half of the hole. The conductivity of the dielectric column is greater than 5e3S / m and the refractive index is less than 2.5.
[0006] Furthermore, the dielectric column is made of doped BN material, AlN material or GaN material.
[0007] Furthermore, a passivation layer is prepared between the P-type DBR layer and the P-side electrode, and a light exit hole is exposed in the hollow area between the P-side electrode and the passivation layer.
[0008] Furthermore, the substrate is an N-type GaAs substrate, and the N-type DBR layer is 34 pairs of alternately grown Al 0.3 Ga 0.7As layer and Al 0.9 Ga 0.1 As layer, active layer is GaAs / Al 0.3 Ga 0.7 As quantum well structure, the oxidation limiting layer is Al 0.98 Ga 0.02 As layer, the passivation layer is a SiO2 passivation layer, and the P-type DBR layer is 12 pairs of heavily doped p-type AlGaAs layers.
[0009] A method for preparing a semiconductor laser with high base film output power comprises the following steps: S1: Using metal organic chemical vapor deposition technology to alternately grow 34 pairs of Al on N-type GaAs substrate 0.3 Ga 0.7 As layer and Al 0.9 Ga 0.1 As layer, forming an N-type DBR layer; S2: Using metal organic chemical vapor deposition technology to grow Al on the N-type DBR layer 0.98 Ga 0.02 As layer, forming an oxidation restriction layer; S3: Growth of GaAs / Al on an oxide confinement layer using metal organic chemical vapor deposition 0.3 Ga 0.7 As quantum well structure, forming the active layer; S4: growing 12 pairs of heavily doped p-type AlGaAs layers on the active layer using metal organic compound chemical vapor deposition technology to form a P-type DBR layer; wherein the N-type DBR layer, the oxidation restriction layer, the active layer and the P-type DBR layer constitute an epitaxial structure; S5: Photolithography the epitaxial structure using dry etching technology to form a mesa and expose the sidewall of the oxide restriction layer; S6: using a wet oxidation technique to laterally oxidize the sidewalls of the oxidation limiting layer to form a current limiting hole; S7: A SiO2 passivation layer is deposited on the epitaxial structure by plasma enhanced chemical vapor deposition technology, and the SiO2 passivation layer at the light exit hole is removed by etching; S8: using RIE technology to etch the P-type DBR layer from top to bottom until two pairs of heavily doped p-type AlGaAs layers remain, forming a circular hole; S9: performing ion implantation into the lower half of the hole to form a high resistance region; S10: using magnetron sputtering technology to deposit a dielectric column material in the upper half of the hole to form a dielectric column and strip off excess dielectric column material; wherein the dielectric column material is a doped BN material, AlN material or GaN material; S11: sputter Ti / Au on the SiO2 passivation layer using magnetron sputtering technology to form a P-side electrode, and peel off the photoresist to expose the light output hole; S12: Thinning and polishing the N-type GaAs substrate, sputtering AuGeNi / Au to form an N-side electrode, and performing annealing.
[0010] Compared with the prior art, the invention can achieve the following beneficial effects: 1. The present invention grows dielectric columns near the light-emitting hole to attract the light field at the edge of the light-emitting area. The high-order modes of the laser will be attracted by the dielectric columns with low refractive index during transmission, thereby filtering out the high-order modes and improving the fundamental mode efficiency. At the same time, since the dielectric columns have high conductivity, the current distribution in the light-emitting area will be improved and the light field characteristics of the device will be optimized.
[0011] 2. The present invention performs ion implantation on the N-type DBR layer to form a high resistance region, thereby reducing the area of the injected current, lowering the threshold current, and further improving the working efficiency of the device.
[0012] 3. The present invention can reduce the difficulty of the etching process. Conventional photonic crystal structures require air apertures with high aspect ratios, which will make the manufacturing process difficult and increase the threshold current. The dielectric columns prepared by the present invention have a lower aspect ratio, a smaller threshold, and a simpler manufacturing process. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments and descriptions of the present invention are used to explain the present invention and do not constitute an improper limitation on the present invention. In the drawings: Figure 1 A schematic structural diagram of a semiconductor laser with high base film output power according to an embodiment of the present invention.
[0014] Description of reference numerals: N-side electrode 1, substrate 2, N-type DBR layer 3, oxidation restriction layer 4, active layer 5, P-type DBR layer 6, passivation layer 7, P-side electrode 8, ion implantation region 9, dielectric column 10. DETAILED DESCRIPTION
[0015] In order to make the purpose, technical solution and advantages of the invention more clear, the invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described here are only used to explain the invention and do not constitute a limitation of the invention.
[0016] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0017] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0018] In the description of the invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installation", "connection" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the invention can be understood according to specific circumstances.
[0019] The following will refer to Figure 1 The invention is described in detail with reference to the embodiments.
[0020] like Figure 1As shown, an embodiment of the present invention provides a semiconductor laser with high base film output power, which can adopt InGaAs / GaAs, AlGaAs / GaAs, InGaAsP / GaAs and other material systems, and is selected according to the light-emitting band. The semiconductor laser includes, from bottom to top, an N-side electrode 1, a substrate 2, an N-type DBR layer 3, an oxidation restriction layer 4, an active layer 5, a P-type DBR layer 6, a passivation layer 7 and a P-side electrode 8. The hollow area between the P-side electrode 8 and the passivation layer 7 exposes a light exit hole to achieve laser emission. A circular hole is formed inside the P-type DBR layer 6 at a position corresponding to the light exit hole. The lower half of the hole is an ion implantation area 9. The ion implantation area 9 is transformed into a high resistance area by ion implantation, thereby reducing the area of the injected current, reducing the threshold current, and further improving the working efficiency of the device. A dielectric column 10 with a conductivity greater than 5e3S / m and a refractive index <2.5 is grown in the upper half of the hole, which is easy to grow and easy to remove. By growing a dielectric column 10 near the light-emitting hole to attract the light field at the edge of the light-emitting area, when the high-order mode of the laser is transmitted, the propagation path of the laser is affected by the law of refraction of light and the principle of least action, and will be attracted by the dielectric column 10 with a low refractive index, thereby filtering out the high-order mode and improving the fundamental mode efficiency; at the same time, since the dielectric column 10 has excellent conductive properties, it will improve the current distribution in the light-emitting area and optimize the light field characteristics of the device.
[0021] In a specific embodiment of the present invention, the dielectric pillar 10 is made of doped BN material, doped AlN material or doped GaN material.
[0022] Conventional photonic crystal structures require air apertures with high aspect ratios, which makes the manufacturing process difficult and increases the threshold current. The dielectric columns prepared in the present invention have a lower aspect ratio, a smaller threshold, and a simpler manufacturing process.
[0023] In another specific embodiment of the present invention, the substrate is an N-type GaAs substrate, and the N-type DBR layer is 34 pairs of alternately grown Al 0.3 Ga 0.7 As layer and Al 0.9 Ga 0.1 As layer, active layer is GaAs / Al 0.3 Ga 0.7 As quantum well structure, the oxidation limiting layer is Al 0.98 Ga 0.02 As layer, the passivation layer is a SiO2 passivation layer, and the P-type DBR layer is 12 pairs of heavily doped p-type AlGaAs layers.
[0024] The above content describes in detail the semiconductor laser with high base film output power provided by the embodiment of the present invention. Corresponding to the semiconductor laser with high base film output power, the present invention also provides a method for preparing the semiconductor laser, which specifically includes the following steps: S1: Using metal organic chemical vapor deposition technology to alternately grow 34 pairs of Al on N-type GaAs substrate 0.3 Ga 0.7 As layer and Al 0.9 Ga 0.1 As layer, forming an N-type DBR layer.
[0025] Al 0.3 Ga 0.7 As layer and Al 0.9 Ga 0.1 The As layers grow alternately, with a total of 34 pairs.
[0026] S2: Using metal organic chemical vapor deposition technology to grow Al on the N-type DBR layer 0.98 Ga 0.02 As layer, forming an oxidation restriction layer.
[0027] S3: Growth of GaAs / Al on an oxide confinement layer using metal organic chemical vapor deposition 0.3 Ga 0.7 As quantum well structure, forming the active layer.
[0028] S4: 12 pairs of heavily doped p-type AlGaAs layers are grown on the active layer using metal organic compound chemical vapor deposition technology to form a P-type DBR layer; wherein the N-type DBR layer, the oxidation restriction layer, the active layer and the P-type DBR layer constitute an epitaxial structure.
[0029] S5: Photolithography the epitaxial structure using dry etching technology to form a mesa and expose the sidewall of the oxidation restriction layer.
[0030] S6: Laterally oxidizing the sidewalls of the oxidation limiting layer using a wet oxidation technique to form a current limiting hole.
[0031] The diameter of the current limiting hole is about 10 μm.
[0032] S7: A SiO2 passivation layer is deposited on the epitaxial structure using plasma enhanced chemical vapor deposition technology, and the SiO2 passivation layer at the light exit hole is etched away.
[0033] S8: Etching the P-type DBR layer from top to bottom using RIE technology until only two pairs of heavily doped p-type AlGaAs layers remain, forming a circular hole.
[0034] S9: Ion implantation is performed into the lower half of the hole to form a high resistance region.
[0035] S10: depositing a dielectric column material in the upper half of the hole by magnetron sputtering technology to form a dielectric column and stripping off excess dielectric column material; wherein the dielectric column material is a doped BN material, a doped AlN material or a doped GaN material.
[0036] S11: Sputter Ti / Au on the SiO2 passivation layer using magnetron sputtering technology to form a P-side electrode, and strip off the photoresist to expose the light output hole.
[0037] S12: Thinning and polishing the N-type GaAs substrate, sputtering AuGeNi / Au to form an N-side electrode, and performing annealing.
[0038] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps described in the disclosure of the present invention can be performed in parallel, sequentially or in different orders, as long as the desired results of the technical solution disclosed in the present invention can be achieved, and this document does not limit this.
[0039] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A semiconductor laser with high base film output power, characterized in that: From bottom to top, it includes an N-side electrode, a substrate, an N-type DBR layer, an oxidation restriction layer, an active layer, a P-type DBR layer and a P-side electrode, characterized in that a circular hole is formed inside the P-type DBR layer corresponding to the position of the light output hole, the lower half area of the hole is converted into a high-resistance area by ion implantation, and a dielectric column is prepared in the upper half area of the hole, and the conductivity of the dielectric column is greater than 5e3S / m and the refractive index is <2.
5.
2. The semiconductor laser with high base film output power according to claim 1, characterized in that: The dielectric column is made of doped BN material, AlN material or GaN material.
3. The semiconductor laser with high base film output power according to claim 1 or 2, characterized in that: A passivation layer is further prepared between the P-type DBR layer and the P-side electrode, and the light exit hole is exposed in the hollow area between the P-side electrode and the passivation layer.
4. The semiconductor laser with high base film output power according to claim 3, characterized in that: The substrate is an N-type GaAs substrate, and the N-type DBR layer is 34 pairs of alternately grown Al 0.3 Ga 0.7 As layer and Al 0.9 Ga 0.1 As layer, active layer is GaAs / Al 0.3 Ga 0.7 As quantum well structure, the oxidation restriction layer is Al 0.98 Ga 0.02 As layer, the passivation layer is a SiO2 passivation layer, and the P-type DBR layer is 12 pairs of heavily doped p-type AlGaAs layers.
5. A method for preparing a semiconductor laser with high base film output power, characterized in that: The steps include: S1: Using metal organic chemical vapor deposition technology to alternately grow 34 pairs of Al on N-type GaAs substrate 0.3 Ga 0.7 As layer and Al 0.9 Ga 0.1 As layer, forming an N-type DBR layer; S2: using metal organic compound chemical vapor deposition technology to grow Al on the N-type DBR layer 0.98 Ga 0.02 As layer, forming an oxidation restriction layer; S3: Growing GaAs / Al on the oxide confinement layer using metal organic chemical vapor deposition technology 0.3 Ga 0.7 As quantum well structure, forming the active layer; S4: growing 12 pairs of heavily doped p-type AlGaAs layers on the active layer using metal organic compound chemical vapor deposition technology to form a P-type DBR layer; wherein the N-type DBR layer, the oxidation restriction layer, the active layer and the P-type DBR layer constitute an epitaxial structure; S5: performing photolithography on the epitaxial structure using dry etching technology to form a mesa and expose the sidewall of the oxidation restriction layer; S6: using a wet oxidation technique to laterally oxidize the sidewalls of the oxidation limiting layer to form a current limiting hole; S7: depositing a SiO2 passivation layer on the epitaxial structure by plasma enhanced chemical vapor deposition technology, and etching away the SiO2 passivation layer at the light exit hole; S8: etching the P-type DBR layer from top to bottom using RIE technology until two pairs of heavily doped p-type AlGaAs layers remain, forming a circular hole; S9: performing ion implantation into the lower half of the hole to form a high resistance region; S10: using magnetron sputtering technology to deposit a dielectric column material in the upper half of the hole to form a dielectric column and strip off excess dielectric column material; wherein the dielectric column material is a doped BN material, AlN material or GaN material; S11: sputtering Ti / Au on the SiO2 passivation layer using magnetron sputtering technology to form a P-side electrode, and stripping the photoresist to expose the light output hole; S12: thinning and polishing the N-type GaAs substrate, sputtering AuGeNi / Au to form an N-side electrode, and performing annealing.
Citation Information
Cited By
Vertical cavity surface emitting laser and preparation method thereof
CN121216222A