Composition for activated carbon production, method for producing same, molded article for activated carbon production, method for producing same, fiber for activated carbon fiber production, method for producing same, activated carbon precursor, activated carbon fiber precursor, carbide, carbon fiber, activated carbon, method for producing same, and activated carbon fiber and method for producing same

By melting, mixing and molding the composition of phenolic resin and lignin, combined with carbonization and activation processes, the problems of insufficient mesopore volume and poor formability of activated carbon are solved, and the manufacturing of activated carbon with high specific surface area and high mesopore volume is achieved, which is suitable for Activated carbon and activated carbon fiber in various shapes.

CN118748982APending Publication Date: 2024-10-08IDEMITSU KOSAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380019459.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-02-13
Filing Date
2023-02-14
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The mesopore volume of activated carbon in the prior art is insufficient, resulting in poor performance, and heavy metal elements remain in the activated carbon fiber, or the formability and strength are poor, making it difficult to form into shapes other than pellets.

Method used

A combination of phenolic resin and lignin with a softening point of 100 to 175°C is used to form activated carbon with high specific surface area and high mesopore volume through melt mixing and molding. Combined with carbonization and activation processes, excellent activated carbon manufacturing materials are produced. Compositions and shaped bodies.

Benefits of technology

It achieves activated carbon with high specific surface area and high mesopore volume, and has excellent formability. It is suitable for manufacturing activated carbon and activated carbon fibers of various shapes, and improves adsorption performance and shape stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748982A_ABST
    Figure CN118748982A_ABST
Patent Text Reader

Abstract

A composition for producing activated carbon, which contains a phenolic resin and lignin having a softening point of 100-175 DEG C. Also disclosed is a molded body for producing activated carbon, which contains the composition for producing activated carbon. Also disclosed is a fiber for producing activated carbon fibers, which contains the composition for producing activated carbon. And an activated carbon precursor comprising a cured product of the composition for producing activated carbon. And an activated carbon fiber precursor comprising a cured product of the composition for producing activated carbon. And a carbide obtained by carbonizing the activated carbon precursor. And a carbon fiber obtained by carbonizing the activated carbon fiber precursor. And activated carbon obtained by activating the carbide. And the active carbon fiber is obtained by activating the carbon fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composition for producing activated carbon, a method for producing the same, a molded body for producing activated carbon, a method for producing the same, a fiber for producing activated carbon fiber, a method for producing the same, an activated carbon precursor, an activated carbon fiber precursor, a carbide, a carbon fiber, activated carbon, a method for producing the same, and activated carbon fiber and a method for producing the same.

[0002] This application claims priority based on Japanese Patent Application No. 2022-020649 filed in Japan on February 14, 2022 and Japanese Patent Application No. 2023-020122 filed in Japan on February 13, 2023, and the contents of which are incorporated herein by reference. Background Art

[0003] Activated carbon is a substance with many pores and a large specific surface area. It is suitably used as an adsorbent material, an electrode for an electric double layer capacitor, etc. by utilizing this characteristic. Activated carbon is usually produced by carbonizing and activating an activated carbon precursor. Activation is a treatment for forming pores in activated carbon, which is usually carried out by reacting with specific gases or chemicals under high temperature conditions. Activation is sometimes also called activation.

[0004] In the past, as activated carbon precursors, in the case of powdered activated carbon, coconut shells, sawdust, wood components, coal tar, petroleum asphalt, etc. were mainly used, and in the case of fibrous activated carbon, so-called activated carbon fibers, pitch-based fibers, acrylic fibers, phenolic resin fibers, rayon fibers, etc. were mainly used.

[0005] In addition, lignin has also been studied for use as an activated carbon precursor.

[0006] Patent Document 1 discloses a method of preparing lignin having a hydrophilic group, forming precursor fibers from the lignin, and then insolubilizing the precursor fibers by acid treatment, carbonizing the precursor fibers to form carbon fibers, and activating the carbon fibers.

[0007] Patent Document 2 discloses a method of dispersing a metal element having hydrogenation activity in carbon fibers such as lignin-polyvinyl alcohol-based carbon fibers, and heat-treating the carbon fibers in which the metal element is dispersed in a reducing atmosphere.

[0008] Patent Document 3 discloses a method in which pellets of wood residue containing lignin, which are derived from a production process of bioethanol using wood-based biomass as a raw material, are carbonized and activated by heating under a specific atmosphere.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2013-147768

[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 11-269763

[0013] Patent Document 3: Japanese Patent Application Publication No. 2010-207693 Summary of the invention

[0014] Problems to be solved by the invention

[0015] However, the mesopore volume of activated carbon obtained by the methods described in Patent Documents 1 to 3 is insufficient, and thus the performance is poor. For example, in the activated carbon fiber obtained by the method of Patent Document 1, the micropore volume accounts for more than 75% of the total pore volume, and the adsorption capacity of large molecules is insufficient.

[0016] In addition, the method of Patent Document 2 requires heavy metal elements, so heavy metal elements remain in the obtained activated carbon fibers. Such activated carbon fibers cannot be used depending on the application.

[0017] In addition, in the method of patent document 3, the wood residue as the precursor does not melt, so the formability is poor and it is difficult to form into a shape other than pellets, such as a fibrous shape. Even if it can be formed into other shapes, the strength and toughness of the precursor are also poor, and its shape is likely to be damaged when carbonized or activated.

[0018] The object of the present invention is to provide activated carbon having a high specific surface area and a high mesopore volume obtained by carbonization and activation, a composition for producing activated carbon having excellent moldability and a method for producing the same; as well as an activated carbon molded body obtained using the activated carbon composition, a method for producing the same, fibers for producing activated carbon fibers, a method for producing the same, an activated carbon precursor, a carbide thereof, an activated carbon fiber precursor, carbon fibers, activated carbon, a method for producing the same, activated carbon fibers and a method for producing the same.

[0019] Means for solving problems

[0020] The present invention has the following aspects.

[0021] [1] A composition for producing activated carbon, comprising a phenolic resin and lignin having a softening point of 100 to 175°C.

[0022] [2] The composition for producing activated carbon according to [1] above, wherein the ash content of the lignin is 0.1 to 2.0% by mass.

[0023] [3] The composition for producing activated carbon according to [1] or [2], wherein the phenolic resin is a novolac-type phenolic resin.

[0024] [4] The composition for producing activated carbon according to any one of [1] to [3], wherein the ratio of the lignin to the total mass of the lignin and the phenolic resin is 5 to 90% by mass.

[0025] [5] A method for producing a composition for producing activated carbon, which is a method for producing the composition for producing activated carbon according to any one of [1] to [4], wherein:

[0026] The lignin and the phenolic resin are melt-mixed at 160 to 200°C.

[0027] [6] A molded body for producing activated carbon, comprising the composition for producing activated carbon according to any one of [1] to [4].

[0028] [7] A method for producing a molded body for producing activated carbon, which is a method for producing the molded body for producing activated carbon according to [6], wherein:

[0029] The lignin and the phenolic resin are melt-mixed at 160 to 200° C., and the obtained mixture is molded.

[0030] [8] A fiber for producing activated carbon fiber, comprising the composition for producing activated carbon according to any one of [1] to [4].

[0031] [9] A method for producing a fiber for producing activated carbon fiber, which is a method for producing the fiber for producing activated carbon fiber according to the above-mentioned [8], wherein:

[0032] The lignin and the phenolic resin are melt-spun at 160 to 200°C.

[0033]

[10] An activated carbon precursor comprising a solidified product of the composition for producing activated carbon according to any one of [1] to [4].

[0034]

[11] The activated carbon precursor according to

[10] above, which is a shaped body.

[0035]

[12] An activated carbon fiber precursor comprising a cured product of the composition for producing activated carbon according to any one of [1] to [4].

[0036]

[13] A carbide obtained by carbonizing the activated carbon precursor of

[10] or

[11] above.

[0037]

[14] Carbon fiber obtained by carbonizing the activated carbon fiber precursor of the above-mentioned

[12] .

[0038]

[15] Activated carbon obtained by activating the carbide of the above-mentioned

[13] .

[0039]

[16] A method for producing activated carbon, comprising solidifying the composition for producing activated carbon according to any one of [1] to [4], carbonizing the obtained solidified product, and activating the obtained carbonized product.

[0040]

[17] A method for producing activated carbon, comprising solidifying the molded body for producing activated carbon according to [6], carbonizing the obtained solidified product, and activating the obtained carbide.

[0041]

[18] Activated carbon fiber, which is obtained by activating the carbon fiber of the above-mentioned

[14] .

[0042]

[19] A method for producing activated carbon fibers, comprising curing the fibers for producing activated carbon fibers according to [8], carbonizing the obtained cured product, and activating the obtained carbon fibers.

[0043] Effects of the Invention

[0044] According to the present invention, there can be provided activated carbon having a high specific surface area and a high mesopore volume obtained by carbonization and activation, a composition for producing activated carbon having excellent moldability and a method for producing the same; as well as an activated carbon molded body obtained using the activated carbon composition, a method for producing the same, fibers for producing activated carbon fibers, a method for producing the same, an activated carbon precursor, a carbide thereof, an activated carbon fiber precursor, carbon fibers, activated carbon, a method for producing the same, activated carbon fibers and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a graph showing changes in strength and elongation relative to the lignin blending ratio of the lignin fiber A.

[0046] Figure 2 This is a graph showing changes in strength and elongation relative to the lignin compounding ratio of the lignin fiber B.

[0047] Figure 3 This is a graph showing changes in the raw material yield and the mesopore volume relative to the lignin compounding ratio of the lignin activated carbon fiber A.

[0048] Figure 4 This is a graph showing changes in the raw material yield and the specific surface area relative to the lignin compounding ratio of the lignin activated carbon fiber A.

[0049] Figure 5 This is a graph showing changes in the raw material yield and the mesopore volume relative to the lignin compounding ratio of the lignin-activated carbon fiber B.

[0050] Figure 6 This is a graph showing changes in the raw material yield and the specific surface area relative to the lignin compounding ratio of the lignin activated carbon fiber B.

[0051] Figure 7 is the pore distribution of lignin activated carbon fiber A.

[0052] Figure 8 is the pore distribution of lignin activated carbon fiber B.

[0053] Fig. 9 is the pore distribution of lignin activated carbon fiber C.

[0054] Fig.10 It is the pore distribution of lignin activated carbon A and lignin activated carbon B.

[0055] Fig.11 This is a graph showing changes in the raw material yield and the mesopore volume with respect to the activation time of the lignin activated carbon fiber A (lignin blending ratio of 50 mass %).

[0056] Fig.12 This is a graph showing changes in raw material yield and specific surface area with respect to activation time of lignin activated carbon fibers A (lignin blending ratio: 50% by mass).

[0057] Fig.13 This is a graph showing changes in pore size distribution due to activation time of lignin activated carbon fiber A (lignin blending ratio: 50 mass %). DETAILED DESCRIPTION

[0058] [Composition for producing activated carbon]

[0059] The composition for producing activated carbon according to one embodiment of the present invention (hereinafter also referred to as "the present composition") contains a phenolic resin and lignin having a softening point of 100 to 175°C.

[0060] Lignin is a polymer obtained by polymerizing three types of lignin monomers, which are p-hydroxycinnamyl alcohols, and has a basic skeleton represented by the following formula (1).

[0061] [Chemistry 1]

[0062]

[0063] In the above formula (1), R 1 and R 2 Each independently represents a hydrogen atom or a methoxy group. 1 Indicates bond to carbon atom, X 2 Indicates bond to a hydrogen atom or a carbon atom.

[0064] R 1 and R 2 The core with two hydrogen atoms is called p-hydroxyphenyl core (H-type skeleton). 1 and R 2A nucleus in which either of the two is a hydrogen atom is called a guaiacyl nucleus (G-type skeleton). 1 and R 2 The two nuclei that are not hydrogen atoms are called eugenol nuclei (S-type skeletons).

[0065] The lignin used in the present composition has a softening point of 100 to 175°C. If the softening point of the lignin is above 100°C, the present composition has sufficient melt viscosity and the wire drawing property becomes high. If the softening point of the lignin is below 175°C, the lignin is sufficiently softened and melt-mixed before the lignin undergoes thermal decomposition. Therefore, the present composition has excellent moldability and raw material yield when manufacturing activated carbon. The softening point of the lignin can be 120 to 175°C, and can further be 135 to 175°C. From the viewpoint of wire drawing property, moldability, and raw material yield, the softening point of the lignin is more preferably 100 to 145°C, further preferably 120 to 145°C, and can be 135 to 145°C.

[0066] The softening point is determined by the following procedure.

[0067] The lignin sample was ground in a mortar, and 10 to 20 mg of the ground sample was placed in an aluminum cup (round upper lower part The aluminum cup containing the sample was placed on a hot plate (IKA C-MAG HP7), covered with aluminum foil and heated to 100°C. The temperature was then increased in 10°C increments and visually observed. The temperature at which the sample melted was defined as the softening point.

[0068] Typically, lignin contains ash. Examples of the ash include F, Cl, Br, S, Na, K, Ca, Mg, Al, Si, P, Fe, Mn, Ti, Zn, Ba, Cr, Cu, and V.

[0069] The ash content of lignin is preferably 0.1 to 2.0 mass %, more preferably 0.5 to 0.6 mass % relative to the total mass of lignin. When the ash content of lignin is below the upper limit, carbonization and activation of the present composition can be performed well.

[0070] The ash content of lignin was calculated as follows: About 10 mg of sample was weighed into a Pt pot using a thermogravimetric-differential thermal simultaneous measuring apparatus (manufactured by Hitachi High-Tech Science & Technology Co., Ltd., TG / DTA6300), and the ash content was calculated based on the mass ratio of the residual components. The ash content of lignin was calculated as follows: About 10 mg of sample was weighed into a Pt pot, and the sample was measured at a heating rate of 10°C / min, a measuring atmosphere of air 200 mL / min, and a temperature of 35°C to 800°C.

[0071] Lignin can use commercially available lignin or lignin produced by a known production method. Lignin having a softening point of 100 to 175° C. can be produced by the method described in, for example, International Publication No. 2019 / 031609.

[0072] The softening point of lignin can be adjusted according to the molecular weight of lignin, etc. For example, there is a tendency that the softening point becomes lower as the molecular weight of lignin becomes lower.

[0073] Examples of the phenolic resin include novolac-type phenolic resins, resol-type phenolic resins, various modified phenolic resins, and mixtures thereof.

[0074] Novolac type phenolic resin is a phenolic resin obtained by reacting phenols with aldehydes in the presence of an acidic catalyst. Resol type phenolic resin is a phenolic resin obtained by reacting phenols with aldehydes in the presence of an alkaline catalyst. As modified phenolic resins, there can be cited resins obtained by modifying novolac type or resol type phenolic resins by known techniques such as boron modification, silicon modification, heavy metal modification, nitrogen modification, sulfur modification, oil modification, and rosin modification.

[0075] The phenols may be any phenols that react with aldehydes in the presence of an acidic or basic catalyst to give phenolic resins, and examples thereof include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 3,5-xylenol, m-ethylphenol, m-propylphenol, m-butylphenol, p-butylphenol, o-butylphenol, resorcinol, hydroquinone, catechol, 3-methoxyphenol, 4-methoxyphenol, 3-methylcatechol, 4-methylcatechol, methylhydroquinone, 2-methylresorcinol, 4-methyl-2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol, 2-hydroxy-2-ol Phenol, 2,3-dimethylhydroquinone, 2,5-dimethylresorcinol, 2-ethoxyphenol, 4-ethoxyphenol, 4-ethylresorcinol, 3-ethoxy-4-methoxyphenol, 2-propenylphenol, 2-isopropylphenol, 3-isopropylphenol, 4-isopropylphenol, 3,4,5-trimethylphenol, 2-isopropoxyphenol, 4-propoxyphenol, 2-allylphenol, 3,4,5-trimethoxyphenol, 4-isopropyl-3-methylphenol, pyrogallol, phloroglucinol, 1, 2,4-Benzenetriol, 5-isopropyl-3-methylphenol, 4-butoxyphenol, 4-tert-butylcatechol, tert-butylhydroquinone, 4-tert-amylphenol, 2-tert-butyl-5-methylphenol, 2-phenylphenol, 3-phenylphenol, 4-phenylphenol, 3-phenoxyphenol, 4-phenoxyphenol, 4-hexyloxyphenol, 4-hexanoylresorcinol, 3,5-diisopropylcatechol, 4-hexylresorcinol, 4-heptyloxyphenol, 3,5-di-tert-butylphenol, 3,5-di-tert-butylphenol Butylcatechol, 2,5-di-tert-butylhydroquinone, di-sec-butylphenol, 4-cumylphenol, nonylphenol, 2-cyclopentylphenol, 4-cyclopentylphenol, 1-naphthol, 2-naphthol, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 1,8-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, bisphenol A, bisphenol F, etc.

[0076] Among them, phenol, o-cresol, m-cresol, p-cresol, bisphenol A, 2,3-xylenol, 3,5-xylenol, m-butylphenol, p-butylphenol, o-butylphenol, 4-phenylphenol, and resorcinol are preferred, and phenol is most preferred. The above phenols may be used alone or in combination of two or more.

[0077] Examples of the aldehydes include formaldehyde, trioxane, furfural, paraformaldehyde, benzaldehyde, methyl hemiformal, ethyl hemiformal, propyl hemiformal, salicylaldehyde, butyl hemiformal, phenyl hemiformal, acetaldehyde, propionaldehyde, phenylacetaldehyde, α-phenylpropylaldehyde, β-phenylpropylaldehyde, o-hydroxybenzaldehyde, m-hydroxybenzaldehyde, p-hydroxybenzaldehyde, o-chlorobenzaldehyde, o-nitrobenzaldehyde, m-nitrobenzaldehyde, p-nitrobenzaldehyde, o-tolualdehyde, m-tolualdehyde, p-tolualdehyde, p-ethylbenzaldehyde, and p-n-butylbenzaldehyde.

[0078] Among them, formaldehyde, paraformaldehyde, furfural, benzaldehyde, and salicylaldehyde are preferred, and formaldehyde and paraformaldehyde are particularly preferred. The above aldehydes may be used alone or in combination of two or more.

[0079] Examples of the acidic catalyst include hydrochloric acid, oxalic acid, sulfuric acid, phosphoric acid, formic acid, acetic acid, oxalic acid, butyric acid, lactic acid, benzenesulfonic acid, p-toluenesulfonic acid, boric acid, or salts of zinc chloride, zinc acetate, and metals.

[0080] Among them, hydrochloric acid or oxalic acid is preferably used as a catalyst, and hydrochloric acid is particularly preferred, from the viewpoint of easily obtaining activated carbon having a high mesopore ratio.

[0081] The acidic catalyst may be used alone or in combination of two or more.

[0082] The acidic catalyst is used in an amount of preferably 0.05 to 3.00% by mass, more preferably 0.05 to 1.00% by mass, based on 100% by mass of the phenols.

[0083] When neutralization is performed at the end of the reaction using the acidic catalyst, a sodium hydroxide solution, ammonia water, zinc acetate, potassium hydroxide, or the like can be used as the neutralizing solution.

[0084] Examples of the alkaline catalyst include alkali metal hydroxides such as sodium hydroxide and lithium hydroxide; alkaline earth metal hydroxides such as calcium hydroxide and barium hydroxide; ammonium hydroxide; and amines such as diethylamine, triethylamine, triethanolamine, ethylenediamine, and hexamethylenetetramine.

[0085] Among them, amines are preferred, and amines selected from ammonia and diethylamine are particularly preferred, from the viewpoint of easily obtaining a solid resol-type phenolic resin.

[0086] The basic catalyst may be used alone or in combination of two or more.

[0087] The basic catalyst is used in an amount of preferably 0.5 to 3.0% by mass, more preferably 0.8 to 2.0% by mass, based on 100% by mass of the phenols.

[0088] As the phenolic resin, among the above, novolac type phenolic resin and resol type phenolic resin are preferred. If the form is solid, lignin and the additives described later can be easily dispersed uniformly. Therefore, novolac type phenolic resin and solid resol type phenolic resin are more preferred, and novolac type phenolic resin is particularly preferred.

[0089] Compared with resol-type phenolic resins, novolac-type phenolic resins have excellent thermal stability and are less likely to undergo unexpected polymerization due to heating during melting. Therefore, they can be stably molded into various shapes such as fibers.

[0090] The weight average molecular weight of the novolac phenol resin is preferably 1000 to 10000, more preferably 2000 to 9000, and even more preferably 3000 to 8000. When the weight average molecular weight is within the above range, the stringiness is more excellent.

[0091] The weight average molecular weight is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0092] The present composition may further contain other components as necessary within a range not impairing the effects of the present invention.

[0093] Examples of other components include fatty acids, fatty acid amides, fatty acid esters, fatty acid metal salts, fatty acid alcohols, fatty acid hydrazides, polyoxyethylene derivatives of fatty acid esters, and silane coupling agents.

[0094] In the present composition, the ratio of lignin to the total mass of lignin and phenolic resin (hereinafter also referred to as "lignin blending ratio") is preferably 5 to 90 mass %, more preferably 20 to 80 mass %, and further preferably 40 to 60 mass %. If the lignin blending ratio is above the aforementioned lower limit, there is a tendency for the mesopore volume of the activated carbon to increase, and if it is below the aforementioned upper limit, there is a tendency for the moldability of the present composition, the strength of the cured product of the present composition, the elongation, and the specific surface area of ​​the activated carbon to increase.

[0095] In the present composition, the total content of lignin and phenolic resin is preferably 87% by mass or more, more preferably 93% by mass or more, and may be 100% by mass, based on the total mass of the present composition.

[0096] The present composition can be obtained, for example, by melt-mixing the aforementioned lignin and phenolic resin at 160 to 200° C. At this time, other components may be mixed as necessary.

[0097] The temperature (melt mixing temperature) when lignin and phenolic resin are melt-mixed is 160 to 200° C., preferably 175 to 185° C. If the melt mixing temperature is 160° C. or higher, lignin is sufficiently softened, and lignin and phenolic resin can be easily mixed. If the melt mixing temperature is 200° C. or lower, thermal decomposition of lignin is easily suppressed.

[0098] The time for melt mixing lignin and phenolic resin (melt mixing time) is preferably 30 to 120 minutes, more preferably 60 to 90 minutes. If the melt mixing time is above the lower limit, the two can be mixed more uniformly, and if it is below the upper limit, it is easy to suppress the thermal decomposition of lignin.

[0099] The melt mixing can be carried out using a known melt mixing device. Examples of the melt mixing device include an extruder type kneading machine, an open roll, a Banbury mixer, and a high-speed biaxial continuous mixer.

[0100] [Molded body for producing activated carbon]

[0101] A molded body for producing activated carbon according to one embodiment of the present invention (hereinafter also referred to as "the present molded body") is a molded body comprising the present composition described above.

[0102] Examples of the shape of the molded body include fiber, plate, granular, and film. Among these, fiber is preferred from the viewpoints of high specific surface area, air permeability, liquid permeability, flexibility, and secondary moldability into cloth or felt.

[0103] When the present molded body is a fiber, the present molded body is used as, for example, a fiber for producing activated carbon fiber.

[0104] The fineness of the fiber is preferably 1 to 10 deniers, more preferably 2 to 6 deniers. When the fineness is at most the upper limit, poor curing is less likely to occur when the fiber is cured, and the strength and elongation of the cured product are more excellent.

[0105] The present molded product can be obtained by, for example, melt-mixing the above-mentioned lignin and phenolic resin at 160 to 200° C. and molding the obtained mixture (present composition).

[0106] The preferred temperature and time for melt mixing of lignin and phenolic resin are the same as those described above. At this time, other components may be mixed as needed.

[0107] As the molding method, a known molding method can be applied according to the shape of the molded body.

[0108] For example, when forming into a fiber, a known method such as wet spinning, dry spinning, dry / wet spinning, melt spinning, gel spinning, liquid crystal spinning, etc. can be appropriately selected. Among them, melt spinning is preferred from the perspective of simplicity of the apparatus and economic advantages.

[0109] When melt spinning is used as the spinning method, a general melt spinning apparatus can be used. As a dissolving apparatus of the melt spinning apparatus, a grate type, a single screw extruder type, a twin screw extruder type, a tandem extruder type, etc. can be used.

[0110] In order to prevent oxidation of the molten present composition, nitrogen substitution may be performed in the melt spinning apparatus, or a trace amount of residual solvent or monomers may be removed using an extruder equipped with vent holes.

[0111] During melt spinning, the temperature condition is preferably 160 to 200° C., more preferably 175 to 185° C. By setting the temperature condition to a preferred lower limit or more, lignin is sufficiently softened, and efficient spinning is possible. By setting the temperature condition to a preferred upper limit or less, thermal decomposition of lignin is easily suppressed.

[0112] As the spinning head, a common head can be used, and the hole diameter is preferably 0.05 mm or more and less than 1 mm, more preferably 0.1 mm or more and less than 0.5 mm, and the (length L / diameter D) of the capillary part is preferably 0.5 or more and less than 10, more preferably 1 to 5. By setting the hole diameter and L / D to the above preferred ranges, stable spinning can be achieved.

[0113] In the case of a method for producing special fibers (for example, side-by-side composite fibers, core-sheath composite fibers, island-in-sea composite fibers, etc.), a side-by-side die or core-sheath die, or a conjugated die combined with a third component polymer may be used.

[0114] The spinning speed is preferably 15 m / min or more and less than 3000 m / min, more preferably 30 m / min or more and less than 2000 m / min, and further preferably 50 m / min or more and less than 1600 m / min. By setting the spinning speed to a preferred lower limit or more, efficient spinning is possible. By setting the spinning speed to a lower limit than a preferred upper limit, wire breakage during spinning can be suppressed.

[0115] When forming into a plate shape, for example, it is only necessary to form using a mold.

[0116] When forming into pellets, for example, pelletization may be performed using a pelletizer.

[0117] When forming into a film shape, for example, film formation may be performed using a film forming apparatus.

[0118] When the method of molding the mixture through the molding step is a melt molding method (melt spinning, etc.), the melt mixing step and the molding step can be performed continuously, and there can be a step of cooling the molten mixture obtained by the melt mixing step between the melt mixing step and the molding step.

[0119] 〔Activated carbon precursor〕

[0120] An activated carbon precursor according to one embodiment of the present invention (hereinafter also referred to as "the present precursor") includes a solidified product of the present composition.

[0121] The present precursor is preferably a molded product. The present composition is excellent in moldability, and therefore, when the present precursor is a molded product, the usefulness of the present invention is high.

[0122] As the shape of the molded body, the same shapes as those mentioned above can be cited, and the preferred aspects are also the same. That is, the present precursor is preferably an activated carbon fiber precursor.

[0123] The present precursor is obtained by curing the present composition that has been shaped (the present shaped body) or the present composition that has not been shaped.

[0124] The phenolic resin is a novolac-type phenolic resin. When the present molded body is cured, the curing can be performed by bringing the present molded body into contact with a catalyst and, if necessary, an aqueous treatment liquid containing aldehydes.

[0125] The phenolic resin is a novolac type phenolic resin, and when the present composition before molding is cured, curing can be performed by mixing a catalyst and, if necessary, an aldehyde into the present composition.

[0126] Examples of the catalyst include alkaline catalysts such as amines such as ammonium hydroxide, diethylamine, triethylamine, triethanolamine, ethylenediamine, hexamethylenetetramine, and mixtures thereof; acidic catalysts such as salts of hydrochloric acid, sulfuric acid, phosphoric acid, formic acid, acetic acid, oxalic acid, butyric acid, lactic acid, benzenesulfonic acid, p-toluenesulfonic acid, boric acid, zinc chloride or zinc acetate and metals, and mixtures thereof. The catalyst may be used alone or in combination of two or more.

[0127] The phenolic resin is a novolac type phenolic resin, and when the molded article is cured, an acidic catalyst is preferably used as a catalyst.

[0128] The phenolic resin is a novolac type phenolic resin, and when the unmolded present composition is cured, hexamethylenetetramine is preferably used as a catalyst.

[0129] When the treatment liquid contains an acid catalyst, the concentration of the acid catalyst in the treatment liquid is preferably 16.5 to 19.0 mass %, more preferably 17.5 to 18.0 mass % relative to the total mass of the treatment liquid. When the concentration of the acid catalyst is within the above range, the elongation of the cured product is good.

[0130] Examples of the aldehydes include formaldehyde, trioxane, furfural, paraformaldehyde, benzaldehyde, methyl hemiformal, ethyl hemiformal, propyl hemiformal, salicylaldehyde, butyl hemiformal, phenyl hemiformal, acetaldehyde, propionaldehyde, phenylacetaldehyde, α-phenylpropylaldehyde, β-phenylpropylaldehyde, o-hydroxybenzaldehyde, m-hydroxybenzaldehyde, p-hydroxybenzaldehyde, o-chlorobenzaldehyde, o-nitrobenzaldehyde, m-nitrobenzaldehyde, p-nitrobenzaldehyde, o-tolualdehyde, m-tolualdehyde, p-tolualdehyde, p-ethylbenzaldehyde, and p-n-butylbenzaldehyde.

[0131] Among them, formaldehyde, paraformaldehyde, furfural, benzaldehyde, and salicylaldehyde are preferred, and formaldehyde and paraformaldehyde are more preferred. The aldehydes may be used alone or in combination of two or more.

[0132] When hexamethylenetetramine is used as a catalyst, no aldehydes are required.

[0133] When a treatment liquid is used, curing is preferably performed by heating in the treatment liquid at a temperature of 60° C. or higher and lower than 110° C. for 3 hours or more and less than 30 hours.

[0134] Curing can be performed by heating in a gas phase after bringing the mixture into contact with a treatment liquid or kneading the catalyst and, if necessary, an aldehyde.

[0135] Furthermore, after being heated and cured in the treatment liquid, the material may be washed and dried, and then heated at 100 to 300° C. in an inert gas such as nitrogen, helium, or carbon dioxide to further cure.

[0136] In addition, a known curing treatment may be performed.

[0137] The specific method of contact with the treatment liquid is not particularly limited. As methods for obtaining a fibrous solidified product (activated carbon fiber precursor), there are listed: a method in which the present composition formed into a bundle or a filament shape is immersed in the treatment liquid in a reaction container and solidified in a batch manner; a method in which the present composition formed into a bobbin or a reel shape is contacted with the treatment liquid for solidification; a method in which the present composition formed into a filament shape is continuously contacted with the treatment liquid for solidification, etc.

[0138] On the other hand, when the phenolic resin is a resol-type phenolic resin, a cured product can be obtained by heat treatment using a wet heat method or a dry heat method.

[0139] The heat treatment temperature is preferably 100 to 220° C., more preferably 120 to 180° C., and the heat treatment time is preferably 5 to 120 minutes, more preferably 20 to 60 minutes.

[0140] 〔carbide〕

[0141] The carbide according to one embodiment of the present invention (hereinafter also referred to as "the present carbide") is obtained by carbonizing the present precursor.

[0142] The shape of the present carbide is the same as that of the present precursor. For example, when the present precursor is fibrous (activated carbon fiber precursor), the present carbide is also fibrous. Fibrous carbide is also called carbon fiber.

[0143] For carbonization, a conventionally known method of heating in the presence of an inert gas can be used.

[0144] Examples of the inert gas used for carbonization include gases that do not substantially contain oxygen, such as nitrogen, helium, argon, hydrogen, carbon monoxide, and carbon dioxide.

[0145] The temperature during carbonization is preferably 480 to 1200°C, more preferably 520 to 1000°C, and even more preferably 600 to 900°C.

[0146] Carbonization can be performed using a multi-stage furnace, a rotary furnace, a fluidized bed furnace, or the like.

[0147] The carbide is activated to produce activated carbon.

[0148] 〔Activated carbon〕

[0149] The activated carbon according to one embodiment of the present invention (hereinafter also referred to as "present activated carbon") is obtained by activating the present carbonized product. In other words, it is obtained by carbonizing and activating the present precursor.

[0150] The shape of the present activated carbon is the same as that of the present carbide. For example, when the present carbide is fibrous (carbon fiber), the present activated carbon is also fibrous. Fibrous activated carbon is also called activated carbon fiber.

[0151] The present activated carbon has mesopores, which are fine pores with a diameter of 2 to 50 nm.

[0152] The present activated carbon may have, in addition to mesopores, micropores with a diameter of less than 2 nm and macropores with a diameter of more than 50 nm.

[0153] The specific surface area of ​​the activated carbon is preferably 1400 to 2400 m 2 / g, more preferably 1600 to 2400 m 2 / g, more preferably 1800 to 2400 m 2When the specific surface area is greater than the above lower limit, the adsorption performance and electrostatic capacity tend to be improved. When the specific surface area is less than the above upper limit, the mesopore volume tends to be increased.

[0154] Here, the specific surface area is a value obtained by the BET method (BET specific surface area).

[0155] The mesopore volume of the activated carbon is preferably 0.1 to 2.6 cm 3 / g, more preferably 0.5 to 2.6 cm 3 / g, more preferably 1.9 to 2.6 cm 3 When the mesopore volume is greater than or equal to the above lower limit, the adsorption performance tends to be improved. When the mesopore volume is less than or equal to the above upper limit, the specific surface area and the yield during production tend to be improved.

[0156] Here, the mesopore volume is a value obtained by the BJH method.

[0157] The present activated carbon is obtained by activating the above-mentioned carbonized material.

[0158] The activation can be carried out by a conventionally known activation method such as a gas activation method or a drug activation method.

[0159] In the gas activation method, activation is performed by bringing an activation gas into contact with carbides.

[0160] Examples of the activating gas include water vapor, air, carbon monoxide, carbon dioxide, hydrogen chloride, oxygen, or a gas containing a mixture of these.

[0161] In the agent activation method, the agent is brought into contact with carbide to be activated.

[0162] Examples of the chemical include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; alkaline earth metal hydroxides such as calcium hydroxide; inorganic acids such as boric acid, phosphoric acid, sulfuric acid, and hydrochloric acid; and inorganic salts such as zinc chloride.

[0163] In the case of the drug activation method, after activation, the product and the chemicals used may be neutralized with an acid or an alkali, or may be removed by washing with water or the like.

[0164] Among the above activation methods, the gas activation method is preferred, and the gas activation method using water vapor is particularly preferred, from the viewpoint of simplicity of equipment and no need for special treatment after activation.

[0165] The activation can be performed using a multi-stage furnace, a rotary furnace, a fluidized bed furnace, or the like.

[0166] Regarding the activation temperature (the temperature when the activating gas and the agent are brought into contact with the carbide), in the gas activation method, it is preferably 750 to 1200°C, more preferably 850 to 1200°C, and further preferably 900 to 1000°C. In the chemical activation method, it is preferably 550 to 800°C, more preferably 600 to 800°C, and further preferably 700 to 750°C.

[0167] The activation time (the time for contacting the activation gas and reagent with the carbide) is preferably 30 to 75 minutes, and more preferably 45 to 60 minutes. If the activation time is above the lower limit, there is a tendency for the mesopores to grow sufficiently and the mesopore volume to increase, and if it is below the upper limit, there is a tendency for the specific surface area and yield of the activated carbon to increase.

[0168] Example

[0169] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to the following descriptions. Hereinafter, "%" means "mass %" unless otherwise specified.

[0170] <Materials used>

[0171] Lignin A: manufactured by Idemitsu Kosan Co., Ltd., softening point: 135 to 145° C., ash content: 0.5%.

[0172] Lignin B: manufactured by Idemitsu Kosan Co., Ltd., softening point: 165 to 175° C., ash content: 0.6%.

[0173] Lignin C: manufactured by Idemitsu Kosan Co., Ltd., softening point: 125 to 135° C., ash content: 0.5%.

[0174] Phenolic resin A: novolac type, manufactured by Gun-Ei Chemical Industry Co., Ltd., weight average molecular weight: 6201.

[0175] Phenolic resin B: novolac type, manufactured by Gun-Ei Chemical Industry Co., Ltd., weight average molecular weight: 3,980.

[0176] Phenolic resin fiber: a fiber composed of a cured product of a novolac-type phenolic resin, manufactured by Gunei Chemical Industry Co., Ltd., trade name “KF-0570”.

[0177] The softening point, ash content and weight average molecular weight are measured as follows.

[0178] Softening point: The sample was crushed in a mortar and 10 to 20 mg of the crushed sample was placed in an aluminum cup (round upper lower part × depth 15mm). The aluminum cup containing the sample was placed on a hot plate (IKA C-MAG HP7) and covered with aluminum foil. After heating to 100°C, the temperature was increased in 10°C increments and visually observed. The temperature at which dissolution occurred was set as the softening point.

[0179] Ash content: Using TG / DTA6300 manufactured by Hitachi High-Tech Science & Technology Co., Ltd., about 10 mg of a sample was weighed into a Pt pan and measured at a heating rate of 10°C / min, a measuring atmosphere of air at 200 mL / min, and a temperature of 35°C to 800°C. The mass ratio of the residual component was determined and the value was set as the ash content.

[0180] Weight average molecular weight: measured as a polystyrene-equivalent value by gel permeation chromatography (GPC) under the following conditions.

[0181] GPC device: HLC8320GPC manufactured by Tosoh Corporation.

[0182] Column: TSKgel G3000HXL+G3000HXL+G2000HXL manufactured by Tosoh Corporation.

[0183] <Examples 1 to 8>

[0184] (Manufacturing of lignin activated carbon fibers)

[0185] The following steps were followed to produce lignin activated carbon fibers.

[0186] (1) Into a reaction vessel (500 mL flask) equipped with a thermometer, a stirrer and a condenser, 100 g of lignin A or lignin B and 100 g of phenolic resin A (mass ratio: lignin / phenolic resin = 5 / 5) were added, the temperature was raised to 180° C. and stirred for 30 minutes.

[0187] (2) Then, the mixture was stirred for 30 minutes under a reduced pressure of 5 mmHg while maintaining the temperature at 180° C. to remove volatile components, thereby finally obtaining a mixed resin in the form of a black-brown solid.

[0188] (3) The mixed resin is crushed into particles and fed into a nozzle having a thermometer, a nickel-chromium electric heating wire heater and a single hole at the bottom. The nozzle is heated to melt the mixed resin, and then nitrogen gas is applied from the top of the nozzle to extrude the melt for spinning.

[0189] (4) Next, the obtained fiber was immersed in an aqueous solution of 17.5-18.0% hydrochloric acid and 9.5-10.0% formalin in a plastic bottle and heated at about 95° C. for 7 hours to cause a curing reaction.

[0190] (5) After the curing reaction, neutralization, washing and drying are carried out to obtain dark brown lignin fibers.

[0191] (6) The fineness (denier) of the obtained lignin fiber was measured using a denier calculator (manufactured by SATCH Co., Ltd., DC-11B), and the strength and elongation were measured using a tensile testing machine (manufactured by ARD DYE Co., Ltd., RTG-1210, sample length: 20 mm, test speed: 20 mm / min).

[0192] (7) The lignin fibers obtained by the above (5) were placed in a crucible, and the temperature was raised from room temperature at 5°C / min under a nitrogen atmosphere. After being maintained at 300°C for 1 hour, the temperature was raised to 800°C at 5°C / min and maintained for 1 hour, thereby obtaining lignin carbon fibers.

[0193] (8) The obtained lignin carbon fiber was put into a crucible and placed in a horizontal tubular furnace, and the temperature was raised to 900°C at a heating rate of 5°C / min while nitrogen was flowing, and then nitrogen was introduced through warm water pre-adjusted to 80°C, thereby introducing water vapor at 4.125 mL / min into the aforementioned tubular furnace together with nitrogen, and heating was continued at 900°C for 60 minutes for activation. Then, by cooling while only nitrogen was introduced, lignin activated carbon fiber was obtained.

[0194] (9) About 50 mg of the obtained lignin activated carbon fiber was collected and dried in vacuum at 300°C for 4 hours under reduced pressure. The carbon fiber was then measured using a surface area-pore size distribution measuring apparatus (3Flex, manufactured by MICROMERITICS) at a relative pressure of 1.0 × 10 -7 The amount of nitrogen gas adsorbed at the boiling point of liquid nitrogen (-195.8°C) was measured in the range of 0.99 to 0.99, and an adsorption isotherm was prepared. The following calculation was performed based on the results.

[0195] [a] Calculate the BET specific surface area (m 2 / g).

[0196] [b] Calculation of micropore volume (cm) by MP method 3 / g) and micropore distribution.

[0197] [c] Calculate the mesopore volume (cm) by BJH method 3 / g) and mesopore distribution.

[0198] (10) The carbonization yield, activation yield and raw material yield were calculated by the following formula.

[0199] Carbonization yield (%) = (dry mass after carbonization (g) / dry mass before carbonization (g)) × 100

[0200] Activation yield (%) = (dry mass after activation (g) / dry mass before activation (g)) × 100

[0201] Raw material yield (%) = (carbonization yield (%) × activation yield (%)) / 100

[0202] (11) For lignin A, the above-mentioned operations (1) to (10) are carried out with a mixing ratio of lignin / phenolic resin = 5 / 95, 2 / 8, 5 / 5, 8 / 2, and 9 / 1. For lignin B, the above-mentioned operations (1) to (10) are carried out with a mixing ratio of lignin / phenolic resin = 5 / 95, 2 / 8, and 5 / 5.

[0203] <Example 9>

[0204] (12) Add 1250 g of lignin C and 1250 g of phenolic resin B (mass ratio: lignin / phenolic resin B = 5 / 5) to a reaction container (3 L flask), heat in an oven at 170°C for 5 hours to melt them, then install a thermometer, a stirring device and a condenser in the reaction container, and stir at 170°C for 60 minutes.

[0205] (13) Then, the mixture was stirred for 60 minutes under a reduced pressure of 5 mmHg while maintaining the temperature at 170° C. to remove volatile components, thereby finally obtaining a mixed resin in the form of a black-brown solid.

[0206] Thereafter, the same operations as in the above (3) to (10) were carried out to obtain lignin activated carbon fibers, except that only the activation time in the above (8) was set to 33 minutes.

[0207] <Comparative Example 1>

[0208] The same operations as in (6) to (10) above were carried out using phenolic resin fibers instead of lignin fibers to obtain phenolic resin activated carbon fibers.

[0209] <Comparative Examples 2 to 3>

[0210] Powdered lignin A or lignin B is used instead of lignin fibers, and the same operations as those in (7) to (10) are carried out to obtain powdered lignin activated carbon.

[0211] Table 1 shows the fineness and tensile test results of the lignin fibers of Examples 1 to 9 and the phenolic resin fiber of Comparative Example 1. Figure 1 This is a graph in which the lignin compounding ratio of the lignin fiber A of Examples 1 to 5 is plotted on the horizontal axis and the strength and elongation are plotted on the vertical axis. Figure 2 This is a graph with the lignin compounding ratio of the lignin fibers B of Examples 6 to 8 as the horizontal axis and the strength and elongation as the vertical axis. The lignin fibers containing lignin and a phenolic resin have sufficient strength and elongation.

[0212] Table 2 shows the yields of lignin activated carbon fibers, phenolic resin activated carbon fibers, and lignin activated carbon in the carbonization and activation treatments and the results of the specific surface area-pore distribution measurements. Figure 3 This is a graph in which the lignin compounding ratio of the lignin activated carbon fibers A of Examples 1 to 5 is plotted on the horizontal axis, and the raw material yield and the mesopore volume are plotted on the vertical axis. Figure 4 This is a graph in which the lignin compounding ratio of the lignin activated carbon fibers A of Examples 1 to 5 is plotted on the horizontal axis, and the raw material yield and specific surface area are plotted on the vertical axis. Figure 5 This is a graph in which the lignin compounding ratio of the lignin activated carbon fibers B of Examples 6 to 8 is plotted on the horizontal axis, and the raw material yield and the mesopore volume are plotted on the vertical axis. Figure 6 The graph shows the lignin blending ratio of the lignin activated carbon fibers B of Examples 6 to 8 as the horizontal axis and the raw material yield and specific surface area as the vertical axis. The maximum specific surface area of ​​the lignin activated carbon fibers was 2363 cm 2 / g, the maximum mesopore volume is 2.5200cm 3 / g, achieving high specific surface area and high mesopore volume.

[0213] Figure 7 , Figure 8 , Fig. 9 The pore distribution of each of lignin activated carbon fiber A obtained using lignin A, lignin activated carbon fiber B obtained using lignin B, and lignin activated carbon fiber C obtained using lignin C is shown in the figure. Regarding the peak of the pore distribution, in lignin activated carbon fiber A, when the lignin blending ratio is 5%, it appears at a pore diameter of 3.8nm, and when the lignin blending ratio is 20% or more, it appears at a pore diameter of 15nm; in lignin activated carbon fiber B, when the lignin blending ratio is 20%, it appears at a pore diameter of 3.8nm, and when the lignin blending ratio is 50%, it appears at a pore diameter of 15nm; in lignin activated carbon fiber C, when the lignin blending ratio is 50%, it appears at a pore diameter of 22nm.

[0214] Fig.10 : shows the pore distribution of the lignin activated carbons obtained in Comparative Examples 2 to 3. The peak of the pore distribution appears at a pore diameter of 9.9 nm in lignin activated carbon A obtained using lignin A, and appears at a pore diameter of 15 nm in lignin activated carbon obtained using lignin B.

[0215] [Table 1]

[0216]

[0217]

[0218] Table 1-2 and Figures 1 to 10 Here, "lignin compounding ratio" means the ratio (%) of lignin to the total mass of lignin and phenol resin, and "D" means denier (the same applies hereinafter).

[0219] <Examples 10 to 13>

[0220] The same operations as those in (1) to (5) of Example 3 were carried out to prepare lignin fibers A having a lignin blending ratio of 50% (lignin A / phenolic resin = 5 / 5).

[0221] The same operations as (7) to (10) were carried out on the lignin fibers A except that the activation time in (8) was changed to 10 minutes, 30 minutes, 45 minutes or 60 minutes, thereby obtaining lignin activated carbon fibers.

[0222] <Comparative Examples 4 to 6>

[0223] Phenolic resin activated carbon fibers were obtained by carrying out the same operations as those in (7) to (10) above except that phenolic resin fibers were used instead of lignin fibers and the activation time in (8) was changed to 10 minutes, 30 minutes or 60 minutes.

[0224] Table 3 Fig.11 , Fig.12 The yields of carbonization activation treatment at various activation times for lignin activated carbon fiber A and phenolic resin activated carbon fiber with a lignin blending ratio of 50% and the results of specific surface area-pore distribution measurement are shown in the figure. It is clear that in the case of lignin fiber A, the mesopore volume increases sharply after the activation time is 45 minutes, and the specific surface area is saturated at the activation time of 45 minutes.

[0225] Fig.13 The pore distribution at each activation time of lignin activated carbon fiber A with a lignin blending ratio of 50% is shown in the figure. The peak of the pore distribution appears at a pore diameter of 3.8 nm until the activation time is 30 minutes, at a pore diameter of 9.7 nm when the activation time is 45 minutes, and at a pore diameter of 15 nm when the activation time is 60 minutes.

[0226]

[0227] Industrial Applicability

[0228] According to the present invention, there can be provided activated carbon having a high specific surface area and a high mesopore volume obtained by carbonization and activation, a composition for producing activated carbon having excellent moldability and a method for producing the same; as well as an activated carbon molded body obtained using the activated carbon composition, a method for producing the same, fibers for producing activated carbon fibers, a method for producing the same, an activated carbon precursor, a carbide thereof, an activated carbon fiber precursor, carbon fibers, activated carbon, a method for producing the same, activated carbon fibers and a method for producing the same.

Claims

1. A composition for producing activated carbon, comprising a phenolic resin and lignin having a softening point of 100 to 175°C.

2. The composition for producing activated carbon according to claim 1, wherein The ash content of the lignin is 0.1 to 2.0% by mass.

3. The composition for producing activated carbon according to claim 1 or 2, wherein The phenolic resin is a novolac type phenolic resin.

4. The composition for producing activated carbon according to any one of claims 1 to 3, wherein The ratio of the lignin to the total mass of the lignin and the phenolic resin is 5 to 90 mass %.

5. A method for producing a composition for producing activated carbon, the method comprising producing the composition for producing activated carbon according to any one of claims 1 to 4, wherein: The lignin and the phenolic resin are melt-mixed at 160-200°C. 6 . A molded body for producing activated carbon, comprising the composition for producing activated carbon according to claim 1 .

7. A method for producing a molded body for producing activated carbon, which is a method for producing the molded body for producing activated carbon according to claim 6, wherein: The lignin and the phenolic resin are melt-mixed at 160-200° C., and the obtained mixture is molded.

8. Fibers for producing activated carbon fibers, comprising the composition for producing activated carbon according to any one of claims 1 to 4.

9. A method for producing a fiber for producing activated carbon fiber, which is a method for producing the fiber for producing activated carbon fiber according to claim 8, wherein: The lignin and the phenolic resin are melt-spun at 160-200°C. 10 . An activated carbon precursor comprising a solidified product of the composition for producing activated carbon according to claim 1 . The activated carbon precursor according to claim 10 , which is a shaped body. 12 . An activated carbon fiber precursor comprising a cured product of the composition for producing activated carbon according to claim 1 .

13. A carbide obtained by carbonizing the activated carbon precursor according to claim 10 or 11.

14. Carbon fiber obtained by carbonizing the activated carbon fiber precursor according to claim 12.

15. Activated carbon obtained by activating the carbide according to claim 13.

16. A method for producing activated carbon, wherein: The composition for producing activated carbon according to any one of claims 1 to 4 is solidified, the obtained solidified product is carbonized, and the obtained carbide is activated.

17. A method for producing activated carbon, wherein: The molded body for producing activated carbon according to claim 6 is solidified, the obtained solidified product is carbonized, and the obtained carbide is activated.

18. Activated carbon fiber obtained by activating the carbon fiber according to claim 14.

19. A method for producing activated carbon fibers, wherein: The fiber for producing activated carbon fiber according to claim 8 is cured, and the obtained cured product is carbonized to activate the obtained carbon fiber.