N-type Ti3C2Tx flexible thermoelectric thin film and regulation and control method thereof
Through the electrochemical control method, the problem of improving the performance of n-type Ti3C2Tx thermoelectric materials has been solved, high stability and significantly improved thermoelectric performance have been achieved, the preparation process has been simplified, and it is suitable for large-scale applications.
Patent Information
- Application Number
- CN202410721477.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-08
AI Technical Summary
Existing technology is difficult to effectively control the conductivity and Seebeck coefficient of n-type Ti3C2Tx thermoelectric materials, resulting in limited improvement in thermoelectric performance and difficulty in realizing large-scale power generation applications.
Using electrochemical control method, Ti3AlC2 is etched by mixing LiF and HCl solution to prepare multi-layer Ti3C2Tx powder, and a flexible thermoelectric film is formed through ultrasonic, centrifugal and electrochemical control, and the surface is controlled by cyclic voltammetry and potentiostatic method. Oxygen vacancies improve thermoelectric performance.
The Ti3C2Tx thermoelectric film achieves high stability and significantly improved room temperature conductivity, with a maximum value of 4052.31S cm-1 and a power factor of 6-22.18μWm-1K-2. It simplifies the preparation process and is suitable for popularization and application.
Smart Images

Figure CN118748905A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermoelectric materials, in particular to an n-type Ti3C2T x Control methods for flexible thermoelectric films. Background Art
[0002] Thermoelectric technology can achieve the mutual conversion between thermal energy and electrical energy through the transport of carriers in materials, and is one of the frontiers of green and clean energy research. Compared with the mature p-type thermoelectric materials, the research on n-type thermoelectric materials is limited.
[0003] Ti3C2T x As a unique natural n-type carbon-based material, it is attractive. Due to its large interlayer spacing, good chemical stability, tunable surface chemical properties, high conductivity and excellent flexibility, it has broad application prospects in the field of thermoelectrics. However, Ti3C2T x Research in this field is still in its infancy and more efforts are needed to further improve thermoelectric performance.
[0004] Currently for Ti3C2T x The regulation is limited to compounding, annealing and construction of Ti3C2T x Organic superlattices are used to improve thermoelectric performance. However, these control methods are difficult to decouple conductivity and Seebeck coefficient, resulting in limited improvement in thermoelectric performance and difficulty in achieving large-scale power generation applications. Therefore, it is necessary to further develop simple and efficient control methods to improve the performance of n-type Ti3C2T x Thermoelectric properties are of great significance. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for efficiently regulating Ti3C2T x The method of thermoelectric performance is simple to control and has excellent stability, making it suitable for popularization and application.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] On the one hand, the present invention provides an n-type Ti3C2T x Flexible thermoelectric film, the n-type Ti3C2T x Flexible thermoelectric films are prepared by electrochemical regulation methods.
[0008] Furthermore, the n-type Ti3C2T x The power factor of the flexible thermoelectric film is 6-22.18μWm -1 K -2 .
[0009] On the other hand, the present invention also provides the n-type Ti3C2T x The control method of the flexible thermoelectric film includes:
[0010] (1) Mix LiF and HCl solution to etch Ti3AlC2 to obtain multilayer Ti3C2T x powder;
[0011] (2) Multilayer Ti3C2T x The powder was dispersed in aqueous solution, and Ti3C2T was obtained by ultrasonication and centrifugation. x Solution, for Ti3C2T x The solution is filtered and vacuum dried;
[0012] (3) The Ti3C2T prepared in step 2 x Electrochemical regulation of thin films;
[0013] (4) The Ti3C2T prepared in step 3 x The film is dried.
[0014] Furthermore, in step (3), the electrochemical regulation mainly includes cyclic voltammetry regulation and constant potential regulation; in the electrochemical regulation, the reference electrode is a saturated calomel electrode, Ag / AgCl, or mercury oxide electrode, the counter electrode is a graphite electrode or a platinum electrode, and the working electrode is Ti3C2T x The film is H2SO4 electrolyte with a molar concentration of 0.5 to 6 mol / L, a potential window of -0.8 to 0.4 V, a scan rate of 1 to 100 mV / s, and a cycle of 50 to 500 cycles.
[0015] Furthermore, in step (3), the electrochemical regulation is cyclic voltammetry regulation, the reference electrode is a saturated calomel electrode, the counter electrode is a graphite electrode, the molar concentration of H2SO4 is 0.5 mol / L, the potential window is -0.5 to 0 V, the scan rate is 50 mV / s, the cycle is 200, and the potential regulated by the constant potential method is -0.5 V for 900 s.
[0016] Furthermore, in the step (1), the etching treatment conditions are heating in an oil bath, a reaction temperature of 40-50°C, a reaction time of 12h-24h, a Ti3AlC2 purity greater than 98%, 300-400 mesh, a LiF to Ti3AlC2 mass ratio of 1-2:1, and a HCl solution molar concentration of 6-9mol / L.
[0017] Furthermore, in step (2), the multilayer Ti3C2T xThe mass concentration of the powder is 0.5-5 mg / ml; the ultrasonic condition time is 0.5-3 h, and the ultrasonic power is 200W-650W; the centrifugal condition is 2000-5000 rpm, 5-30 min; the drying temperature is 40-90 DEG C, and the drying time is 1-12 h.
[0018] Furthermore, in step (2), the multilayer Ti3C2T x The mass concentration of the powder is 5 mg / ml; the ultrasonic time is 1 h, the ultrasonic power is 400 W; the centrifugal conditions are 3000 rpm, 30 min; the drying temperature is 60° C., and the drying time is 3 h.
[0019] Furthermore, in step (4), Ti3C2T x The film was immersed in deionized water for 5 min and dried at 60 °C for 1 h.
[0020] The present invention has the following beneficial effects:
[0021] (1) The present invention adopts an electrochemical method to generate n-type Ti3C2T x The generation of surface-induced oxygen vacancies avoids the use of complex preparation processes such as high-temperature hydrogen reduction. It has low requirements for reaction equipment, simple operation, mild conditions, high preparation efficiency, and can effectively simplify the preparation process, making it suitable for promotion and application.
[0022] (2) Highly stable oxygen vacancies can be generated by electrochemical methods. The introduction of oxygen vacancies significantly improves the room temperature conductivity, with a maximum value of 4052.31 S cm -1 This value is the highest reported in the thermoelectric field for Ti3C2T x The maximum value. On the basis of ensuring good thermoelectric performance, it also has excellent stability;
[0023] (3) Electrochemical regulation can selectively extract oxygen groups on the surface of MXene through cations in the electrolyte, so this method can be further extended to other MXene materials to produce oxygen vacancies to adapt to various application fields;
[0024] (4) This universal route through electrochemical regulation can serve as a platform for surface modification and be extended to other layered materials to discover new, efficient thermoelectric materials. The unlimited choice of various electrolytes can further diversify the composition to provide strategies for optimizing thermoelectric performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Ti3C2T prepared in Example 6 of the present invention x film;
[0026] Figure 2Ti3C2T prepared in Example 6 of the present invention x EPR spectrum of the material after being placed in air for 3 weeks;
[0027] Figure 3 Ti3C2T prepared in Example 6 of the present invention x Flexible thermoelectric film and Ti3C2T substrate without electrochemical control treatment x Thin film power factor comparison. DETAILED DESCRIPTION
[0028] In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail with reference to the accompanying drawings and specific embodiments. However, the present invention is by no means limited to these examples. The following is only a preferred embodiment of the present invention, which is only used to explain the present invention and cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
[0029] Unless otherwise specified, the components used in the present invention are all commercially available products, and the experimental test conditions are not particularly specified, and are all conventional technical operations in the art.
[0030] The present invention aims at improving Ti3C2T x Thermoelectric performance control methods are limited and difficult to achieve large-scale power generation applications. A simple control method and excellent stability are provided for an n-type Ti3C2T x Flexible thermoelectric films and control methods thereof.
[0031] Example
[0032] An n-type Ti3C2T x Flexible thermoelectric film is prepared by electrochemical regulation method.
[0033] Electrochemical control methods include:
[0034] 1) Mix 1.2g LiF with 12ml 9M HCl and heat 1g Ti3AlC2 in an oil bath to 40-50℃ and etch for 24h to obtain multilayer Ti3C2T x powder;
[0035] 2) Multilayer Ti3C2T x The powder was dispersed in deionized water to prepare a solution with a mass concentration of 5 mg / ml. Ultrasonication was performed for 1 h at a power of 400 W and centrifuged at 3000 rpm for 30 min to collect the few-layer Ti3C2T x solution; collect the few-layer Ti3C2T xThe solution was filtered and then vacuum dried at 60°C for 3 h.
[0036] 3) The few-layer Ti3C2T x The film was electrochemically regulated by cyclic voltammetry, with a saturated calomel electrode as the reference electrode, a graphite electrode as the counter electrode, and a Ti3C2T x Thin film, electrolyte is H2SO4, molar concentration is 0.5mol / L, potential window is -0.8~0.4V, scan rate is 1~100mV / s, cycle is 50~500 times;
[0037] 4) Ti3C2T after electrochemical regulation x The film was immersed in deionized water for 5 min and dried at 60 °C for 1 h. -0.5V .
[0038] Determination of the electrochemical regulation of Ti3C2T by cyclic voltammetry in Example 1-7 x The power factor of the film, the specific reaction conditions and the Ti3C2T x The power factor of the film is shown in the following table:
[0039]
[0040] Example 8-12 Control of Ti3C2T by constant potential method x films, specific reaction conditions and Ti3C2T x The power factor of the film is shown in the following table:
[0041]
[0042] As can be seen from Examples 1-12, the present invention provides a method for efficiently regulating Ti3C2T x Thermoelectric properties of Ti3C2T x Thermoelectric film morphology Figure 1 As shown in the figure, the power factor parameters were comprehensively determined and the Ti3C2T x The film achieved better results.
[0043] like Figure 2 As shown, the Ti3C2T prepared in Example 6 x EPR spectrum of the thin film material after being placed in air for 3 weeks. The results show that electrochemical regulation can produce highly stable oxygen vacancies to maintain Ti3C2T for a long time. x High thermoelectric performance.
[0044] Figure 3 Ti3C2T prepared in Example 6 xFlexible thermoelectric film and Ti3C2T substrate without electrochemical control treatment x Thin film power factor comparison, under the same conditions, the matrix Ti3C2T without electrochemical control treatment x The room temperature power factor of the film (labeled MXene) is less than 5 μWm -1 K -2 In Example 6 of the present invention, Ti3C2T x Significant improvement in the power factor of thin film materials, exceeding 20 μW m -1 K -2 , and exceeds most existing studies on Ti3C2T x Material properties reported.
[0045] Therefore, the present invention develops a simple and low-cost n-type Ti3C2T x The control method is to control the cation and n-type Ti3C2T by changing the potential window and the number of scans in a three-electrode system. x The interaction between surface functional groups enables intercalation and surface chemical modification, resulting in a power factor exceeding 20 μWm -1 K -2 . On the basis of ensuring good thermoelectric performance, it also has excellent stability. This regulation method has the advantages of simple operation, high efficiency, safety and environmental protection, and provides a new idea for optimizing the thermoelectric performance of n-type MXene by surface group modification. The obtained n-type thermoelectric film can be widely used in waste heat recovery, heating elements, electronic equipment and other fields, and has broad application prospects and market potential.
[0046] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An n-type Ti3C2T x Flexible thermoelectric film, characterized in that The n-type Ti3C2T x Flexible thermoelectric films are prepared by electrochemical regulation methods.
2. The n-type Ti3C2T according to claim 1 x Flexible thermoelectric film, characterized in that The n-type Ti3C2T x The power factor of the flexible thermoelectric film is 6-22.18μWm -1 K -2 .
3. An n-type Ti3C2T x A method for regulating a flexible thermoelectric film, characterized in that: The control method comprises: (1) Mix LiF and HCl solution to etch Ti3AlC2 to obtain multilayer Ti3C2T x powder; (2) Multilayer Ti3C2T x The powder was dispersed in aqueous solution, and Ti3C2T was obtained by ultrasonication and centrifugation. x Solution, filtering and vacuum drying the Ti3C2Tx solution; (3) The Ti3C2T prepared in step 2 x Electrochemical regulation of thin films; (4) The Ti3C2T prepared in step 3 x The film is dried.
4. The n-type Ti3C2Tx flexible thermoelectric film according to claim 3, characterized in that: In the step (3), the electrochemical regulation mainly includes cyclic voltammetry regulation and constant potential regulation; in the electrochemical regulation, the reference electrode is a saturated calomel electrode, Ag / AgCl, or mercury oxide electrode, the counter electrode is a graphite electrode or a platinum electrode, and the working electrode is Ti3C2T x The film is H2SO4 electrolyte with a molar concentration of 0.5 to 6 mol / L, a potential window of -0.8 to 0.4 V, a scan rate of 1 to 100 mV / s, and a cycle of 50 to 500 cycles.
5. The n-type Ti3C2T3 according to claim 4 x Flexible thermoelectric film, characterized in that In the step (3), the electrochemical regulation is cyclic voltammetry regulation and constant potential regulation, the reference electrode is a saturated calomel electrode, the counter electrode is a graphite electrode, the molar concentration of H2SO4 is 0.5 mol / L, the potential window of cyclic voltammetry regulation is -0.5 to 0 V, the scanning rate is 50 mV / s, the cycle is 200, and the potential of the constant potential regulation is -0.5 V, and the time is 900 s.
6. The n-type Ti3C2T3 according to claim 3 x Flexible thermoelectric film, characterized in that In the step (1), the etching treatment conditions are heating in an oil bath, a reaction temperature of 40-50° C., a reaction time of 12 h-24 h, a Ti3AlC2 purity greater than 98%, 300-400 mesh, a LiF to Ti3AlC2 mass ratio of 1-2:1, and a HCl solution molar concentration of 6-9 mol / L.
7. The n-type Ti3C2T3 according to claim 3 x Flexible thermoelectric film, characterized in that In the step (2), the mass concentration of the multilayer Ti3C2Tx powder in the aqueous solution is 0.5-5 mg / ml; the ultrasonic condition time is 0.5-3 h, and the ultrasonic power is 200 W-650 W; the centrifugal condition is 2000-5000 rpm, 5-30 min; the drying temperature is 40-90° C., and the drying time is 1-12 h.
8. The n-type Ti3C2T3 according to claim 7 x Flexible thermoelectric film, characterized in that In the step (2), the multilayer Ti3C2T x The mass concentration of the powder is 5 mg / ml; the ultrasonic time is 1 h, the ultrasonic power is 400 W; the centrifugal conditions are 3000 rpm, 30 min; the drying temperature is 60° C., and the drying time is 3 h.
9. The n-type Ti3C2T3 according to any one of claims 3 to 8 x Flexible thermoelectric film, characterized in that In the step (4), Ti3C2T x The film was immersed in deionized water for 5 min and dried at 60 °C for 1 h.