CO2 adsorption systems and methods of CO2 adsorption using humidity-stable polystyrene-divinylaniline functionalized polymeric adsorbents

By using amino-functional adsorbent materials with specific specific surface area and pore volume distribution, the instability problem of adsorbent materials in DAC under different humidity conditions is solved, achieving stable carbon dioxide capture in the entire relative humidity range, ensuring Continuous and efficient direct air capture process.

CN118748950APending Publication Date: 2024-10-08CLIMEWORKS AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280082993.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2021-12-16
Filing Date
2022-12-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

In the existing technology, in direct air capture (DAC), the carbon dioxide adsorption performance of the adsorbent material is unstable under different relative humidity conditions, which affects the continuity and efficiency of the gas separation process.

Method used

Using amino-functionalized solid inorganic or organic non-polymeric or polymeric materials with specific specific surface area and pore volume distribution as adsorbents, through pore volume distribution and surface functionalization in the range of 50nm to 350nm, 0% to 100% Stable carbon dioxide adsorption performance within % relative humidity range.

Benefits of technology

It achieves stable and efficient carbon dioxide capture capabilities under different relative humidity conditions, allows continuous operation under different weather and seasonal conditions, and improves the applicability and controllability of adsorbent materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748950A_ABST
    Figure CN118748950A_ABST
Patent Text Reader

Abstract

The invention relates to a method for separating gaseous carbon dioxide from air, in particular from ambient atmospheric air (1), by cyclic adsorption / desorption with an adsorbent material (3), said adsorbent material (3) being a solid inorganic or organic non-polymeric or polymeric carrier material functionalized on the surface with amino functionality capable of reversibly binding carbon dioxide, having a BET specific surface area, preferably measured by nitrogen adsorption, in the range of 10 m < 2 > / g to 25 m < 2 > / g, and having a pore volume distribution such that a cumulative pore volume in the range of 50 nm to 350 nm is in the range of 0.3 cm < 3 > / g to 1.5 cm < 3 > / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the use of an adsorbent material for separating gaseous carbon dioxide from a gas mixture, in particular for direct air capture (DAC), and to a corresponding method, in particular for the direct capture of carbon dioxide from atmospheric air. Prior art

[0002] The Paris Agreement reached consensus on the threat of climate change and the need for a global response in order to keep global temperature rise to well below 2 degrees Celsius above pre-industrial levels. To achieve this goal, a variety of possibilities have been proposed, from planting new forests to technological means. Planting new trees resonates widely in public opinion, but the scope and feasibility of such projects are controversial and may not be as simple a solution as one might think.

[0003] Among technical approaches, the most advanced technologies include storing CO2 from point sources, such as exhaust gas capture, and capturing CO2 directly from the air, known as direct air capture (DAC). Both technical strategies have the potential to mitigate climate change.

[0004] Specific advantages of capturing CO2 from the atmosphere over exhaust gas capture include: DAC (i) can process emissions from dispersed sources (e.g., cars, airplanes); (ii) does not need to be attached to the emission source, but can be located independently of the emission source; (iii) can process emissions from the past, so if combined with a safe and permanent method to store CO2 (e.g., through underground mineralization), negative emissions can be achieved. DAC is also used as one of several means of providing key reactants for the synthesis of renewable materials or fuels, such as described in WO-A-2016 / 161998.

[0005] As far as suitable capture materials are concerned, several DAC technologies have been described in the literature, for example, the formation of calcium carbonate using alkaline earth oxides in water, as described, for example, in US-A-2010034724. Different approaches include the use of solid CO2 adsorbents, hereinafter referred to as adsorbents, characterized by the use of packed beds and wherein the CO2 is captured at the gas-solid interface. Such adsorbents may comprise different types of amino functionalizations and polymers, for example immobilized aminosilane-based adsorbents as reported in US-B-8,834,822, and amine-functionalized cellulose as disclosed in WO-A-2012 / 168346.

[0006] WO-A-2011 / 049759 describes the use of ion exchange materials comprising aminoalkylated bead polymers for removing carbon dioxide from industrial applications.

[0007] WO-A-2016 / 037668 describes an adsorbent for reversibly adsorbing CO2 from a gas mixture, wherein the adsorbent comprises a polymer adsorbent having primary amino functionality and having 25 m 2 / g to 75m 2 The material has a high specific surface area of ​​1.176 million t / g (calculated by the Brunauer-Emmet-Teller method) and a specific average pore size. The material is regenerated after capture by applying pressure or humidity changes.

[0008] WO-A-2016 / 038339 describes a method for removing carbon dioxide using a polymer adsorbent having primary amine units immobilized on a solid support. The adsorbent is then regenerated by heating the adsorbent at a temperature ranging from 55°C to 75°C while passing air through the adsorbent.

[0009] US-B-6716888 and US-B-6503957 describe a process in which a ground ion exchange resin is introduced into a polymeric binder molten at a temperature of 125° C. to 130° C. and the multiphase mixture is formed into sheets having a maximum thickness of 0.125 mm for use in water purification.

[0010] US-A-2012076711 discloses a structure comprising an adsorbent having amine groups capable of undergoing a reversible adsorption and desorption cycle for capturing CO2 from a gas mixture, wherein the structure comprises fiber filaments, wherein the fiber material is carbon and / or polyacrylonitrile.

[0011] US-A-2018043303 discloses a porous adsorbent structure capable of reversible adsorption and desorption cycles for capturing CO2 from a gas mixture, and comprising a carrier matrix formed by a network of surface-modified cellulose nanofibers. The porosity of the carrier matrix is ​​at least 20%. The surface-modified cellulose nanofibers are composed of cellulose nanofibers having a diameter of about 4 nm to about 1000 nm and a length of 100 nm to 1 mm, which are covered with a coupling agent covalently bonded to their surface. The coupling agent comprises at least one monoalkyldialkoxyaminosilane.

[0012] US-A-2019224647 provides a new solid adsorbent synthesized by reacting polyamines with polyaldehyde phosphorus dendrimer (P-dendrimer) compounds. The adsorbent is stable and exhibits rapid reaction kinetics with carbon dioxide, making the adsorbent suitable for carbon capture and can be easily regenerated for further use. The material is stable to aqueous and organic media as well as strong acids and bases. The adsorbent maintains full capacity during expanded use. The material can be used for CO2 capture from pure CO2 streams, mixed gas streams, simulated exhaust gases, and ambient air. In addition, the material can be adhered to surfaces for reversible CO2 capture applications outside of bulk particle-based processes.

[0013] US-A-2017203249 discloses a method for separating gaseous carbon dioxide from a mixture by using a cyclic adsorption / desorption device comprising an adsorber structure having an adsorbent material, wherein the method comprises the following steps: (a) contacting the mixture with the adsorbent material under ambient conditions so that the gaseous carbon dioxide is adsorbed; (b) evacuating the device to a pressure in the range of 20 mbar abs to 400 mbar abs and heating the adsorbent material to a temperature in the range of 80°C to 130°C using an internal heat exchanger; and (c) repressurizing the device to ambient atmospheric pressure conditions and actively cooling the adsorbent material to a temperature greater than or equal to ambient temperature; wherein in step (b), water vapor is injected into the device so that it flows through and contacts the adsorbent material under saturated water vapor conditions, and wherein the molar ratio of the injected water vapor to the released gaseous carbon dioxide is less than 20:1.

[0014] Irani et al. ("Facilely synthesized porous polymer as support of poly(ethyleneimine)for effective CO2 capture", Energy (157), pp. 1 to 9 (2018)) proposed an effective adsorbent (polyHIPE / PEI) for CO2 capture technology. For this purpose, a porous polymer was prepared using 2-ethylhexyl methacrylate (EHMA) and divinylbenzene (DVB) by high internal phase emulsion (HIPE). The prepared porous polymer (polyHIPE) was then used as a new support for wet impregnation of polyethyleneimine (PEI), thereby obtaining a polyHIPE / PEI adsorbent. The prepared adsorbent was characterized. At an optimal PEI loading of 60 wt% on polyHIPE, the CO2 adsorption capacity reached 4 mmolCO2 / g-adsorbent using 10 vol% CO2 and 3 vol% H2O in N2 at 70°C. Kinetic and thermodynamic adsorption studies showed that the activation energies of CO2 adsorption and desorption on polyHIPE / PEI were 13.74 kJ / mol and 36.12 kJ / mol, respectively.

[0015] Jung et al. reported in Energy Fuels 2014, 28, 3994-4001 the use of poly(ethyleneimine) (PEI) as an amine and mesoporous poly(methyl methacrylate) (PMMA) beads as a support to prepare solid amine adsorbents with sufficient particle size and high CO2 adsorption capacity. The PEI-impregnated PMMA-supported adsorbent exhibited a CO adsorption capacity of up to 4.26 mmol / g using PMMA-55 at 75°C in a pure CO gas stream. The effect of temperature on the adsorption capacity of PMMA-55 was studied, and the maximum adsorption capacity was obtained at 50°C and 180 minutes of CO2 exposure time, which is different from the trend of most silica-supported adsorbents. Due to the different surface properties between PMMA and silica, the effect of surfactant addition on the adsorption performance of PMMA-supported adsorbents is different from that on the adsorption performance of silica-supported adsorbents. Adsorption / desorption cycles were also performed to examine the suitability of amine adsorbents for potential applications.

[0016] Hammache et al. reported in Energy & fuels that amine adsorbents prepared by impregnating polyethyleneimine on silica were tested for water vapor stability. At 105 ° C, multiple water vapor cycles of 90% by volume H2O / He were used in a fixed bed reactor to study the stability of the adsorbent, and the gas effluent was monitored by a mass spectrometer. It was found that the CO2 absorption of the adsorbent decreased with repeated exposure to water vapor. The spent adsorbent was characterized using N2 physical adsorption, SEM and thermogravimetric analysis (TGA), indicating that the reduction in CO2 loading may be attributed to the re-agglomeration of amines in the pores of silica. No supporting effect was found in this study. It was found that the commercial SiO2 used, Cariact G10, was stable under the conditions used. Although it was found that subjecting the adsorbent to several water vapor cycles reduced its CO2 absorption, continuous exposure of the adsorbent to water vapor did not have a significant performance impact. The water vapor stability of the silanized adsorbent was also studied, and the silanized adsorbent was composed of a mixture of PEI and aminopropyl-triethoxysilane on a SiO2 carrier. Similar to the unsilanized sorbent, the CO2 loading of this sorbent decreases upon water vapor exposure, although the mechanism for this change has not yet been hypothesized.

[0017] US 6,279,576 B1 relates to a regenerative adsorber device for removing CO2 from expired gas during anesthesia. The device comprises a container having an inlet for the expired gas and an outlet for outputting the gas, from which the CO content in the container has been substantially removed. The device is provided with an ion exchanger having the ability to absorb CO2, the ion exchanger being arranged in the container so that the gas flows from the inlet through the ion exchanger to the outlet. The new anesthesia method comprises the use of a CO2 adsorber device.

[0018] Liu et al. reported in J.APPL.POLYM.SCI.2017,134,45046 how to prepare a solid amine adsorbent by modifying a porous polystyrene resin (XAD-4) with chloroacetyl chloride: by Friedel-Crafts acylation, followed by amination with tetraethylenepentamine (TEPA). The performance of adsorbing CO2 from simulated exhaust gas on the solid amine adsorbent was evaluated. Factors that can determine the CO adsorption performance of the adsorbent, such as the type of amine, adsorption temperature and moisture, were studied. The experimental results show that the solid amine adsorbent modified with TEPA (XAD-4-TEPA) with a longer chain shows an amine efficiency superior to that of the other two amine species with shorter chains. With increasing temperature, the adsorption capacity of CO2 decreases significantly because the reaction between CO2 and amine groups is an exothermic reaction, and its adsorption capacity reaches 1.7 mmol / g under dry conditions at 10°C. The presence of water can significantly increase the CO2 adsorption capacity of the adsorbent and promote the chemical adsorption of CO2 on XAD-4-TEPA. After 10 adsorption-desorption cycles, the adsorbent maintained almost the same adsorption capacity. All these results indicate that amine-functionalized XAP-4 resin is a promising CO2 adsorbent.

[0019] US2017 / 0203249 relates to a method for separating gaseous carbon dioxide from a mixture by cyclic adsorption / desorption using an apparatus comprising an adsorber structure having an adsorbent material, wherein the method comprises the following steps: (a) contacting the mixture with the adsorbent material under ambient conditions so that the gaseous carbon dioxide is adsorbed; (b) evacuating the apparatus to a pressure in the range of 20 mbar to 400 mbar and heating the adsorbent material to a temperature in the range of 80°C to 130°C; and (c) repressurizing the apparatus to ambient atmospheric pressure conditions and actively cooling the adsorbent material to a temperature greater than or equal to ambient temperature; wherein in step (b), water vapor is injected into the apparatus so that it flows through and contacts the adsorbent material under saturated water vapor conditions, and wherein the molar ratio of the injected water vapor to the released gaseous carbon dioxide is less than 20:1. Summary of the invention

[0020] The present invention relates to a process for separating gaseous carbon dioxide from a gas mixture, preferably from at least one of ambient atmospheric air, exhaust gas and biogas, in particular to a DAC process using a specific adsorbent material, and to the use of such a specific adsorbent material for gas separation purposes, in particular DAC.

[0021] Herein it is shown that the prior art claims that crosslinked polystyrene adsorbents, in particular substituted with primary aminoalkyl functional groups and featuring a high specific surface area, and also other adsorbents based on inorganic or organic non-polymeric or polymeric materials having a high specific surface area, are particularly useful for DAC applications. Surprisingly, it has now been found that, contrary to this belief, inorganic or organic non-polymeric or polymeric materials functionalized with amino groups, in particular (but not exclusively) crosslinked polystyrene adsorbents, such as crosslinked polystyrene adsorbents based on divinylbenzene (DVB), thus for example (poly(styrene-co-divinylbenzene)), have a specific surface area in a very specific medium range combined with a pore volume distribution in a specific range - i.e. the cumulative pore volume in the range of 50 nm to 350 nm must be within 0.28 cm 3 / g to 1.5cm 3 / g range - shows unexpectedly stable carbon dioxide adsorption performance that is essentially independent of humidity conditions during water vapor desorption. This is crucial for process stability under different weather and input gas composition conditions: namely under conditions with variable relative humidity (RH, for example defined as the amount of water vapor present in the air, expressed as a percentage of said amount required for saturation at the same temperature, for experiments with water vapor desorption, given here as 15°C, typically in the incoming gas flow of a DAC device with the corresponding adsorbent; the relative humidity given here is generated by using a humidifier system in which a dry flow (RH 0%) is mixed with a saturated flow in different ratios depending on the target RH. The saturated flow is generated by bubbling a dry gas through a water column. The relative humidity is determined using a Vaisala humidity and temperature probe HMP110) type device. In an exemplary adsorption test conducted after air-purged temperature swing desorption, the temperature of the reactor was maintained at 30°C and the RH was controlled by varying the temperature of the bubbler through which the inlet gas was fed to reach a target RH value at 30°C.

[0022] Specifically, according to the present invention, the adsorbent material is a solid inorganic or organic non-polymeric or polymeric support material functionalized on the surface with amino functionalities capable of reversibly binding carbon dioxide, having a molecular weight of 10 m 2 / g to 25m 2 The invention has a BET specific surface area in the range of 0.28 cm / g and a cumulative pore volume in the range of 50 nm to 350 nm pore size. 3 / g to 1.5cm 3 / g or 0.3cm 3 / g to 1.5m 3 The pore volume distribution is in the range of 1000 Å / g.

[0023] In fact, one of the unexpected findings of the study is that, in the case of water vapor desorption, there are adsorbent materials suitable for high relative humidity (RH% greater than 60%) and there are adsorbent materials suitable for low relative humidity (RH% in the range of 0% to 60%). The former are characterized by having a maximum relative humidity of up to 10 m 2 / g, while the latter is characterized by having a specific surface area greater than 25m 2 / g specific surface area.

[0024] Surprisingly, on the other hand, if such an adsorbent material (i.e. an adsorbent material based on inorganic or organic non-polymeric or polymeric materials) has a BET specific surface area of ​​10 m 2 / g to 25m 2 / g is within the claimed window, and if such adsorbent material has a cumulative porosity within the window of 50 nm to 350 nm as detailed below, it is found that the carbon dioxide adsorption performance of the corresponding adsorbent material is substantially stable over the entire relative humidity range of 0% to 100% without impaired overall capacity reduction.

[0025] This performance is specific to the case of water vapor desorption. In fact, this unexpectedly stable performance for this type of porosity independent of relative humidity selective capture capacity is not found if the desorption is performed in the absence of water vapor, in particular using a thermal desorption process, as will be demonstrated in further detail below.

[0026] The stable carbon dioxide capture capability for variable relative humidity allows a corresponding stable and controllable high efficiency process independent of relative humidity conditions and a corresponding optimized process control of adsorbent materials based on inorganic or organic non-polymeric or polymeric materials.

[0027] Interestingly, all of these adsorbent materials that behave differently during water vapor desorption, independently of the specific surface area value, have essentially the same carbon dioxide capture performance when used for air purge temperature variations, i.e. when desorption occurs only by heating and not by the introduction of water vapor. The carbon dioxide adsorption of these adsorbent materials under these conditions increases slightly over the entire range for increasing relative humidity. This performance may be due to the increase in amine efficiency at higher RH also described in the literature. In such a process, at each cycle, the adsorbent material is desorbed by heating the bed of adsorbent material (resistive heating) and passing air and / or N2 through the bed.

[0028] In contrast, when the bed of adsorbent material was regenerated by condensing water vapor rather than by inductively heating the bed, a different performance was unexpectedly obtained. Specifically, a completely different dependence on RH% was observed. Adsorbent materials with low surface area performed best at high RH%, while they did not perform well at low RH%. On the other hand, adsorbent materials with high surface area performed well at lower RH%, while they lost capacity at higher RH%.

[0029] On the other hand, the adsorbent material having the claimed characteristics behaves significantly more constant over the relevant RH% range.

[0030] This is due to the special surface and porosity characteristics of the claimed adsorbent material and in particular the presence of a large cumulative pore volume in the region of the larger pores.

[0031] Thus, the present invention relates to adsorbent materials that also have suitable morphology (surface area and preferably also total pore volume and pore size distribution) to operate over a range of RH% without much variation in cyclic CO2 capture capacity, thereby allowing continuous and relatively constant plant operation throughout different times of the day (e.g., humid nights versus dry days) and throughout seasonal changes (hot and humid summers and dry and cold winters).

[0032] The specific characteristics of such adsorbent materials are 10m 2 / g to 25m 2 / g or 10m 2 / g to 20m 2 / g surface area, high pore volume of macropores (especially pore diameter>100nm, pore volume in the range of 50nm to 350nm, 0.28cm 3 / g to 1.5cm 3 / g or 0.3cm 3 / g to 1.5cm 3 / g).

[0033] These adsorbent materials can be polymeric or non-polymeric as their basis. The adsorbent materials can also be organic or inorganic, but mixed forms are also possible. The main characteristic features of these adsorbent materials are not so much chemical properties, but the physical properties of the porous structure.

[0034] In particular, it is shown that if the functionalized solid support of the adsorbent material has a porosity in the range claimed and has a high proportion and volume of macropores (pores with a diameter of more than 50 nm) and further preferably also has a low proportion or is essentially free of mesopores (i.e. pores with a diameter of 2 nm to 50 nm), and / or preferably also has a low proportion or is essentially free of micropores (i.e. pores with a diameter of not more than or less than 2 nm), this achieves a reduced accumulation of condensed water in the pores and, for carbon dioxide capture processes in the presence of water and / or water vapor, a much higher capacity in cyclic operation.

[0035] In the context of the present disclosure, the expressions "ambient atmospheric pressure" and "ambient atmospheric temperature" refer to the pressure and temperature conditions to which the equipment operating outdoors is exposed, i.e. a typical ambient atmospheric pressure represents a pressure in the range of 0.8 bar abs to 1.1 bar abs, and a typical ambient atmospheric temperature refers to a temperature in the range of -40°C to 60°C, more typically -30°C to 45°C. The gas mixture used as input to the process is preferably ambient atmospheric air, i.e. air at ambient atmospheric pressure and at ambient atmospheric temperature, which typically means a CO2 concentration in the range of 0.03% to 0.06% by volume. However, air with a lower or higher CO2 concentration may also be used as input to the process, for example a CO2 concentration of 0.1% to 0.5% by volume, so generally speaking, it is preferred that the input CO2 concentration of the input gas mixture is in the range of 0.01% to 0.5% by volume. However, waste gases may also be the source, in which case the input CO2 concentration of the input gas mixture is typically in the range of up to 20 vol% or up to 12 vol%, preferably in the range of 1 vol% to 20 vol% or 1 vol% to 12 vol%.

[0036] In the sequence of steps (a) to (e) of the carbon dioxide capture process as detailed herein, in steps (a) and (e), reference is made to ambient atmospheric pressure conditions and ambient atmospheric temperature conditions. This only applies if the supply gas mixture is provided under these conditions, for example in the case of direct air capture, where the source of the gas mixture is atmospheric air. However, if the source of the gas mixture is a different source, it is likely that the supply conditions are not ambient atmospheric pressure and / or are not ambient atmospheric temperature conditions. In particular, in the case of exhaust gases, the gas mixture may and often is at an elevated temperature, for example at a temperature above room temperature, which may even be at a temperature above 50°C. The temperature may even rise to 70°C, and in this case, the setting is typically adjusted so that the temperature at which the carbon dioxide is desorbed from the adsorbent material in step (c) is at least 10°C higher, preferably at least 20°C higher, than the temperature of the supply gas. Thus, in step (a) and in step (e) under these non-atmospheric temperature and pressure conditions, typically the pressure and temperature conditions are different, in particular the contacting in step (a) takes place at the temperature and pressure conditions of the supplied gas mixture, whereas in step (e) the adsorbent material is brought to the temperature and pressure conditions of the supplied gas mixture.

[0037] The properties of the ambient atmospheric air to which the adsorbent material is exposed have a strong influence on the performance of amine-based adsorbent materials in terms of both temperature and humidity range. For example, under dry conditions (i.e., relative humidity, RH=0%), amines show an efficiency of 2:1, which is defined as the stoichiometric coefficient of the reaction between the amino group and CO2, while under wet conditions, the efficiency is 1:1. Having a high relative humidity of the gas stream containing carbon dioxide during the adsorption step has benefits on the adsorption capacity (defined as moles of CO2 captured per kilogram of adsorbent). The prior art does not disclose the effect of high relative humidity of the gas stream containing CO2 on the cyclic adsorption / desorption performance when water vapor is used to desorb the adsorbent material.

[0038] More generally, the invention proposes a process for separating gaseous carbon dioxide from a gas mixture, preferably from ambient atmospheric air, comprising said gaseous carbon dioxide and another gas different from gaseous carbon dioxide, by cyclic adsorption / desorption in a unit using an adsorbent material which adsorbs said gaseous carbon dioxide. If reference is made hereinafter to ambient atmospheric air, this also includes other gas mixtures, such as waste gases and biogas.

[0039] The method comprises at least steps (a) to (e) in the following order and repeated in this order:

[0040] (a) contacting said gas mixture, preferably ambient atmospheric air, with an adsorbent material by passing a flow-through through said unit in an adsorption step, preferably under ambient atmospheric pressure conditions (if an aerator or the like is used to push ambient atmospheric air through the apparatus, this is still considered to be ambient atmospheric pressure conditions for the purposes of this application, even if the air pushed through the reactor by the aerator has a pressure slightly above the surrounding ambient atmospheric pressure and that pressure is within the range as detailed above in the definition of "ambient atmospheric pressure") and ambient atmospheric temperature conditions to adsorb at least said gaseous carbon dioxide on the adsorbent material;

[0041] (b) separating the adsorbent material with adsorbed carbon dioxide in the unit from the flowthrough, preferably while substantially maintaining the temperature in the adsorbent material;

[0042] (c) injecting a saturated or superheated water vapor stream by passing the flow through the unit and thereby causing the temperature of the adsorbent material to increase to a temperature of 60° C. to 110° C., thereby initiating the desorption of CO 2 ;

[0043] (d) extracting at least the desorbed gaseous carbon dioxide from the unit and separating the gaseous carbon dioxide from the water vapour by condensation downstream of the unit;

[0044] (e) bringing the adsorbent material to ambient atmospheric temperature conditions (if the adsorbent material is not cooled to exactly ambient atmospheric temperature conditions in this step, this is still considered to be according to this step, preferably the ambient atmospheric temperature established in this step (e) is within the range of ambient atmospheric temperature + 25°C, preferably + 10°C or + 5°C).

[0045] As indicated above, according to the present invention, the adsorbent material is a solid inorganic or organic non-polymeric or polymeric support material functionalized on the surface with amino functionalities capable of reversibly binding carbon dioxide, having a relative humidity of 10 m 2 / g to 25m 2 / g, the BET specific surface area being determined by applying the BET method as described in ISO 9277 and preferably based on nitrogen adsorption measurements. Therefore, BET (Brunauer, Emmett und Teller) surface area analysis is used to determine the BET specific surface area using the method as described in ISO 9277, and having a cumulative pore volume in the range of 50 nm to 350 nm at 0.28 cm 3 / g to 1.5cm 3 / g or 0.3cm 3 / g to 1.5cm 3 The pore volume distribution is in the range of 1000 Å / g.

[0046] According to a first preferred embodiment, the BET specific surface area of ​​the adsorbent material, preferably measured by nitrogen adsorption, is between 10 m 2 / g to 20m 2 / g, preferably within 12 m 2 / g to 20m 2 / g range.

[0047] Further preferably, the adsorbent material has a pore size distribution measured by mercury intrusion such that 90%, preferably 95%, of the pore volume is in the range of 50 nm to 400 nm, preferably in the range of 80 nm to 350 nm. Regarding the parameters for mercury intrusion measurement, reference is made to the details in the description further below.

[0048] Alternatively or additionally, the adsorbent material preferably has a pore volume distribution measured by mercury intrusion porosimetry such that the maximum pore volume is in the range of 80 nm to 150 nm, preferably in the range of 100 nm to 150 nm. The distribution is preferably such that 90%, more preferably 95%, of the total pore volume of the distribution is within a window of -50 nm and +150 nm, preferably -40 nm and +100 nm around the diameter of the maximum of the pore volume distribution.

[0049] According to yet another preferred embodiment, the adsorbent material has a 3 / g to 1cm 3 / g, preferably 0.35cm 3 / g to 0.80cm 3 / g, most preferably within 0.4 cm 3 / g to 0.7cm 3 The total pore volume measured by mercury intrusion porosimetry is in the range of 1000 Å / g.

[0050] The adsorbent material can also be characterized by its nitrogen content. According to another preferred embodiment, the nitrogen content of the adsorbent material is thus in the range of 5% to 50% by weight, preferably in the range of 6% to 15% by weight, or 8% to 15% by weight or 10% to 12% by weight, in each case for dry adsorbent material. Dryness for the purpose of this determination is defined as treating 6 g of adsorbent material at 90° C. for 90 minutes under a flow of 2 L / min of N2.

[0051] As noted above, the process using the particular adsorbent material can be carried out at essentially any practical relative humidity (RH%), but has the advantage that it is particularly suitable and stable under variable relative humidity conditions (i.e., where the RH% is in the range of 20% to 80%).

[0052] The solid inorganic or organic non-polymer or polymer support material of the adsorbent material can be based on organic or inorganic, preferably organic polymer support, such as thermoplastic or thermosetting material. It can also be a thermoplastic material crosslinked in the subsequent steps of the synthesis. The solid polymer support material can be a crosslinked polymer material, such as polystyrene or polyethylene material, which can be crosslinked by using divinylarene, preferably styrene divinylbenzene copolymer (poly (styrene-co-divinylbenzene), PS-DVB). The solid support material can be in the form of beads, which can be monodisperse or polydisperse.

[0053] To introduce, for example, aminomethyl functionality into the PS-DVB backbone, the following reaction pathway can be performed:

[0054]

[0055] In the first step, PS-DVB can be chloromethylated (a) using chloromethyl methyl ether and a catalyst such as AlCl3 to form a chloromethyl group attached to the PS-DVB skeleton. Afterwards, the amino group (b) can be introduced via a reaction with hexamethylenetetramine. As can be seen from the structure in step c, this produces the formation of a quaternary ammonium salt that cannot covalently bind to CO2. In order to have a primary amine that can bind CO2, the intermediate of step c can be hydrolyzed with HCl, which not only produces a primary amine, but also produces an amine reaction via an acid-base reaction, thereby forming ammonium chloride. In order to obtain the final state of the amine as a free base for capture, a final reaction with NaOH can be performed. The final structure of the aminomethyl PS-DVB adsorbent used in the DAC process as further given in the following experimental evidence is shown in step d.

[0056] The solid inorganic or organic non-polymer or polymer support material of the adsorbent material can also be an inorganic non-polymer support, preferably selected from: silica (SiO2), alumina (Al2O3), titanium dioxide (TiO2), magnesium oxide (MgO), clay, and mixed forms thereof, such as silica-alumina (SiO2-Al2O3), or mixtures thereof.

[0057] The solid support material of the adsorbent material may be in the form of hollow or solid particles, beads, microspheres, monolithic structures, sheets, hollow or solid fibers (preferably in the form of woven or non-woven structures) or extrudates.

[0058] The solid inorganic or organic non-polymeric or polymeric support material of the adsorbent material may also be in the form of particles (powder or granules, e.g. with an average size (D50) of 0.002 mm to 4.0 mm) of such support material which may be embedded in a solid matrix in the form of a composite material.

[0059] The adsorbent material is provided by a carrier material functionalized on the surface with amino functionality, and the adsorbent material shows the claimed specific surface area and the claimed pore volume distribution. Such adsorbent materials can present various three-dimensional forms as described, and they can present the form of blocks, layers, sheets, the form of hollow or solid fibers, or the form of particles. For example, when the fiber presents the form of a woven or nonwoven structure, or when the particles are formed into a block structure made of adsorbent material particles, then these structures can also and preferably form or embed in a superstructure without additional elements. However, the superstructure can also include additional structural elements. For example, it can have a laminated structure, and the laminated structure includes a layer of a porous material such as a polymer woven or nonwoven material that is not an adsorbent material itself, and one or more layers of an adsorbent material in the form of a powder or granular structure can be attached to one or both sides of such a layer. Or the layer of the adsorbent material is embedded in two outer layers of a porous material. In the latter preferred case, where the adsorbent material is sandwiched between two or more outer layers of air permeable / porous material, preferably polymeric air permeable / porous material, it may also be in the form of a layer with a semipermeable membrane, which may be soft or hard. These laminates may then be structured to form further superstructures, such as plates with air channels, for example in the form of such laminates with adsorbent arranged in a zigzag or wave pattern. Such plates may then form even higher level superstructures, such as modules with a rigid frame and outer surface covered with a mesh, to provide a structure that can be easily handled and replaced.

[0060] It should be noted that the porosity properties, and therefore the specific surface area and pore volume distribution, but also the total pore volume and other characteristic parameters related to the adsorbent material itself as detailed herein, may and very often are different for the entirety of such a superstructure. Therefore, such a superstructure containing a specific adsorbent material as a whole may and very often have porosity properties different from the claimed scope due to additional layers etc. For the actual carbon dioxide capture properties, however, what is relevant is the specific surface area and pore volume distribution of the embedded adsorbent material, and in such a superstructure the above-mentioned specific surface area and pore volume distribution characteristics (and preferably the additional characteristics as detailed herein) must be met. In particular, if for example there is a laminate according to the invention having an outer non-adsorbent porous layer and a central layer of adsorbent material, the cumulative pore volume due to the contribution of the non-adsorbent layer of the entire structure can be significantly larger than the cumulative pore volume of the embedded adsorbent material alone.

[0061] In the context of this aspect of the invention, when referring to a solid matrix of a solid inorganic or organic non-polymeric or polymeric support material forming a composite material, this means that the solid matrix does provide the actual three-dimensional structure of the solid inorganic or organic non-polymeric or polymeric support material forming the adsorbent material itself (however, it does not exclude that the adsorbent material is embedded in or attached to further structural elements that do not contribute to carbon dioxide capture). This aspect may include the following: wherein a separate structure provides the actual support, which is then coated, impregnated or soaked with a binder to form a composite solid matrix with adsorbent material particles and subsequently dried, cross-linked or cured in another way; and wherein the binder provides adhesion of the adsorbent material particles to the actual support and / or forms a coating on the support together with the adsorbent material particles.

[0062] Preferably, such a composite material formed only of a solid matrix and particles of adsorbent material may be in the form of a sheet or foil, but granular or block structures are also possible. These elements providing solid inorganic or organic non-polymeric or polymeric composites may be mounted in or on a corresponding support structure, such as some kind of frame etc. for the actual carbon dioxide capture process.

[0063] In particular, foils or sheets of such composite materials of solid inorganic or organic non-polymeric or polymeric support materials containing adsorbent materials can be obtained by extrusion, wherein said particles of adsorbent material, for example functionalized on the surface, are added, for example, to a thermoplastic matrix material after its melting and before thermoforming. This can be done by melt mixing or solution casting, but also by sputtering particles of adsorbent material onto a liquid or at least surface softened layer of thermoplastic material of the solid matrix, followed, if desired, by a lamination process between rollers.

[0064] Alternatively, a solid matrix precursor material may be used to which particles of the adsorbent material are added, mixed, and then the material cured, for example in a cross-linking, sintering or drying process, to produce, for example, a thermoset structure.

[0065] Preferably in such processes involving heating it is ensured that the residence time of the adsorbent material particles in the molten or precursor material is sufficiently short to avoid degradation of the surface and / or porosity properties and / or functionalisation of the particles.

[0066] Furthermore, the actual adsorber structure can be produced starting from the adsorbent material particles in a sintering process, for example by bringing the adsorbent material particles into the corresponding desired three-dimensional shape (for example in the case of a resulting foil, into the form of a layer of substantially the desired thickness), and then heating and / or irradiating and / or chemically treating the corresponding structure analogously to the sintering process in order to produce a coherent macroscopic adsorber structure. This applies in particular to adsorbent materials based on organic thermoplastic polymer materials. However, it is also possible for other materials, for example, if these materials are provided on the surface with corresponding binders which allow such a sintering process. Such sintering can be assisted by slight pressing, for example in a lamination process.

[0067] The solid matrix can also be the same or different solid inorganic or organic non-polymeric or polymeric support material functionalized on the surface with amino functionalities, even itself having the surface and porosity properties as defined above. However, it can also be a material different from one of the particles and not having carbon dioxide capture properties and / or whose matrix does not have the surface area and porosity properties as defined above. Preferably, in this case, the solid matrix is ​​a material different from the adsorbent material particles: it has no surface functionalization but is preferably porous and wherein the adsorbent material particles are exposed on the surface with their functionalized surface capable of acting as carbon dioxide capture moieties.

[0068] Furthermore, such composite materials having adsorbent material particles embedded in a solid matrix may be in the form of hollow or solid particles, beads, microspheres, bulk structures, sheets, hollow or solid fibers (preferably in woven or nonwoven structures), webs, or extrudates.

[0069] The corresponding powder to be embedded in the matrix can be obtained by milling or grinding a particulate resin material which has been surface-functionalized.

[0070] The thickness of such a sheet or foil is preferably in the range of 0.01 mm to 5 mm or 0.05 mm to 3 mm, preferably in the range of 0.1 mm to 1 mm, for the envisaged DAC application to provide the required mechanical properties.

[0071] In order to withstand the conditions of a typical DAC process, it is further preferred that the solid matrix material with embedded adsorbent material particles and / or the solid inorganic or organic non-polymeric or polymeric support material forming the composite structure generally does not lose, or at least does not significantly lose, its mechanical properties under typical DAC process conditions to an extent that the performance of the DAC process is impaired.

[0072] Thus, in general, in the case of amorphous thermoplastic polymer materials, which are usually used for solid matrix or carrier materials, the glass transition temperature should be above 100° C., and in the case of thermoplastic systems with a melting point, the melting point should be above 100° C. On the other hand, in particular with regard to particles which are already functionalized when combined with the matrix, and very particularly with regard to such polymer particles (e.g. based on polystyrene) which are functionalized on the surface, the matrix material should not have too high a processing temperature, since otherwise the polymer particles would also melt during melt mixing and / or the surface functionalization of the particles would be destroyed. With this in mind, the matrix material and / or the carrier material of the adsorbent material should, in the case of amorphous thermoplastic polymer materials, generally preferably have a glass transition temperature of less than 180° C. Thus, in the case of amorphous thermoplastic polymer materials, preferably the glass transition temperature is in the range of 120° C. to 160° C., more preferably in the range of 130° C. to 150° C. In the case of matrix systems and / or carrier materials which usually have a melting point (e.g. microcrystalline or partially crystalline polymer systems), the melting point or softening point should be in the same temperature range, thus it should be above 100° C. and / or below 180° C., preferably in the range of 120° C. to 160° C., more preferably in the range of 130° C. to 150° C. In this context, the glass transition temperature and the melting temperature are to be regarded as measured in accordance with DIN EN ISO 11357 (2012). Amorphous in the sense of the present invention means that the system has a melting enthalpy determined in accordance with ISO 11357 (2012) of less than or equal to 3 J / g.

[0073] It should be noted and emphasized again that the surface area properties and porosity properties described above should be considered as far as they are relevant to the carbon dioxide capture process. Thus, if for example the matrix material is permeable to carbon dioxide, the composite material may have a porosity and / or surface area structure that is not within the ranges as required and as given above, as this is primarily determined by the solid matrix material. However, the adsorbent material particles embedded in such a material do have a porosity and / or surface area structure as defined above, and these properties can be used in the carbon dioxide capture process due to the fact that the matrix material is permeable to carbon dioxide and allows capture active particles to be obtained by diffusion.

[0074] Thus, such a composite structure can be produced, for example, by mixing particles of the adsorbent material with a solid matrix material or a precursor thereof, and subsequently curing and / or extruding. Thus, the solid matrix material can, for example, be a thermoplastic material or a material that only cures after mixing during processing, for example during crosslinking or drying or sintering.

[0075] In this case, the surface functionalization for CO2 capture can be carried out before or after mixing and forming the corresponding composite material. For example, it can also be a process in which non-functionalized particles and matrix materials are mixed, a corresponding porous composite structure with the desired porosity properties is produced, and the solid composite structure is subsequently functionalized on the surface of the embedded particles with amino functionalities. This has the advantage that matrix materials that cannot be functionalized in the composite material can be combined with particles that can be functionalized, first producing a composite material and the composite material only subsequently and only on the corresponding available surfaces of the particles functionalized with amino functionalities as defined above. The particles embedded in the composite material are regarded as adsorbent materials in the above sense.

[0076] Such a solid support is preferably surface functionalized to form an absorbent material, wherein preferably the surface functionalization produces an amine group that can be used for reversible carbon dioxide capture, wherein the surface functionalization can be achieved by impregnation or by grafting with a surface material of the solid support, or a combination thereof. The surface functionalization is preferably provided with an aminomethyl moiety, such as a benzylamino moiety, wherein the solid polymer support material is preferably obtained during suspension polymerization. By adjusting the reactants and reaction conditions, emulsion polymerization can be effectively used to establish a porosity within the claimed scope, and preferably, suspension polymerization is carried out in water with or without a surfactant (such as dimethyl dioctadecyl ammonium chloride), preferably in the presence of a pore-forming agent, the pore-forming agent can be isooctane, toluene, wax or a mixture thereof. But other methods and reagents are also possible. Functionalization can be achieved, for example, by phthalimide addition or chloromethylation. Preferably, the primary amine moiety presents the form of a terminal aminomethyl group, such as the form of the above-mentioned benzylamine moiety. For carbon dioxide capture, according to current knowledge, primary amines are converted into aminoformic acid compounds, which dissociate at high temperatures and / or humidity for releasing carbon dioxide.

[0077] The solid inorganic or organic non-polymeric or polymeric support material may be a polymeric support material in the form of at least one of a block (typically with a sponge-like structure for the gas mixture / ambient air to flow through), a layer or a plurality of layers, a sheet, a hollow or solid fiber (e.g. in a woven or non-woven (layer) structure), but may also be in the form of hollow or solid particles (beads). Preferably, it is in the form of preferably substantially spherical beads, with a particle size (D50) in the range of 0.002 mm to 4 mm, 0.005 mm to 2 mm or 0.01 mm to 1.5 mm, preferably in the range of 0.30 mm to 1.25 mm. Particles with a particle size (D50) in the range of 0.002 mm to 1.5 mm, 0.005 mm to 1.6 mm are also possible.

[0078] In this unit, if the adsorbent material is in the form of beads or powder in the range of 0.002 mm to 4 mm, it can be contained in a layered structure / container having a gas permeable side wall in the form of a film, metal mesh, etc., the latter typically having a mesh width that is large enough to provide a low pressure drop across the corresponding structure, but small enough to ensure that the particles of the adsorbent material are retained in the corresponding container.

[0079] The adsorbent material may have a water retention rate in the range of 3 weight percent to 60 weight percent, preferably in the range of 3 weight percent to 30 weight percent or 5 weight percent to 30 weight percent. In this case, the water retention rate is determined using a moisture analyzer that heats the adsorbent material to 110° C. until a weight change detected is no greater than 0.002 g / 15 seconds.

[0080] In addition, the adsorbent material may have a 3 Up to 400kg / m 3 , preferably 450kg / m 3 Up to 650kg / m 3 The bulk density is within the range of EN ISO 60 (DIN 53468).

[0081] The extraction step (d) is preferably carried out while the adsorbent material is still in contact with water vapour by injecting and / or circulating saturated or superheated water vapour into the unit, so as to flush and purge both water vapour and CO2 from the unit, and preferably the extraction and / or the water vapour supply are simultaneously regulated so as to substantially maintain the temperature in the adsorbent at the end of the previous step (c) and / or so as to substantially maintain the pressure in the adsorbent at the end of the previous step (c). "Substantially maintaining the pressure in the adsorbent at the end of the previous step" means in practice that the pressure is not allowed to deviate by more than ±100 mbar, preferably by more than ±50 mbar, more preferably by more than ±20 mbar from the pressure at the end of step (c). In practice, certain very short time deviations may occur even exceeding this range due to the process of pressure equalisation after the transition from step c) to d), which time deviations depend on the exact implementation of the equipment used to carry out the process. However, they are of short duration, approximately less than 15% of the duration of step d).

[0082] For carrying out the process, preferably a unit comprising said adsorbent material is used, which unit and the adsorbent material are capable of maintaining a temperature of at least 60° C. for the desorption of at least said gaseous carbon dioxide and which unit is openable for the flow of a gas mixture / ambient atmospheric air through it and for contacting the gas mixture / ambient atmospheric air with the adsorbent material for the adsorption step.

[0083] The unit used may comprise an array of individual adsorber elements, each of which comprises at least one carrier layer and at least one adsorbent layer, the at least one adsorbent layer comprising or consisting of at least one adsorbent material, wherein the adsorbent material provides for selective adsorption of CO2 in the presence of moisture or water vapor, wherein the adsorber elements in the array may be arranged substantially parallel to each other and spaced apart from each other, thereby forming parallel fluid channels for the flow of the gas mixture / ambient atmospheric air and / or water vapor. In this context, substantially parallel means that the angle between the planes of the adsorber elements does not exceed a value of 10°, preferably does not exceed a value of 5°, preferably is less than 2°, when observed over the entire length of the adsorber elements. In this context, individual adsorber elements mean that the adsorber elements are not monolithic structures, but can be arranged independently of each other to form substantially parallel channels of an array, wherein the layers are connected to each other with corresponding connecting structures, for example by a frame, into which the layers are inserted, or on which the layers are fixed, or on which the carrier layers can be repeatedly pleated at the desired spacing.

[0084] The unit is preferably capable of being evacuated to a vacuum pressure of 400 mbar (abs) or less, and step (b) may comprise separating the adsorbent with adsorbed carbon dioxide in the unit from the flowthrough while maintaining the temperature in the adsorbent, and then evacuating the unit to a pressure in the range of 20 mbar (abs) to 400 mbar (abs), wherein in step (c) the injection of a saturated or superheated water vapor flow also causes an increase in the internal pressure of the reactor unit, and wherein step (e) comprises bringing the adsorbent material to ambient atmospheric pressure conditions and ambient atmospheric temperature conditions.

[0085] Preferably, after step (d) and before step (e), the following steps are performed:

[0086] (d1) stopping the injection of water vapor and, if used, the circulation of water vapor, and evacuating the unit to a pressure value in the unit in the range of 20 mbar (abs) to 500 mbar (abs), preferably in the range of 50 mbar (abs) to 250 mbar (abs), thereby evaporating water from the adsorbent and not only drying the adsorbent but also cooling the adsorbent.

[0087] Step (e) is preferably carried out simply by contacting said ambient atmospheric air with the adsorbent material under ambient atmospheric pressure conditions and ambient atmospheric temperature conditions to evaporate and carry away water in the unit and to bring the adsorbent material to ambient atmospheric temperature conditions.

[0088] After step (b) and before step (c), the following steps may be performed:

[0089] (b1) flushing the unit with a non-condensable gas of a non-condensable water vapour stream whilst substantially maintaining the pressure of step (b), preferably maintaining the pressure of step (b) within a window of ±50 mbar, preferably within a window of ±20 mbar, and / or maintaining the temperature below 75°C or 70°C or below 60°C, preferably below 50°C.

[0090] In another embodiment of step b1, the temperature of the adsorber structure is increased from the conditions of step (a) to a temperature in the range of 80 to 110°C, preferably in the range of 95 to 105°C.

[0091] In step (b1), while maintaining the pressure of step (b1), the unit can be preferably flushed with saturated water vapor or water vapor superheated up to 20°C at a water vapor rate of 1 kg / hour to 10 kg / hour per liter volume of adsorber structure to purge the remaining gas mixture / ambient air of the reactor. The purpose of removing this part of the ambient air is to increase the purity of the captured CO2.

[0092] In step (c), water vapour may be injected in the form of water vapour introduced via the respective inlet of the unit, and water vapour may be (partially or completely) recycled from the outlet of the unit to the inlet, preferably including reheating of the recycled water vapour, or by reuse of water vapour from a different reactor.

[0093] It should be noted that the heating in step (c) for desorption according to the process is achieved only by the water vapor injection and there is no additional external or internal heating (eg by pipes with hot fluid).

[0094] In step (c), the adsorbent material may further preferably be heated to a temperature in the range of 80°C to 110°C or 80°C to 100°C, preferably to a temperature in the range of 85°C to 98°C.

[0095] According to yet another preferred embodiment, in step (c), the pressure in the unit is in the range of 700 mbar (abs) to 950 mbar (abs), preferably in the range of 750 mbar (abs) to 900 mbar (abs).

[0096] Furthermore, the present invention relates to the use of an adsorbent material for direct air capture, in particular using a temperature, vacuum, or temperature / vacuum swing process, the adsorbent material having a solid inorganic or organic non-polymeric or polymeric support material functionalized on the surface with amino functionalities capable of reversibly binding carbon dioxide, having a carbon dioxide absorption capacity of 10 m / s. 2 / g to 25m 2 / g in the range of 0.28 cm-1 and 0.30 cm-1, preferably in the range of 1.20 cm-1 and 1.50 cm-1, and preferably in the range of 2.50 cm-1 and 3.50 cm-1. 3 / g to 1.5cm 3 The pore volume distribution is preferably measured by Hg pressure in the range of 1000 Å / g.

[0097] This uses a process where a saturated or superheated water vapour stream is injected through the flow through to cause the temperature of the adsorbent material to increase to a temperature of 60°C to 110°C, thereby initiating desorption of CO2.

[0098] Preferably, the adsorbent material for this use is characterized as detailed above with respect to pore size, pore volume, and / or nitrogen content.

[0099] Last but not least, the present invention relates to a direct air capture plant comprising at least one reactor unit comprising an adsorbent material suitable and adapted to flow through a gas mixture, preferably ambient air,

[0100] wherein the reactor unit comprises an inlet for the gas mixture / ambient air during adsorption and an outlet for the gas mixture / ambient air,

[0101] wherein the reactor unit is heatable to a temperature of at least 60° C. for desorption of at least said gaseous carbon dioxide and the reactor unit is openable for the flow of a gas mixture / ambient atmospheric air through and for contacting the gas mixture / ambient atmospheric air with the adsorbent material for the adsorption step, wherein preferably the reactor unit is also evacuable to a vacuum pressure of 400 mbar (abs) or less,

[0102] The adsorbent material is preferably in the form of an adsorber structure comprising an array of individual adsorber elements, each adsorber element preferably comprising at least one carrier layer and at least one adsorbent material layer, the at least one adsorbent material layer comprising or consisting of at least one adsorbent material, wherein the adsorbent material comprises a solid inorganic or organic non-polymeric or polymeric carrier material functionalized on the surface with amino functionalities capable of reversibly binding carbon dioxide, having a carbon dioxide content of 10 m / s. 2 / g to 25m 2 / g in the range of 0.28 cm-1 and 0.30 cm-1, preferably in the range of 1.20 cm-1 and 1.50 cm-1, and preferably in the range of 2.50 cm-1 and 3.50 cm-1. 3 / g to 1.5cm 3 / g, preferably measured by pressure Hg, which provides selective adsorption of CO2 in the presence of moisture or water vapor, wherein preferably, the adsorber elements in the array are arranged substantially parallel to each other and spaced apart from each other so as to form parallel flow channels for the gas mixture / ambient atmospheric air and / or water vapor to flow through,

[0103] at least one device for separating carbon dioxide from water, preferably a condenser,

[0104] Preferably, at the gas outlet side of the device for separating carbon dioxide from water, preferably the condenser, there is at least one of a carbon dioxide concentration sensor and a gas flow sensor, preferably both, for controlling the desorption process.

[0105] The application also relates to methods for producing surface-functionalized solid support materials suitable and adaptable for these processes, in particular including surface impregnation or grafting for surface functionalization.

[0106] Further embodiments of the invention are set forth in the dependent claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0107] Preferred embodiments of the present invention are described below with reference to the accompanying drawings, which are for the purpose of illustrating the present preferred embodiments of the present invention and not for the purpose of limiting the same. In the accompanying drawings,

[0108] Figure 1 A schematic diagram of a direct air capture device is shown;

[0109] Figure 2 shows the pore size distribution measured by Hg porosimetry;

[0110] Figure 3 The pore volume is shown as a function of the pore size measured by Hg pressure;

[0111] Figure 4 The equilibrium adsorption capacity of the adsorbent after desorption with an air purge temperature swing at 94°C using an air flow rate of 2 L / min and 60% RH at 30°C is shown;

[0112] Figure 5 The cyclic adsorption capacity of the adsorbent after water vapor desorption at different RH using a gas stream containing 450 ppm CO2 with a volume flow rate of 11 L / min and at 15°C is shown;

[0113] Figure 6 Shown are the cyclic adsorption capacities of the adsorbents after desorption with an air purge temperature swing at 94°C at different RH using an air flow rate of 2 L / min at 30°C. DETAILED DESCRIPTION

[0114] The presented adsorbent material can be produced using the following method:

[0115] For the general reaction scheme for the introduction of aminomethyl functionality into the PS-DVB backbone, reference is made to the schemes given further in this disclosure.

[0116] The morphology of the PS-DVB beads can be controlled by the amount of DVB in the monomer phase and the amount and type of porogen. Generally speaking, at a constant type and amount of porogen, a larger amount of DVB produces a larger specific surface area. On the other hand, a larger amount of porogen produces a larger pore size and a lower specific surface area. In order to obtain a specific morphology (e.g., surface area, pore volume, and pore size), the optimal value between the amount of DVB, the amount of porogen, and the type of porogen is adjusted.

[0117] The different porosities in Examples IER_A to IER_D given below were determined using these criteria.

[0118] Steps for synthesizing IER_A:

[0119] In a 1L reactor, 1% (mass ratio) of gelatin and 2% (mass ratio) of sodium chloride were dissolved in 350mL water at 45°C for 1 hour. In another flask, 1g of benzoyl peroxide was dissolved in a mixture of 55.4g of styrene, 8.2g of divinylbenzene (content 80%) and 52.6g of C11-C13 isoparaffins. The resulting mixture was then added to the reactor. Afterwards, the reaction mixture was stirred and heated to 70°C, maintained at this temperature for 2 hours, then the temperature was raised to 80°C, and maintained for 3 hours, and then raised to 90°C for 6 hours. The reaction mixture was cooled to room temperature, and beads were filtered out using a glass funnel filter and vacuum suction. The beads were washed with toluene and dried in a rotary evaporator.

[0120] The polystyrene-divinylbenzene beads were functionalized using chloromethylation. 5 g of the beads thus obtained were added to a 3-necked flask containing 50 mL of chloromethyl methyl ether. The mixture was stirred for 1 hour, 2 g of zinc chloride was added, and heated to 40 ° C and kept for 24 hours. Afterwards, the beads were filtered out and washed with 25% HCl and water to obtain chloromethylated beads. In order to obtain the benzylamine unit, the following steps were used to aminize the chloromethylated beads. The chloromethylated beads were added to a three-necked flask with 27 g of methylal, and the mixture was stirred for 1 hour. To the mixture, 16 g of hexamethylenetetramine and 13 g of water were added and kept at a gentle reflux for 24 hours. The beads were filtered out and washed with water. In order to have primary amines, a hydrolysis step is required, followed by alkali treatment. The beads were placed in a 3-necked flask containing 140 mL of hydrochloric acid (30%)-ethanol (95%) (volume ratio 1:3), and the reaction mixture was heated to 80 ° C and kept at this temperature for 20 hours. Afterwards, the beads were filtered off and washed with water. At this stage, the amine was protonated and, in order to release the base, the beads were treated with 50 mL of 2M NaOH solution and stirred at 80° C. for 1 hour. The aminated beads were filtered off and washed with demineralized water to neutral pH.

[0121] Steps for synthesizing IER_B:

[0122] In a 1L reactor, 1% (mass ratio) of gelatin and 2% (mass ratio) of sodium chloride were dissolved in 340mL water at 45°C for 1 hour. In another flask, 1g of benzoyl peroxide was dissolved in a mixture of 59.7g of styrene, 3.9g of divinylbenzene (content 80%) and 65.3g of C11-C13 isoparaffins. The resulting mixture was then added to the reactor. Afterwards, the reaction mixture was stirred and heated to 70°C, maintained at this temperature for 2 hours, then the temperature was raised to 80°C, and maintained for 3 hours, and then raised to 90°C for 6 hours. The reaction mixture was cooled to room temperature, and beads were filtered out using a glass funnel filter and vacuum suction. The beads were washed with toluene and dried in a rotary evaporator.

[0123] The polystyrene-divinylbenzene beads were functionalized using chloromethylation. 5 g of the beads thus obtained were added to a 3-necked flask containing 50 mL of chloromethyl methyl ether. The mixture was stirred for 1 hour, 2 g of zinc chloride was added, and heated to 40 ° C and kept for 24 hours. Afterwards, the beads were filtered out and washed with 25% HCl and water to obtain chloromethylated beads. In order to obtain the benzylamine unit, the following steps were used to aminize the chloromethylated beads. The chloromethylated beads were added to a three-necked flask with 27 g of methylal, and the mixture was stirred for 1 hour. To the mixture, 16 g of hexamethylenetetramine and 13 g of water were added and kept at a gentle reflux for 24 hours. The beads were filtered out and washed with water. In order to have primary amines, a hydrolysis step is required, followed by alkali treatment. The beads were placed in a 3-necked flask containing 140 mL of hydrochloric acid (30%)-ethanol (95%) (volume ratio 1:3), and the reaction mixture was heated to 80 ° C and kept at this temperature for 20 hours. Afterwards, the beads were filtered off and washed with water. At this stage, the amine was protonated and, in order to release the base, the beads were treated with 50 mL of 2M NaOH solution and stirred at 80° C. for 1 hour. The aminated beads were filtered off and washed with demineralized water to neutral pH.

[0124] Steps for synthesizing IER_C:

[0125] In a 1L reactor, 1% (mass ratio) of gelatin and 2% (mass ratio) of sodium chloride were dissolved in 340mL water at 45°C for 1 hour. In another flask, 1g of benzoyl peroxide was dissolved in a mixture of 58.8g of styrene, 4.9g of divinylbenzene (content 80%) and 63.2g of C11-C13 isoparaffins. The resulting mixture was then added to the reactor. Afterwards, the reaction mixture was stirred and heated to 70°C, maintained at this temperature for 2 hours, then the temperature was raised to 80°C, and maintained for 3 hours, and then raised to 90°C for 6 hours. The reaction mixture was cooled to room temperature, and beads were filtered out using a glass funnel filter and vacuum suction. The beads were washed with toluene and dried in a rotary evaporator.

[0126] The polystyrene-divinylbenzene beads were functionalized using chloromethylation. 5 g of the beads thus obtained were added to a 3-necked flask containing 50 mL of chloromethyl methyl ether. The mixture was stirred for 1 hour, 2 g of zinc chloride was added, and heated to 40 ° C and kept for 24 hours. Afterwards, the beads were filtered out and washed with 25% HCl and water to obtain chloromethylated beads. In order to obtain the benzylamine unit, the following steps were used to aminize the chloromethylated beads. The chloromethylated beads were added to a three-necked flask with 27 g of methylal, and the mixture was stirred for 1 hour. To the mixture, 16 g of hexamethylenetetramine and 13 g of water were added and kept at a gentle reflux for 24 hours. The beads were filtered out and washed with water. In order to have primary amines, a hydrolysis step is required, followed by alkali treatment. The beads were placed in a 3-neck flask containing 140 mL of hydrochloric acid (30%)-ethanol (95%) (volume ratio 1:3), and the reaction mixture was heated to 80 ° C and kept at this temperature for 20 hours. Afterwards, the beads were filtered off and washed with water. At this stage, the amine was protonated and, in order to release the base, the beads were treated with 50 mL of 2M NaOH solution and stirred at 80° C. for 1 hour. The aminated beads were filtered off and washed with demineralized water to neutral pH.

[0127] Steps for synthesizing IER_D:

[0128] In a 1L reactor, 1% (mass ratio) of gelatin and 2% (mass ratio) of sodium chloride were dissolved in 340mL water at 45°C for 1 hour. In another flask, 1g of benzoyl peroxide was dissolved in a mixture of 57.8g of styrene, 5.86g of divinylbenzene (content 80%) and 63.84g of C11-C13 isoparaffins. The resulting mixture was then added to the reactor. Afterwards, the reaction mixture was stirred and heated to 70°C, maintained at this temperature for 2 hours, then the temperature was raised to 80°C, and maintained for 3 hours, and then raised to 90°C for 6 hours. The reaction mixture was cooled to room temperature, and beads were filtered out using a glass funnel filter and vacuum suction. The beads were washed with toluene and dried in a rotary evaporator.

[0129] The polystyrene-divinylbenzene beads were functionalized using chloromethylation. 5 g of the beads thus obtained were added to a 3-necked flask containing 50 mL of chloromethyl methyl ether. The mixture was stirred for 1 hour, 2 g of zinc chloride was added, and heated to 40 ° C and kept for 24 hours. Afterwards, the beads were filtered out and washed with 25% HCl and water to obtain chloromethylated beads. In order to obtain the benzylamine unit, the following steps were used to aminize the chloromethylated beads. The chloromethylated beads were added to a three-necked flask with 27 g of methylal, and the mixture was stirred for 1 hour. To the mixture, 16 g of hexamethylenetetramine and 13 g of water were added and kept at a gentle reflux for 24 hours. The beads were filtered out and washed with water. In order to have primary amines, a hydrolysis step is required, followed by alkali treatment. The beads were placed in a 3-neck flask containing 140 mL of hydrochloric acid (30%)-ethanol (95%) (volume ratio 1:3), and the reaction mixture was heated to 80 ° C and kept at this temperature for 20 hours. Afterwards, the beads were filtered off and washed with water. At this stage, the amine was protonated and, in order to release the base, the beads were treated with 50 mL of 2M NaOH solution and stirred at 80° C. for 1 hour. The aminated beads were filtered off and washed with demineralized water to neutral pH.

[0130] The beads according to the examples were tested in an experimental setup where the beads were contained in a packed bed reactor or a gas permeable layer. Figure 1 The device is schematically shown in FIG. There is an ambient air inflow structure 1, and the actual reactor unit 8 comprises a container or wall 7 in which a layer of adsorbent material 3 is located. There is an inflow structure 4 for desorption and, if, for example, water vapor is used for desorption, there is a reactor outlet 5 for extraction. Furthermore, there is a vacuum unit 6 for evacuating the reactor.

[0131] For adsorption measurements using dry gas to desorb the adsorbent, 6 g of dry sample was loaded into a cylinder with an inner diameter of 40 mm and a height of 40 mm and placed in a CO adsorption / desorption apparatus, where it was exposed to a 2.0 NL / min air flow containing 450 ppmv CO at 30° C. with relative humidity of 20%, 40%, 60% and 80% for a duration of 600 minutes. Prior to adsorption, the adsorbent bed was desorbed by heating the adsorbent to 94° C. using an air flow of 2.0 NL / min. The amount of CO adsorbed on the adsorbent was determined by integrating the infrared sensor signal measuring the CO content in the air flow leaving the cylinder.

[0132] For the adsorption measurements using water vapor to desorb the adsorbent, 15 g of dry sample were loaded into a square reactor with an inner diameter of 60 mm and a height of 60 mm and placed in a CO2 adsorption / desorption apparatus, where it was exposed to 11 NL / min of air streams containing 450 ppmv CO2 at 15°C with relative humidity of 20%, 40%, 60% and 80% for a duration of 600 minutes. Before adsorption, the adsorbent bed was brought to 200 mbar abs, then 3 mL / min of water vapor was injected into the reactor to reach a temperature in the adsorbent bed of about 95°C, at which the adsorbent was kept for 6 minutes. Afterwards, the reactor was closed and the pressure was set to 200 mbar abs, after reaching the target pressure, the reactor was re-pressurized to atmospheric pressure. The amount of CO2 adsorbed on the adsorbent was determined by the integration of the infrared sensor signal measuring the CO2 content in the air stream leaving the reactor. Specific embodiment:

[0134] In this Examples section, four samples were analyzed and compared: one with a high surface area, with a BET surface area of ​​>25 m2 / g, hereinafter referred to as the high surface area polymer (IER_A); and a second with a low surface area, <25 m2 / g. 2 / g, which is referred to as low surface area polymer (IER_B) hereinafter.

[0135] Two samples with the same basic structure but with the best surface area and porosity distribution, namely IER_C and IER_D, were further analyzed.

[0136] Pore ​​size, pore volume and specific surface area of ​​adsorbent:

[0137] Method used for specific surface area measurement:

[0138] Nitrogen adsorption measurements were performed on Quantachrome ASiQ at 77K. The mass of the sample used was 0.2g to 1.0g. Since the sample contains a large amount of water, it is important to use a treatment that does not change its inherent porosity and pore structure. Therefore, before degassing, the sample is treated using the elutropicrow method, which involves removing water and replacing it with organic solvents with lower boiling points in the following order: methanol, acetone and n-heptane. 2g of sample is placed in a chromatographic column with a frit and rinsed with 20cm3 of each solvent in order of decreasing polarity. The sample is then spread out in a petri dish and placed in a vacuum oven at 40°C for 24 hours. Afterwards, the sample is degassed under vacuum at 70°C for twelve hours before measurement.

[0139] The BET (Brunauer, Emmett und Teller) surface area analysis was used according to method ISO 9277.

[0140] The results of the specific surface area measurements are given in Table 1 below.

[0141] Sample ID <![CDATA[SBET / m 2 g -1 ]]> IER_A 44.2 IER_B 8.8 IER_C 13 IER_D 19

[0142] Table 1: Specific surface areas calculated and determined by N2 adsorption measurements using the BET method.

[0143] Mercury porosimetry measures:

[0144] Mercury porosimetry measurements were performed to analyze pore size and pore volume that were not available through N2 adsorption measurements. To perform the mercury porosimetry measurements, the following parameters were used:

[0145] Mercury surface tension: 0.48N / m

[0146] Mercury contact angle: 150°

[0147] Maximum pressure: 400MPa

[0148] Increase speed: 6MPa / min to 19MPa / min

[0149] Prior to Hg porosimetry, the samples were degassed at 70 °C under vacuum for 12 h.

[0150] The results of the Hg porosimetry analysis are presented in Figure 2 and Figure 3 and are summarized in Table 2 below:

[0151]

[0152] Table 2: Porosity data obtained by Hg porosimetry

[0153] Elemental Analysis:

[0154] Elemental analysis of the materials was performed using a LECO CHN-900 combustion furnace. Prior to measurement, the samples were ground in a mortar and treated at 90° C. under a N 2 flow (2 L / min) for 2 hours.

[0155] The analysis results of the materials are summarized in Tables 3 to 6.

[0156]

[0157] Table 3. Elemental analysis results of IER_A

[0158] element Nr.1 / weight% Nr.2 / weight% Average value / weight% C 78.59 78.56 78.58 H 8.26 8.25 8.26 N 10.88 10.99 10.94

[0159] Table 4. Elemental analysis results of IER_B

[0160] element Nr.1 / weight% Nr.2 / weight% Average value / weight% C 81.05 81.08 81.07 H 8.16 8.17 8.17 N 9.37 9.12 9.25

[0161] Table 5. Elemental analysis results of IER_C

[0162] element Nr.1 / weight% Nr.2 / weight% Average value / weight% C 77.90 77.85 77.88 H 8.04 8.16 8.10 N 8.70 8.69 8.70

[0163] Table 6. Elemental analysis results of IER_D

[0164] Adsorption measurements:

[0165] 6 g of dry sample are loaded into a cylinder with an inner diameter of 40 mm and a height of 40 mm and placed in a CO2 adsorption / desorption device, where it is exposed to a flow of 2.0 NL / min of air containing 450 ppmv CO2 at 30°C with a relative humidity of 60% corresponding to a temperature of 30°C for a duration of 600 minutes. Prior to adsorption, the adsorbent bed is desorbed by heating the adsorbent to 94°C under an air flow of 2.0 NL / min. The amount of CO2 adsorbed on the adsorbent is determined by integrating the signal of an infrared sensor measuring the CO2 content in the air flow leaving the reactor. Figure 4 The CO2 equilibrium capacities at 30°C and 60% RH are shown in FIG. As we can see, the IER_B adsorbent exhibits the largest CO2 cumulative capacity (1.7 mmol / g) compared to the other adsorbents that exhibit equilibrium capacities ranging from 1.1 mmol / g to 1.3 mmol / g. The difference in equilibrium capacity is due to the different amine loadings in the samples, as evidenced by the different nitrogen contents of the adsorbents (see Tables 3 to 6). If the RH of the inlet gas is varied between 20% and 80%, all adsorbents show a linear increase in cyclic CO2 capacity, as shown in FIG. Figure 6 This behavior is consistent with what is known about the RH dependence of amine-based adsorbents.

[0166] The results of the CO2 adsorption measurements are summarized in Table 7.

[0167] Sample ID <![CDATA[Cumulative CO2 capacity per g of dry adsorbent / mmol C O 2]]> IER_A 1.1 IER_B 1.7 IER_C 1.2 IER_D 1.3

[0168] Table 7: Cumulative CO2 adsorption capacity of adsorbents

[0169] Cyclic adsorption / desorption measurements:

[0170] The cyclic adsorption / desorption capacity was measured in a continuous operation at a relative humidity of the ambient air in the range of 20% to 80%. The desorption process was carried out using a warm fluid to increase the temperature of the adsorbent. In this specific example, saturated water vapor was used. The adsorbent bed was first subjected to adsorption for 200 minutes using ambient air. After the adsorption was completed, the pressure of the system was reduced to 200 mbar abs. Once this pressure was reached, saturated water vapor was supplied to the adsorbent bed until a temperature of about 95°C was reached. Afterwards, the adsorbent was brought to 200 mbar abs until a temperature of 60°C was reached. This cycle was repeated several times and the results are shown in Figure 5 middle.

[0171] Figure 6 Results of a similar experiment are shown, but in this case the desorption process was carried out using an air flow of 2.0 NL / min by heating the adsorbent to 94° C. This cycle was repeated multiple times.

[0172] By applying water vapor to desorb the adsorbent and using air in the RH range of 20 to 80%, the desorption capacity of IER_A shows a constant decrease in the cyclic adsorption / desorption capacity, while IER_B shows a constant increase in the cyclic adsorption / desorption capacity until it becomes constant at RH about 80%. Only IER_C and IER_D show essentially constant performance in the measured RH range.

[0173] The adsorbent material may also be a solid inorganic non-polymeric support material functionalized on the surface with amino functionalities capable of reversibly binding carbon dioxide, having a relative humidity of 10 m 2 / g to 25m 2 The invention has a BET specific surface area in the range of 100 nm to 200 nm and a cumulative pore volume in the range of 50 nm to 350 nm at 0.3 cm 3 / g to 1.5cm 3 The pore volume distribution is in the range of 1000 Å / g.

[0174] Silica (SiO2), alumina (Al2O3), silica-alumina (SiO2-Al2O3), titanium dioxide (TiO2), magnesium oxide (MgO), clay, and mixtures thereof are possible.

[0175] With regard to organic polymer materials, preferably for these organic or organic non-polymer support materials, the total pore volume measured by mercury intrusion porosimetry is between 0.3 and 0.7 cm 3 / g, and / or the pore size distribution measured by mercury porosimetry is such that 90%, preferably 95%, of the pore volume is in the range of 50 nm to 300 nm.

[0176] In the case of silica microspheres with these porosity characteristics, they can be produced using the following protocol:

[0177] Monodisperse colloidal SiO2 is prepared by seed growth method. The seed of commercially available Ludox AS-40 silica sol particles is added to a mixture of ammonia (2mol / L), deionized water (6mol / L) and ethanol to form a suspension. While the reaction mixture is maintained at 25 ℃, tetraethyl orthosilicate (TEOS, 2.2mol / L) is added to the mixture at a controlled speed under stirring. Monodisperse SiO2 particles are obtained by the growth of seed. Obtaining a monodisperse SiO2 microsphere with a diameter of 500nm, then calcined at 700 ℃ for 2 hours, and subsequently hydrothermally treated at 220 ℃ for 5 hours to regenerate the surface silanol groups lost during calcination.

[0178] The resulting silica material has a 10m 2 / g specific surface area, 95nm median pore size, 0.3cm 3 / g of total pore volume determined by mercury intrusion porosimetry, and an average particle size of 500 μm.

[0179] In the case of alumina microspheres having these porosity characteristics, they are commercially available from, for example, Saint GobainNor Pro-catalyst support.α-Alumina having no surface hydroxyl groups can be used for modification by impregnation.

[0180] In the case of titania microspheres having these porosity characteristics, they are commercially available from Saint Gobain Nor Pro-catalyst support. Rutile titania having no surface hydroxyl groups may be used for modification by impregnation.

[0181] Reference numerals list

[0182] 1 ambient air, ambient air 4 water vapor, water for desorption

[0183] Inflow into structure Steam inflow into structure

[0184] 2 Reactor outlet for extraction in adsorption flow mode 5

[0185] Ambient air in suction 6 vacuum units / separators

[0186] 7 wall with outflow behind the attached unit

[0187] 3 Adsorbent materials 8 Reactor units

Claims

1. A method for separating gaseous carbon dioxide from a gas mixture, preferably from at least one of ambient atmospheric air (1), waste gas and biogas, said gas mixture comprising said gaseous carbon dioxide and a further gas different from gaseous carbon dioxide, by cyclic adsorption / desorption using an adsorbent material (3) which adsorbs said gaseous carbon dioxide, in a unit (8), The method comprises at least the following steps (a) to (e) in the following order and repeated in this order: (a) in an adsorption step, in the case of ambient atmospheric air as the gas mixture, under ambient atmospheric pressure conditions and ambient atmospheric temperature conditions, and in the other case under the temperature and pressure conditions of the supplied gas mixture, contacting the gas mixture with the adsorbent material (3) by passing the flowthrough through the unit (8) so as to adsorb at least the gaseous carbon dioxide on the adsorbent material (3); (b) separating the adsorbent material (3) with adsorbed carbon dioxide in the unit (8) from the flowthrough while maintaining the temperature in the adsorbent; (c) injecting a saturated or superheated water vapor stream (4) by passing the flow through the unit (8) and thereby causing the temperature of the adsorbent material (3) to increase to a temperature of 60°C to 110°C, thereby initiating the desorption of CO2; (d) extracting at least the desorbed gaseous carbon dioxide from said unit (8) and separating the gaseous carbon dioxide from the water vapour by condensation downstream of said unit (8); (e) in the case of ambient atmospheric air as the gas mixture, bringing the adsorbent material (3) to the temperature conditions of the ambient atmosphere and in the other case bringing the adsorbent material (3) to the temperature and pressure conditions of the supplied gas mixture; The adsorbent material (3) is a solid inorganic or organic non-polymer or polymer support material functionalized on the surface with amino functionalities capable of reversibly binding carbon dioxide, having a molecular weight of 10 m 2 / g to 25m 2 The invention has a BET specific surface area in the range of 1000 nm to 2000 nm and a cumulative pore volume in the range of 50 nm to 350 nm at 0.28 cm 3 / g to 1.5cm 3 The pore volume distribution is in the range of 1000 Å / g.

2. The method according to claim 1, wherein the BET specific surface area of ​​the adsorbent material (3) is between 10 m 2 / g to 20m 2 / g, preferably within 12 m 2 / g to 20m 2 The BET specific surface area is preferably measured by nitrogen adsorption.

3. The method according to any one of the preceding claims, wherein the adsorbent material (3) has a pore size distribution measured by mercury intrusion porosimetry such that 90%, preferably 95%, of the pore volume is in the range of 50 nm to 400 nm, preferably in the range of 80 nm to 350 nm, and / or wherein the adsorbent material (3) has a pore volume distribution measured by mercury porosimetry such that the maximum pore volume is in the range of 80 nm to 150 nm, preferably in the range of 100 nm to 150 nm, wherein preferably 90%, more preferably 95% of the total pore volume of the distribution is within a window of -50 nm and +150 nm, preferably -40 nm and +100 nm around the diameter of said maximum of the pore volume distribution, And / or wherein the adsorbent material (3) has a 3 / g to 1cm 3 / g, preferably 0.35cm 3 / g to 0.8cm 3 / g, most preferably within 0.4 cm 3 / g to 0.7cm 3 The total pore volume measured by mercury intrusion porosimetry is in the range of 1000 Å / g.

4. The method according to any of the preceding claims, wherein the nitrogen content of the adsorbent material (3) is in the range of 5% to 50% by weight, preferably in the range of 8% to 15% by weight or 10% to 12% by weight, in each case for dry adsorbent material.

5. A method according to any one of the preceding claims, wherein the gas mixture is ambient atmospheric air.

6. The process according to any one of the preceding claims, wherein the solid inorganic or organic non-polymeric or polymeric support material of the adsorbent material is: an organic or inorganic polymer support, preferably an organic polymer support, in particular a polystyrene-based material, preferably a styrene divinylbenzene copolymer, preferably to form an adsorbent material surface functionalized with primary amines, preferably methylamine, most preferably benzylamine moieties, wherein the solid polymer support material is preferably obtained in a suspension and / or emulsion polymerization process, Alternatively, it is a non-polymer inorganic carrier, preferably selected from: silica (SiO2), alumina (Al2O3), titania (TiO2), magnesium oxide (MgO), clay, and mixed forms thereof, such as silica-alumina (SiO2-Al2O3), or mixtures thereof.

7. The method according to any one of the preceding claims, wherein the solid inorganic or organic non-polymeric or polymeric support material of the adsorbent material functionalized with amino functionalities on the surface is in the form of at least one of a block, a layer or a sheet, a hollow or solid fiber, a hollow or solid particle, or an extrudate, the hollow or solid fiber preferably being in the form of a woven or non-woven structure, wherein preferably the solid inorganic or organic non-polymeric or polymeric support material is in the form of substantially spherical beads preferably having a particle size (D50) in the range of 0.002 mm to 4 mm or 0.01 mm to 1.5 mm, preferably in the range of 0.30 mm to 1.25 mm, Or wherein the adsorbent material (3) of a solid inorganic or organic non-polymer or polymeric carrier material functionalized with amino functionality on the surface is preferably in the form of solid particles and / or fibers embedded or attached to a porous / breathable or non-porous matrix or carrier structure, wherein preferably the adsorbent material (3) is in the form of a layer of adsorbent material, preferably in the form of particles and / or fibers, the adsorbent material (3) being attached to at least one additional layer of a porous / breathable carrier material, preferably a porous / breathable polymer carrier material, preferably embedded between two layers of porous / breathable carrier material layers to form a laminate, which itself can preferably be further structured to form a plate or module.

8. The method according to any one of the preceding claims, wherein the adsorbent material (3) has a pore volume in the range of 50 nm to 350 nm of 0.3 cm 3 / g to 1.2cm 3 / g, preferably 0.35cm 3 / g to 0.7cm 3 The pore volume distribution is in the range of 1000 Å / g.

9. The method according to any of the preceding claims, wherein the adsorbent material (3) has a water retention in the range of 3 to 60 weight percent, preferably in the range of 3 to 30 weight percent or 5 to 30 weight percent and / or a bulk density in the range of 750 to 400 kg / m3, preferably 450 to 650 kg / m3 (EN ISO 60 (DIN 53468)), And / or wherein the process is carried out under conditions wherein the gas mixture or the ambient atmospheric air passing through the adsorbent material in step (a) has a relative humidity varying in the range of 20% RH to 80% RH, at least during 5% or 10% or 50% of the cycle over a day, a month and / or more than a year.

10. The method according to any one of the preceding claims, wherein step (d) is carried out by still bringing the adsorbent material (3) into contact with water vapour by injecting and / or circulating saturated or superheated water vapour into the unit, so as to flush and purge both water vapour and CO2 from the unit, while regulating the extraction and / or water vapour supply so as to substantially maintain the temperature in the adsorbent at the end of the previous step (c) and / or so as to substantially maintain the pressure in the adsorbent at the end of the previous step (c).

11. The method according to any one of the preceding claims, wherein a unit comprising the adsorbent material (3) is used, the unit and the adsorbent material being capable of maintaining a temperature of at least 60° C. for at least the desorption of the gaseous carbon dioxide, and the unit being openable for the flow of the gas mixture, preferably ambient atmospheric air, and for contacting the gas mixture with the adsorbent material for the adsorption step, Wherein preferably the unit comprises an array of individual adsorber elements, each adsorber element comprising at least one carrier layer and at least one adsorbent layer, the at least one adsorbent layer comprising or consisting of at least one adsorbent material, wherein the adsorbent material provides selective adsorption of CO2 in the presence of moisture or water vapor, wherein the adsorber elements in the array are arranged essentially parallel to each other and spaced apart from each other, thereby forming parallel fluid channels for passing a gas mixture, preferably ambient atmospheric air and / or water vapor.

12. A process according to any one of the preceding claims, wherein the unit is capable of being evacuated to a vacuum pressure of 400 mbar (abs) or less, and wherein step (b) comprises separating the adsorbent with adsorbed carbon dioxide in the unit from the flowthrough while maintaining the temperature in the adsorbent, and then evacuating the unit to a pressure in the range of 20 mbar (abs) to 400 mbar (abs), wherein in step (c) the injection of a saturated or superheated water vapour stream also causes an increase in the internal pressure of the reactor unit, and wherein step (e) comprises bringing the adsorbent material to ambient atmospheric pressure conditions and ambient atmospheric temperature conditions, and wherein preferably after step (d) and before step (e) the following steps are carried out: (d1) stopping the injection of water vapor and, if used, the circulation of water vapor, and evacuating the unit to a pressure value in the unit ranging from 20 mbar (abs) to 500 mbar (abs), preferably from 50 mbar (abs) to 250 mbar (abs), thereby evaporating water from the adsorbent and not only drying the adsorbent but also cooling the adsorbent.

13. A method according to any one of the preceding claims, wherein step (e) is carried out solely by contacting the ambient atmospheric air with the adsorbent material under ambient atmospheric pressure conditions and ambient atmospheric temperature conditions to evaporate and carry away water in the unit and to bring the adsorbent material to ambient atmospheric temperature conditions.

14. Use of an adsorbent material (3) for separating gaseous carbon dioxide from a gas mixture, preferably from at least one of ambient atmospheric air (1), waste gas and biogas, preferably for direct air capture, in particular using a temperature, vacuum, or temperature / vacuum swing process, using a process wherein a saturated or superheated water vapor stream (4) is injected through the flow stream to cause the temperature of the adsorbent material (3) to increase to a temperature of 60° C. to 110° C., thereby initiating the desorption of CO2, the adsorbent material (3) having a solid inorganic or organic non-polymeric or polymeric support material functionalized on the surface with amino functionalities capable of reversibly binding carbon dioxide, having a carbon dioxide content of 10 m / s and a carbon dioxide content of 10 m / s. 2 / g to 25m 2 / g in the range of 0.28 cm-1 and 0.30 cm-1, preferably in the range of 1.20 cm-1 and 1.50 cm-1, and preferably in the range of 2.50 cm-1 and 3.50 cm-1. 3 / g to 1.5cm 3 / g or 0.3cm 3 / g to 1.5cm 3 The adsorbent material (3) has a pore volume distribution in the range of 100 Å / g, and the adsorbent material (3) is used as it is or preferably attached to or embedded in a porous and / or non-porous matrix and / or support structure.

15. An apparatus for separating gaseous carbon dioxide from a gas mixture, preferably from at least one of ambient atmospheric air (1), waste gas and biogas, preferably a direct air capture apparatus, comprising at least one reactor unit (8) comprising an adsorbent material (3) suitable and adapted for flowing the gas mixture (1) through the reactor unit, wherein the reactor unit comprises an inlet (1) for the gas mixture, preferably for ambient air, during adsorption, and an outlet (2) for the gas mixture, preferably for ambient air, wherein the reactor unit is heatable to a temperature of at least 60° C. for at least the desorption of the gaseous carbon dioxide and is openable for the flow of the gas mixture, preferably the ambient atmospheric air, and for contacting the gas mixture with the adsorbent material for the adsorption step, wherein preferably the reactor unit is also evacuable to a vacuum pressure of 400 mbar (abs) or less, wherein the adsorbent material (3) is preferably in the form of at least a part of an adsorber structure comprising an array of individual adsorber elements, each adsorber element preferably comprising at least one block or carrier layer or sheet and at least one adsorbent material layer or adsorbent material block, the at least one adsorbent material layer or adsorbent material block comprising or consisting of at least one adsorbent material (3), wherein the adsorbent material comprises a solid inorganic or organic non-polymeric or polymeric carrier material functionalized on the surface with amino functionalities capable of reversibly binding carbon dioxide, having a carbon dioxide content of 10 m / s and a carbon dioxide content of 20 m / s. 2 / g to 25m 2 / g in the range of 0.28 cm-1 and 0.30 cm-1, preferably in the range of 1.20 cm-1 and 1.50 cm-1, and preferably in the range of 2.50 cm-1 and 3.50 cm-1. 3 / g to 1.5cm 3 / g or 0.3cm 3 / g to 1.5cm 3 / g, wherein preferably the adsorber elements in the array are arranged substantially parallel to each other and spaced apart from each other so as to form parallel flow channels for the flow of the gas mixture, preferably ambient atmospheric air and / or water vapor, at least one device for separating carbon dioxide from water, preferably a condenser, Preferably, at the gas outlet side of the device for separating carbon dioxide from water, preferably the condenser, there is at least one, preferably both, of a carbon dioxide concentration sensor and a gas flow sensor for controlling the desorption process.