Polyamic acid, polyimide, non-thermoplastic polyimide film, multilayer polyimide film, and metal-clad laminate

By using a specific proportion of polyamic acid to prepare a non-thermoplastic polyimide film and a thermoplastic polyimide adhesive layer to form a multi-layer polyimide film and a metal-clad laminate, the dielectric loss angle in the existing technology is solved. The problem of tangent being difficult to reduce has been achieved, and low loss and high heat resistance of high-frequency circuit substrate materials have been achieved.

CN118749007APending Publication Date: 2024-10-08KANEKA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380023104.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-24
Filing Date
2023-02-13
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing polyimide films still have room for improvement in reducing dielectric loss tangent. Especially in the application of high-frequency circuit substrate materials, it is difficult to effectively suppress transmission losses.

Method used

Using a specific proportion of polyamic acid as a precursor, a non-thermoplastic polyimide film is prepared through an imidization reaction, and combined with a thermoplastic polyimide adhesive layer to form a multi-layer polyimide film and a metal-clad laminate. plate, optimizing the structure of the polymer to reduce the dielectric loss tangent.

Benefits of technology

It effectively reduces the dielectric loss tangent, improves the heat resistance and bendability of the material, is suitable for high-frequency circuit substrates, reduces transmission loss, and suppresses the generation of internal stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118749007A_ABST
    Figure CN118749007A_ABST
Patent Text Reader

Abstract

A polyamic acid according to the present invention has a tetracarboxylic dianhydride residue and a diamine residue. The tetracarboxylic dianhydride residues include a 3, 3 ', 4, 4'-biphenyl tetracarboxylic dianhydride residue and a 3, 3 ', 4, 4'-benzophenone tetracarboxylic dianhydride residue. The diamine residues comprise a p-phenylenediamine residue and a 1, 3-bis (4-aminophenoxy) benzene residue. The multilayer polyimide film (10) has a non-thermoplastic polyimide film (11) and an adhesive layer (12) that is disposed on at least one surface of the non-thermoplastic polyimide film (11) and contains a thermoplastic polyimide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to polyamic acid, polyimide, non-thermoplastic polyimide film, multilayer polyimide film and metal-clad laminate. Background Art

[0002] In recent years, with the expansion of demand for electronic products centered on smart phones, tablet computers, laptops, etc., the demand for flexible printed wiring boards (hereinafter sometimes recorded as "FPC") has continued to grow. Among them, FPC using a multilayer polyimide film having a non-thermoplastic polyimide layer (core layer) and a thermoplastic polyimide layer (adhesive layer) as a material is expected to further increase in demand due to its excellent heat resistance and flexibility. In addition, polyimide has sufficient heat resistance that can only adapt to high temperature processes, and its linear expansion coefficient is relatively small, so it is not easy to generate internal stress, and it is more suitable as a material for FPC.

[0003] In addition, in recent years, with the high-speed signal transmission of electronic devices, the requirements for low dielectric constant and low dielectric loss tangent of electronic substrate materials have been increasing to achieve high frequency of electrical signals propagated in circuits. In order to suppress the transmission loss of electrical signals, it is effective to reduce the dielectric constant and dielectric loss tangent of electronic substrate materials. In recent years, with the dawn of the IoT (Internet of Things) society, the trend of high frequency has been progressing, and substrate materials that can suppress transmission loss in areas above 10 GHz are needed.

[0004] Here, the transmission loss is expressed by the following formula using a proportionality constant (k), a frequency (f), a dielectric loss tangent (Df), and a relative dielectric constant (Dk). The contribution of the dielectric loss tangent to the transmission loss is greater than that of the relative dielectric constant. Therefore, in order to reduce the transmission loss, it is important to particularly reduce the dielectric loss tangent.

[0005] Transmission loss = k × f × Df × (Dk) 1 / 2

[0006] As a material used for a circuit board that can cope with high frequencies, a polyimide film (polyimide layer) that exhibits a low dielectric loss tangent is known (see, for example, Patent Documents 1 to 4).

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application No. 2014-526399

[0010] Patent Document 2: Japanese Patent Application Publication No. 2009-246201

[0011] Patent Document 3: International Publication No. 2018 / 079710

[0012] Patent Document 4: International Publication No. 2016 / 159060 Summary of the invention

[0013] Problem that the invention aims to solve

[0014] However, the techniques described in Patent Documents 1 to 4 still have room for improvement in terms of reducing the dielectric loss tangent.

[0015] The present invention is made in view of the above-mentioned problems, and its purpose is to provide a polyimide capable of reducing dielectric loss tangent and a polyamic acid as a precursor thereof. In addition, the present invention also aims to provide a non-thermoplastic polyimide film, a multilayer polyimide film and a metal-clad laminate produced using the polyimide and the polyamic acid.

[0016] Solutions for solving problems

[0017] <Modes of the Invention>

[0018] The present invention includes the following aspects.

[0019] [1] A polyamic acid having a tetracarboxylic dianhydride residue and a diamine residue,

[0020] The tetracarboxylic dianhydride residues include 3,3',4,4'-biphenyltetracarboxylic dianhydride residues and 3,3',4,4'-benzophenonetetracarboxylic dianhydride residues.

[0021] The diamine residues include a p-phenylenediamine residue and a 1,3-bis(4-aminophenoxy)benzene residue.

[0022] [2] The polyamic acid according to [1] above, wherein the content of the p-phenylenediamine residue is 75 mol% or more and 95 mol% or less relative to the total amount of the diamine residues.

[0023] [3] The polyamic acid according to [1] or [2], wherein the content of the 3,3′,4,4′-biphenyltetracarboxylic dianhydride residues is 55 mol% to 85 mol% based on the total amount of the tetracarboxylic dianhydride residues,

[0024] The content of the 3,3′,4,4′-benzophenonetetracarboxylic dianhydride residue is 10 mol % or more and 30 mol % or less relative to the total amount of the tetracarboxylic dianhydride residues.

[0025] [4] The polyamic acid according to [3] above, wherein the tetracarboxylic dianhydride residue further comprises a pyromellitic dianhydride residue,

[0026] The content of the pyromellitic dianhydride residue is 3 mol % or more and 15 mol % or less relative to the total amount of the tetracarboxylic dianhydride residues.

[0027] [5] A polyimide which is an imide of the polyamic acid according to any one of [1] to [4] above.

[0028] [6] A non-thermoplastic polyimide film comprising the polyimide described in [5] above.

[0029] [7] A multilayer polyimide film comprising the non-thermoplastic polyimide film according to [6] above and an adhesive layer, wherein the adhesive layer is disposed on at least one surface of the non-thermoplastic polyimide film and contains a thermoplastic polyimide.

[0030] [8] The multilayer polyimide film according to [7] above, wherein the adhesive layer is disposed on both surfaces of the non-thermoplastic polyimide film.

[0031] [9] A metal-clad laminate comprising the multilayer polyimide film according to [7] or [8] and a metal layer, wherein the metal layer is disposed on a main surface of at least one of the adhesive layers of the multilayer polyimide film.

[0032] Effects of the Invention

[0033] According to the present invention, a polyimide capable of reducing dielectric loss tangent and a polyamic acid as a precursor thereof can be provided. In addition, according to the present invention, a non-thermoplastic polyimide film, a multilayer polyimide film and a metal-clad laminate produced using the polyimide and the polyamic acid can also be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a cross-sectional view showing an example of the multilayer polyimide film of the present invention.

[0035] Figure 2 It is a cross-sectional view showing an example of the metal-clad laminate of the present invention. DETAILED DESCRIPTION

[0036] Hereinafter, preferred embodiments of the present invention will be described in detail, but the present invention is not limited thereto. In addition, all academic documents and patent documents described in this specification are incorporated herein by reference.

[0037] First, the terms used in this specification are explained. "Constitutional unit" refers to a repeating unit constituting a polymer. "Polyamic acid" is a polymer containing a structural unit represented by the following general formula (1) (hereinafter sometimes referred to as "structural unit (1)").

[0038]

[0039] In the general formula (1), A 1 represents a tetracarboxylic dianhydride residue (a tetravalent organic group derived from tetracarboxylic dianhydride), A 2 It represents a diamine residue (a divalent organic group derived from a diamine).

[0040] The content of the structural unit (1) relative to the total structural units constituting the polyamic acid is, for example, 50 mol% to 100 mol%, preferably 60 mol% to 100 mol%, more preferably 70 mol% to 100 mol%, further preferably 80 mol% to 100 mol%, further more preferably 90 mol% to 100 mol%, and may be 100 mol%.

[0041] Unless otherwise specified, the “linear expansion coefficient” refers to the linear expansion coefficient at elevated temperatures of 50° C. to 250° C. The linear expansion coefficient is measured in the same manner as in the following Examples or in accordance with the same method.

[0042] "Relative dielectric constant" is the relative dielectric constant at a frequency of 10 GHz, a temperature of 23°C, and a relative humidity of 50%. "Dielectric loss tangent" is the dielectric loss tangent at a frequency of 10 GHz, a temperature of 23°C, and a relative humidity of 50%. The relative dielectric constant and dielectric loss tangent are measured by the same method as in the following examples or by a method based thereon.

[0043] "Non-thermoplastic polyimide" refers to a polyimide that maintains a thin film shape (flat film shape) when fixed to a metal fixing frame in a thin film state and heated at a heating temperature of 380°C for 1 minute. "Thermoplastic polyimide" refers to a polyimide that does not maintain a thin film shape when fixed to a metal fixing frame in a thin film state and heated at a heating temperature of 380°C for 1 minute.

[0044] The "main surface" of a layered object (more specifically, a non-thermoplastic polyimide film, an adhesive layer, a multilayer polyimide film, a metal layer, etc.) refers to a surface perpendicular to the thickness direction of the layered object.

[0045] Hereinafter, the compound and its derivatives are sometimes collectively referred to by adding "system" after the compound name. In addition, tetracarboxylic dianhydride is sometimes recorded as "acid dianhydride". In addition, the non-thermoplastic polyimide contained in the non-thermoplastic polyimide film is sometimes simply recorded as "non-thermoplastic polyimide". In addition, the thermoplastic polyimide contained in the adhesive layer is sometimes simply recorded as "thermoplastic polyimide".

[0046] The components, functional groups, and the like exemplified in the present specification may be used alone or in combination of two or more unless otherwise specified.

[0047] For ease of understanding, the drawings referred to in the following description are schematically represented with each component as the main body, and for the convenience of drawing preparation, the size, number, shape, etc. of each component shown in the drawings are sometimes different from the actual ones. In addition, for the convenience of description, in the drawings described later, the same symbols are marked for the same components as the drawings described previously, and their descriptions are sometimes omitted.

[0048] <First Embodiment: Polyamic Acid>

[0049] The polyamic acid of the first embodiment of the present invention (hereinafter, sometimes described as "polyamic acid (1)") has a tetracarboxylic dianhydride residue and a diamine residue. The tetracarboxylic dianhydride residue contains a 3,3',4,4'-biphenyltetracarboxylic dianhydride residue and a 3,3',4,4'-benzophenonetetracarboxylic dianhydride residue. That is, the polyamic acid (1) contains a 3,3',4,4'-biphenyltetracarboxylic dianhydride residue and a 3,3',4,4'-benzophenonetetracarboxylic dianhydride residue as a tetracarboxylic dianhydride residue. In addition, the diamine residue contains a p-phenylenediamine residue and a 1,3-bis(4-aminophenoxy)benzene residue. That is, the polyamic acid (1) contains a p-phenylenediamine residue and a 1,3-bis(4-aminophenoxy)benzene residue as a diamine residue.

[0050] Hereinafter, 3,3',4,4'-biphenyltetracarboxylic dianhydride may be described as "BPDA". In addition, 3,3',4,4'-benzophenonetetracarboxylic dianhydride may be described as "BTDA". In addition, p-phenylenediamine may be described as "PDA". In addition, 1,3-bis(4-aminophenoxy)benzene may be described as "TPE-R". In addition, pyromellitic dianhydride may be described as "PMDA". In addition, 4,4'-oxydiphthalic anhydride may be described as "ODPA".

[0051] The polyimide obtained from the polyamic acid (1) can reduce the dielectric loss tangent. The reason for this is presumably as follows.

[0052] The polyamic acid (1) contains BPDA residues and BTDA residues as tetracarboxylic dianhydride residues, and contains PDA residues and TPE-R residues as diamine residues. In this way, there are residues having a rigid structure and residues having a curved structure in the polyamic acid (1), so the polyimide obtained from the polyamic acid (1) has a stable higher-order structure. Therefore, the dielectric loss tangent can be reduced by using the polyimide obtained from the polyamic acid (1).

[0053] The polyamic acid (1) may have other acid dianhydride residues in addition to the BPDA residue and the BTDA residue. Examples of the acid dianhydride (monomer) for forming other acid dianhydride residues (acid dianhydride residues other than BPDA residues and BTDA residues) include PMDA, ODPA, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 3,4'-oxydiphthalic anhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, ethylenebis(trimellitic acid monoester anhydride), bisphenol A bis(trimellitic acid monoester anhydride), and derivatives thereof.

[0054] In order to obtain a polyimide having improved heat resistance and further reduced dielectric loss tangent, a PMDA residue is preferably used as the other acid dianhydride residue.

[0055] In order to obtain a polyimide that can further reduce the dielectric loss tangent, the total content of BPDA residues and BTDA residues is preferably 80 mol% or more, and can be 85 mol% or more, 88 mol% or more, 90 mol% or more, or 92 mol% or more, and can also be 100 mol%, relative to all the acid dianhydride residues constituting the polyamic acid (1).

[0056] When PMDA residues are used as other acid dianhydride residues, in order to obtain a polyimide that can improve heat resistance and further reduce dielectric loss tangent, the total content of BPDA residues, BTDA residues and PMDA residues relative to all acid dianhydride residues constituting polyamic acid (1) is preferably 85 mol% or more, more preferably 90 mol% or more, and may also be 100 mol%.

[0057] In order to obtain a polyimide that can further reduce the dielectric loss tangent, the content of the BPDA residue is preferably 55 mol% to 85 mol%, more preferably 60 mol% to 80 mol%, and even more preferably 65 mol% to 78 mol%, relative to all the acid dianhydride residues constituting the polyamic acid (1).

[0058] In order to obtain a polyimide having a further reduced dielectric loss tangent, the content of the BTDA residue is preferably 10 mol % to 30 mol %, more preferably 15 mol % to 25 mol %, based on all the acid dianhydride residues constituting the polyamic acid (1).

[0059] In order to obtain a polyimide having improved heat resistance and further reduced dielectric loss tangent, the content of PMDA residues is preferably 3 mol % to 15 mol %, more preferably 5 mol % to 12 mol %, based on all acid dianhydride residues constituting the polyamic acid (1).

[0060] The polyamic acid (1) may have other diamine residues in addition to the PDA residue and the TPE-R residue. Examples of the diamine (monomer) for forming other diamine residues (diamine residues other than PDA residues and TPE-R residues) include 1,4-bis(4-aminophenoxy)benzene, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 1,5-diaminonaphthalene, 4,4'-diaminodiphenyldiethylsilane, 4,4'-diaminodiphenylsilane, 4,4'-diaminodiphenylethylphosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl N-aniline, 1,3-diaminobenzene, 1,2-diaminobenzene, and derivatives thereof.

[0061] In order to obtain a polyimide having a further reduced dielectric loss tangent, the total content of the PDA residues and the TPE-R residues is preferably 85 mol% or more, more preferably 90 mol% or more, further preferably 95 mol% or more, and may be 100 mol% based on all the diamine residues constituting the polyamic acid (1).

[0062] In order to obtain a polyimide that can further reduce the dielectric loss tangent, the content of the PDA residue is preferably 75 mol% to 95 mol%, more preferably 80 mol% to 95 mol%, and even more preferably 80 mol% to 90 mol%, relative to all the diamine residues constituting the polyamic acid (1).

[0063] In order to obtain a polyimide capable of further reducing the dielectric loss tangent, the content of the TPE-R residues relative to all the diamine residues constituting the polyamic acid (1) is preferably 2 mol% to 20 mol%, more preferably 5 mol% to 18 mol%, and even more preferably 10 mol% to 18 mol%.

[0064] In order to obtain a polyimide that can further reduce the dielectric loss tangent, the amount of the total amount of the acid dianhydride residues constituting the polyamic acid (1) divided by the total amount of the diamine residues constituting the polyamic acid (1) is preferably 0.95 or more and 1.05 or less, more preferably 0.97 or more and 1.03 or less, and further preferably 0.99 or more and 1.01 or less. By adjusting the above-mentioned amount of the substance ratio to 0.95 or more and 1.05 or less, the amount of the total amount of the acid dianhydride residues constituting the obtained polyimide is divided by the total amount of the diamine residues constituting the above-mentioned polyimide. The amount of the substance ratio obtained becomes 0.95 or more and 1.05 or less. An example of the method for synthesizing polyamic acid (1) will be described below.

[0065] In order to obtain a polyimide having a further reduced dielectric loss tangent and a small linear expansion coefficient, the polyamic acid (1) preferably satisfies the following condition 1, more preferably satisfies the following condition 2, further preferably satisfies the following condition 3, and particularly preferably satisfies the following condition 4.

[0066] Condition 1: The content of BPDA residues relative to all acid dianhydride residues constituting the polyamic acid (1) is 55 mol% to 85 mol%, and the content of BTDA residues relative to all acid dianhydride residues constituting the polyamic acid (1) is 10 mol% to 30 mol%.

[0067] Condition 2: The above-mentioned condition 1 is satisfied, and the polyamic acid (1) further has a PMDA residue as an acid dianhydride residue.

[0068] Condition 3: The above-mentioned condition 2 is satisfied, and the content of the PMDA residue relative to all the acid dianhydride residues constituting the polyamic acid (1) is 3 mol% or more and 15 mol% or less.

[0069] Condition 4: The above-mentioned condition 3 is satisfied, and the content of the PDA residue relative to all diamine residues constituting the polyamic acid (1) is 75 mol% or more and 95 mol% or less.

[0070] <Second Embodiment: Polyimide>

[0071] Next, the polyimide of the second embodiment of the present invention is described. The polyimide of the second embodiment is an imide of the above-mentioned polyamic acid (1). The polyimide of the second embodiment can be obtained by a known method, and its production method is not particularly limited. An example of a method for imidizing polyamic acid (1) will be described below.

[0072] <Third Embodiment: Non-Thermoplastic Polyimide Film>

[0073] Next, the non-thermoplastic polyimide film of the third embodiment of the present invention is described. The non-thermoplastic polyimide film of the third embodiment is a non-thermoplastic polyimide film containing the polyimide of the second embodiment (specifically, a non-thermoplastic polyimide which is an imide product of polyamic acid (1)).

[0074] The non-thermoplastic polyimide film of the third embodiment may contain ingredients (additives) other than the non-thermoplastic polyimide. As additives, for example, dyes, surfactants, leveling agents, plasticizers, silicones, fillers, sensitizers, etc. can be used. Relative to the total amount of the non-thermoplastic polyimide film, the content of the non-thermoplastic polyimide in the non-thermoplastic polyimide film is, for example, 70% by weight or more, preferably 80% by weight or more, more preferably 90% by weight or more, and may also be 100% by weight.

[0075] [Method for producing non-thermoplastic polyimide film]

[0076] The non-thermoplastic polyimide contained in the non-thermoplastic polyimide film is obtained by imidizing the polyamic acid (1) which is its precursor.

[0077] As a method for producing polyamic acid (1) (synthesis method), all known methods and methods combining them can be used. When producing polyamic acid (1), diamine and tetracarboxylic dianhydride are usually reacted in an organic solvent. The amount of diamine and the amount of tetracarboxylic dianhydride during the reaction are preferably substantially equal. When polyamic acid (1) is synthesized using diamine and tetracarboxylic dianhydride, the desired polyamic acid (1) (polymer of diamine and tetracarboxylic dianhydride) can be obtained by adjusting the amount of each diamine and the amount of each tetracarboxylic dianhydride. The molar fraction of each residue in polyamic acid (1) is consistent with the molar fraction of each monomer (diamine and tetracarboxylic dianhydride) used in the synthesis of polyamic acid (1). The temperature conditions of the reaction of diamine and tetracarboxylic dianhydride, i.e., the synthesis reaction of polyamic acid (1), are not particularly limited, and are, for example, in the range of 10°C or more and 150°C or less. The reaction time of the synthesis reaction of polyamic acid (1) is, for example, in the range of 10 minutes or more and 30 hours or less. In the present embodiment, any method of adding monomers may be used in the production of the polyamic acid (1). The following method may be mentioned as a typical method for producing the polyamic acid (1).

[0078] As a manufacturing method of a polyamic acid (1), the method of carrying out polymerization by following process (Aa) and process (Ab) (it may describe as "A polymerization method" below in some cases) is mentioned, for example.

[0079] (Aa): A step of reacting a diamine and an acid dianhydride in an organic solvent in a state where the diamine is in excess to obtain a prepolymer having amino groups at both ends

[0080] (Ab): A step of polymerizing by adding a diamine having a structure different from that used in step (Aa), and further adding an acid dianhydride having a structure different from that used in step (Aa) so that the diamine and the acid dianhydride in all steps are substantially equimolar.

[0081] Moreover, as a manufacturing method of the polyamic acid (1), the method of polymerizing by following process (Ba) and process (Bb) (it may describe as "B polymerization method" below) is mentioned.

[0082] (Ba): A step of reacting a diamine and an acid dianhydride in an organic solvent in a state where the acid dianhydride is in excess to obtain a prepolymer having an acid anhydride group at both ends

[0083] (Bb): A step of polymerizing by adding an acid dianhydride having a structure different from that used in step (Ba), and further adding a diamine having a structure different from that used in step (Ba) so that the diamine and the acid dianhydride in all steps are substantially equimolar.

[0084] In this specification, a polymerization method (such as the above-mentioned A polymerization method, B polymerization method, etc.) in which the addition order is set in a manner that a specific diamine or a specific acid dianhydride selectively reacts with an arbitrary or specific diamine or an arbitrary or specific acid dianhydride is described as sequential polymerization. In contrast, in this specification, a polymerization method (a polymerization method in which monomers react arbitrarily with each other) in which the addition order of diamine and acid dianhydride is not set is described as random polymerization. In addition, in the case of sequential polymerization in two stages as in the A polymerization method or the B polymerization method, in this specification, the first half of the process (process (Aa), process (Ba), etc.) is described as "1st sequential polymerization process", and the second half of the process (process (Ab), process (Bb), etc.) is described as "2nd sequential polymerization process".

[0085] In this embodiment, in order to obtain a non-thermoplastic polyimide film with a further reduced dielectric loss tangent, the polymerization method of the polyamic acid (1) is preferably sequential polymerization.

[0086] When obtaining the non-thermoplastic polyimide, a method of obtaining the non-thermoplastic polyimide from a polyamic acid solution containing the polyamic acid (1) and an organic solvent can be adopted. As the organic solvent that can be used in the polyamic acid solution, for example, urea solvents such as tetramethylurea and N,N-dimethylethylurea; sulfoxide solvents such as dimethyl sulfoxide; sulfone solvents such as diphenyl sulfone and tetramethyl sulfone; amide solvents such as N,N-dimethylacetamide, N,N-dimethylformamide (hereinafter, sometimes recorded as "DMF"), N,N-diethylacetamide, N-methyl-2-pyrrolidone, and hexamethylphosphoric acid triamide; ester solvents such as γ-butyrolactone; halogenated alkane solvents such as chloroform and dichloromethane; aromatic hydrocarbon solvents such as benzene and toluene; phenol solvents such as phenol and cresol; ketone solvents such as cyclopentanone; ether solvents such as tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, dimethyl ether, diethyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, and p-cresol methyl ether. These solvents are usually used alone, and two or more of them can be appropriately combined as needed. When the polyamic acid (1) is obtained by the above-mentioned polymerization method, the reaction solution (reacted solution) itself can be used as a polyamic acid solution for obtaining a non-thermoplastic polyimide. In this case, the organic solvent in the polyamic acid solution is the organic solvent used for the reaction in the above-mentioned polymerization method. In addition, the solid polyamic acid (1) obtained by removing the solvent from the reaction solution can be dissolved in an organic solvent to prepare the polyamic acid solution.

[0087] In the polyamic acid solution, additives such as dyes, surfactants, leveling agents, plasticizers, silicones, fillers, sensitizers, etc. may be added. The concentration of the polyamic acid (1) in the polyamic acid solution is not particularly limited, and is, for example, 5% by weight or more and 35% by weight or less, preferably 8% by weight or more and 30% by weight or less, relative to the total amount of the polyamic acid solution. When the concentration of the polyamic acid (1) is 5% by weight or more and 35% by weight or less, a suitable molecular weight and solution viscosity may be obtained.

[0088] The method for obtaining a non-thermoplastic polyimide film using a polyamic acid solution is not particularly limited, and various known methods can be applied. For example, a method of obtaining a non-thermoplastic polyimide film through the following steps i) to iii) can be mentioned.

[0089] Step i): a step of coating a dope solution containing a polyamic acid solution on a support to form a coating film

[0090] Step ii): After drying the above-mentioned coating film on a support to prepare a self-supporting polyamic acid film (hereinafter sometimes referred to as a "gel film"), a step of peeling the gel film from the support

[0091] Step iii): a step of heating the gel film to imidize the polyamic acid (1) in the gel film to obtain a non-thermoplastic polyimide film containing non-thermoplastic polyimide

[0092] The method of obtaining a non-thermoplastic polyimide film through steps i) to iii) is roughly divided into a thermal imidization method and a chemical imidization method. The thermal imidization method is a method in which a polyamic acid solution is applied as a doping liquid on a support without using a dehydrating ring-closing agent, etc., and the polyamic acid solution is heated to promote imidization. Another chemical imidization method is a method in which at least one of a dehydrating ring-closing agent and a catalyst is added to a polyamic acid solution as a doping liquid to promote imidization. Either method can be used, but the chemical imidization method has excellent productivity.

[0093] As a dehydration ring-closing agent, an acid anhydride represented by acetic anhydride is suitably used. As a catalyst, tertiary amines such as aliphatic tertiary amines, aromatic tertiary amines, heterocyclic tertiary amines (more specifically, isoquinoline, etc.) are suitably used. When adding at least one of the dehydration ring-closing agent and the catalyst in the polyamic acid solution, it can be directly added without being dissolved in an organic solvent, or it can be added and dissolved in an organic solvent. In the method of directly adding without being dissolved in an organic solvent, sometimes the reaction is rapidly carried out before at least one of the dehydration ring-closing agent and the catalyst diffuses to generate a gel. Therefore, it is preferred to add a solution (imidization accelerator) obtained by dissolving at least one of the dehydration ring-closing agent and the catalyst in an organic solvent in the polyamic acid solution.

[0094] In step i), the method for coating the doping liquid on the support is not particularly limited, and a method using a conventionally known coating apparatus such as a die coater, a comma coater (registered trademark), a reverse coater, or a knife coater can be used.

[0095] As the support body on which the doping liquid is applied in step i), a glass plate, an aluminum foil, an endless stainless steel belt, a stainless steel drum, etc. are preferably used. In step ii), the drying conditions (heating conditions) of the coating film are set according to the thickness of the film finally obtained and the production speed, and the dried polyamic acid film (gel film) is peeled off from the support body. The drying temperature of the coating film is, for example, 50° C. or more and 200° C. or less. In addition, the drying time when the coating film is dried is, for example, 1 minute or more and 100 minutes or less.

[0096] Next, in step iii), for example, by fixing the ends of the above-mentioned gel film, heat treatment is performed while avoiding shrinkage during curing, and water, residual solvent, imidization accelerator, etc. are removed from the gel film, and the remaining polyamic acid (1) is completely imidized, so that a non-thermoplastic polyimide film containing a non-thermoplastic polyimide can be obtained. The heating conditions are appropriately set according to the thickness of the film finally obtained and the production speed. As the heating conditions of step iii), the maximum temperature is, for example, above 370°C and below 420°C, and the heating time at the maximum temperature is, for example, above 10 seconds and below 180 seconds. In addition, any temperature can be maintained for any time before reaching the maximum temperature. Step iii) can be carried out in air, under reduced pressure, or in an inert gas such as nitrogen. There is no particular limitation on the heating device that can be used in step iii), and examples thereof include a hot air circulation oven, a far infrared oven, etc.

[0097] The non-thermoplastic polyimide film thus obtained can reduce the dielectric loss tangent and is therefore suitable, for example, as a material for a high-frequency circuit board (more specifically, a core layer of a multilayer polyimide film, an insulating layer of a metal-clad laminate, etc.).

[0098] [Physical properties of non-thermoplastic polyimide films]

[0099] In order to reduce transmission loss, the relative dielectric constant of the non-thermoplastic polyimide film is preferably 3.70 or less. In order to reduce transmission loss, the dielectric loss tangent of the non-thermoplastic polyimide film is preferably 0.0050 or less, more preferably 0.0040 or less, and further preferably 0.0030 or less.

[0100] In order to suppress the generation of internal stress when used in FPC, the linear expansion coefficient of the non-thermoplastic polyimide film is preferably 25 ppm / K or less, more preferably 18 ppm / K or less, and further preferably 16 ppm / K or less.

[0101] The thickness of the non-thermoplastic polyimide film is not particularly limited, and is, for example, 5 μm or more and 50 μm or less. The thickness of the non-thermoplastic polyimide film can be measured using a laser hologram micrometer.

[0102] <Fourth Embodiment: Multilayer Polyimide Film>

[0103] Next, a multilayer polyimide film according to a fourth embodiment of the present invention is described. The multilayer polyimide film according to the fourth embodiment comprises the non-thermoplastic polyimide film according to the third embodiment and an adhesive layer comprising thermoplastic polyimide. In addition, in the following description, the description of the contents overlapping with the first to third embodiments is sometimes omitted.

[0104] Figure 1 1 is a cross-sectional view showing an example of a multilayer polyimide film according to a fourth embodiment. Figure 1 As shown, the multilayer polyimide film 10 includes a non-thermoplastic polyimide film 11 and an adhesive layer 12 made of thermoplastic polyimide and disposed on at least one surface (one main surface) of the non-thermoplastic polyimide film 11 .

[0105] In addition, Figure 1 In the multilayer polyimide film 10 shown, the adhesive layer 12 is provided only on one side of the non-thermoplastic polyimide film 11, but the adhesive layer 12 may be provided on both sides (both main sides) of the non-thermoplastic polyimide film 11. In the case where the adhesive layer 12 is provided on both sides of the non-thermoplastic polyimide film 11, the two adhesive layers 12 may contain the same polyimide or different types of polyimides. In addition, the thickness of the two adhesive layers 12 may be the same or different. In the following description, the "multilayer polyimide film 10" includes a film in which the adhesive layer 12 is provided only on one side of the non-thermoplastic polyimide film 11, and a film in which the adhesive layer 12 is provided on both sides of the non-thermoplastic polyimide film 11.

[0106] The thickness of the multilayer polyimide film 10 (the total thickness of each layer) is, for example, 6 μm or more and 60 μm or less. The thinner the thickness of the multilayer polyimide film 10, the easier it is to lightweight the obtained FPC, and the bending property of the obtained FPC is improved. In order to ensure mechanical strength and make the FPC easy to lightweight, and to improve the bending property of the FPC, the thickness of the multilayer polyimide film 10 is preferably 7 μm or more and 60 μm or less, and more preferably 10 μm or more and 60 μm or less. The thickness of the multilayer polyimide film 10 can be measured using a laser holographic micrometer.

[0107] In order to ensure adhesion with the metal foil and to easily reduce the thickness of the FPC, the thickness of the adhesive layer 12 (the thickness of each adhesive layer 12 when two adhesive layers 12 are provided) is preferably 1 μm or more and 15 μm or less.

[0108] In addition, in order to easily adjust the linear expansion coefficient of the multilayer polyimide film 10, the thickness ratio of the non-thermoplastic polyimide film 11 and the adhesive layer 12 (the thickness of the non-thermoplastic polyimide film 11 / the thickness of the adhesive layer 12) is preferably 55 / 45 or more and 95 / 5 or less. In the case where two layers of the adhesive layer 12 are provided, the thickness of the adhesive layer 12 when calculating the thickness ratio is the total thickness of the adhesive layer 12.

[0109] In order to suppress the warping of the multilayer polyimide film 10, it is preferable to provide adhesive layers 12 on both sides of the non-thermoplastic polyimide film 11, and it is more preferable to provide adhesive layers 12 containing the same polyimide on both sides of the non-thermoplastic polyimide film 11. In the case where adhesive layers 12 are provided on both sides of the non-thermoplastic polyimide film 11, in order to suppress the warping of the multilayer polyimide film 10, the thickness of the two adhesive layers 12 is preferably the same. In addition, even if the thickness of the two adhesive layers 12 is different from each other, if the thickness of the other adhesive layer 12 is within a range of 40% or more and less than 100% based on the thickness of the thicker adhesive layer 12, the warping of the multilayer polyimide film 10 can be suppressed.

[0110] [Adhesive layer 12]

[0111] The thermoplastic polyimide contained in the adhesive layer 12 has an acid dianhydride residue and a diamine residue. As the acid dianhydride (monomer) used to form the acid dianhydride residue in the thermoplastic polyimide, the same compound as the acid dianhydride (monomer) used to form the acid dianhydride residue in the non-thermoplastic polyimide can be cited. The acid dianhydride residue of the thermoplastic polyimide and the acid dianhydride residue of the non-thermoplastic polyimide may be of the same type or different types.

[0112] In order to ensure thermoplasticity, as the diamine residue possessed by the thermoplastic polyimide, a diamine residue having a bent structure is preferably present. In order to more easily ensure thermoplasticity, the content of the diamine residue having a bent structure is preferably 50 mol% or more, more preferably 70 mol% or more, and further preferably 80 mol% or more, and may also be 100 mol% relative to all the diamine residues constituting the thermoplastic polyimide. As a diamine (monomer) for forming a diamine residue having a bent structure, examples include: 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 1,3-bis(3-aminophenoxy)benzene, TPE-R, 2,2-bis[4-(4-aminophenoxy)phenyl]propane (hereinafter, sometimes described as "BAPP"), etc. In order to more easily ensure thermoplasticity, as the diamine residue possessed by the thermoplastic polyimide, a BAPP residue is preferably present.

[0113] In order to obtain the adhesive layer 12 having excellent adhesion to the metal foil, the thermoplastic polyimide preferably contains one or more selected from the group consisting of BPDA residues and PMDA residues and a BAPP residue.

[0114] The adhesive layer 12 may also contain ingredients (additives) other than the thermoplastic polyimide. As additives, for example, dyes, surfactants, leveling agents, plasticizers, silicones, fillers, sensitizers, etc. can be used. The content of the thermoplastic polyimide in the adhesive layer 12 is, for example, 70% by weight or more, preferably 80% by weight or more, more preferably 90% by weight or more, and may also be 100% by weight relative to the total amount of the adhesive layer 12.

[0115] (Method for Forming Adhesive Layer 12)

[0116] The adhesive layer 12 is formed, for example, by applying a polyamic acid solution (hereinafter, sometimes described as "thermoplastic polyamic acid solution") containing polyamic acid as a precursor of thermoplastic polyimide to at least one side of the non-thermoplastic polyimide film 11, and then heating (drying and imidization of polyamic acid). By this method, a multilayer polyimide film 10 having a non-thermoplastic polyimide film 11 and an adhesive layer 12 disposed on at least one side of the non-thermoplastic polyimide film 11 can be obtained. In addition, a solution containing thermoplastic polyimide (thermoplastic polyimide solution) can be used instead of the thermoplastic polyamic acid solution, and a coating film formed by the thermoplastic polyimide solution is formed on at least one side of the non-thermoplastic polyimide film 11, and the coating film is dried to form the adhesive layer 12.

[0117] Alternatively, for example, a coextrusion die may be used to form a laminate having a layer of polyamic acid, which is a precursor of the non-thermoplastic polyimide in the non-thermoplastic polyimide film 11, and a layer of polyamic acid, which is a precursor of the thermoplastic polyimide, on a support, and then the obtained laminate is heated to simultaneously form the non-thermoplastic polyimide film 11 and the adhesive layer 12. In this method, by using a metal foil as a support, a metal-clad laminate (a laminate of a multilayer polyimide film 10 and a metal foil) can be obtained while completing imidization.

[0118] When manufacturing a multilayer polyimide film 10 comprising three polyimide layers, it is appropriate to repeat the above-mentioned coating process and heating process for multiple times, or to form multiple coating films by coextrusion or continuous coating (continuous casting) and to heat them simultaneously. The outermost surface of the multilayer polyimide film 10 may also be subjected to various surface treatments such as corona treatment and plasma treatment.

[0119] <Fifth Embodiment: Metal-Clad Laminated Plate>

[0120] Next, a metal-clad laminate according to a fifth embodiment of the present invention is described. The metal-clad laminate according to the fifth embodiment comprises the multilayer polyimide film according to the fourth embodiment and a metal layer disposed on a main surface of at least one adhesive layer of the multilayer polyimide film. In the following description, the description of the contents repeated in the first to fourth embodiments is sometimes omitted.

[0121] Figure 2 1 is a cross-sectional view showing an example of a metal-clad laminate according to a fifth embodiment. Figure 2 As shown, the metal-clad laminate 20 includes a multilayer polyimide film 10 and a metal layer 13 (metal foil) disposed on a main surface 12 a of an adhesive layer 12 of the multilayer polyimide film 10 .

[0122] [Method of Manufacturing Metal-Clad Laminated Plate 20]

[0123] When the metal-clad laminate 20 is manufactured using the multilayer polyimide film 10, at least one surface (for example, Figure 2 In the case of the non-thermoplastic polyimide film 11 side of the adhesive layer 12, the main surface 12a) on the opposite side is bonded to the metal foil as the metal layer 13. Thus, it can be obtained Figure 2 The metal-clad laminate 20 shown. There is no particular limitation on the method of laminating the metal foil on the main surface 12a of the adhesive layer 12, and various known methods can be used. For example, a continuous processing method using a hot roll laminating device or a double belt press (DBP) having a pair of or more metal rollers can be used. The specific structure of the device for hot roll lamination is not particularly limited, and in order to make the appearance of the obtained metal-clad laminate 20 good, it is preferred to configure a protective material between the pressurized surface and the metal foil.

[0124] When the adhesive layer 12 is provided on both surfaces of the non-thermoplastic polyimide film 11, a double-sided metal-clad laminate (not shown) can be obtained by laminating metal foils on both surfaces (two main surfaces) of the multilayer polyimide film 10.

[0125] The metal foil as the metal layer 13 is not particularly limited, and all metal foils can be used. For example, metal foils made of copper, stainless steel, nickel, aluminum, and alloys of these metals are suitable. In addition, in common metal-clad laminates, copper foils such as rolled copper foil and electrolytic copper foil are mostly used. In the fifth embodiment, copper foil is also preferably used. In addition, the metal foil can be used to adjust the surface roughness according to the purpose of surface treatment. Furthermore, a rust-proof layer, a heat-resistant layer, an adhesive layer, etc. can also be formed on the surface of the metal foil. There is no particular limitation on the thickness of the metal foil, as long as it is a thickness that can fully function according to its use. In order to suppress the generation of wrinkles when laminating with the multilayer polyimide film 10 and easily realize the thinning of the FPC, the thickness of the metal foil is preferably 5 μm or more and 50 μm or less.

[0126] Example

[0127] Hereinafter, the present invention will be specifically described using examples, but the present invention is not limited to these examples.

[0128] <Measurement Methods of Physical Properties>

[0129] First, the method for measuring the relative dielectric constant, dielectric loss tangent, and linear expansion coefficient of the polyimide film will be described.

[0130] [Relative dielectric constant and dielectric loss tangent]

[0131] The relative dielectric constant and dielectric loss tangent of the polyimide film are measured by a network analyzer ("8719C" manufactured by Hewlett-Packard) and a cavity resonator dielectric constant measuring device ("CP531" manufactured by EMLAB). In detail, first, the polyimide film is cut into 2mm×100mm, and a sample for measuring the relative dielectric constant and dielectric loss tangent is prepared. Then, after the sample for measurement is placed in an atmosphere with a temperature of 23°C and a relative humidity of 50% for 24 hours, the relative dielectric constant and dielectric loss tangent are measured under the conditions of a temperature of 23°C, a relative humidity of 50%, and a measurement frequency of 10GHz using the above-mentioned network analyzer and the above-mentioned cavity resonator dielectric constant measuring device. When the dielectric loss tangent is less than 0.0030, it is evaluated as "the dielectric loss tangent can be reduced". On the other hand, when the dielectric loss tangent exceeds 0.0030, it is evaluated as "the dielectric loss tangent cannot be reduced".

[0132] [Coefficient of linear expansion (CTE)]

[0133] Using a thermal analyzer ("TMA / SS6100" manufactured by Hitachi High-Tech Science), the polyimide film (sample) was heated from -10°C to 300°C at a heating rate of 10°C / min, and then cooled to -10°C at a cooling rate of 40°C / min. Next, the sample was heated again to 300°C at a heating rate of 10°C / min, and the linear expansion coefficient was obtained from the strain at 50°C to 250°C during the second heating. The measurement conditions are shown below.

[0134] The size of the sample (polyimide film): width 3 mm, length 10 mm

[0135] Load: 1g

[0136] Measurement atmosphere: air atmosphere

[0137] <Production of Polyimide Film>

[0138] The following is a description of the method for preparing the polyimide film of the examples and comparative examples. In addition, the following abbreviations are used to describe the types of compounds and reagents. In addition, the preparation of the polyamic acid solution used in the preparation of the polyimide film was carried out in a nitrogen atmosphere at a temperature of 20°C.

[0139] DMF: N,N-dimethylformamide

[0140] PDA: p-phenylenediamine

[0141] TPE-R: 1,3-bis(4-aminophenoxy)benzene

[0142] BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane

[0143] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0144] PMDA: Pyromellitic Dianhydride

[0145] BTDA: 3,3',4,4'-Benzophenonetetracarboxylic dianhydride

[0146] ODPA: 4,4'-oxydiphthalic anhydride

[0147] AA: Acetic anhydride

[0148] IQ: Isoquinoline

[0149] [Example 1]

[0150] (1st sequential polymerization process)

[0151] After adding 314.58 g of DMF and 10.11 g of PDA to a 2000 mL glass flask, 16.25 g of BPDA, 1.54 g of PMDA, and 8.67 g of BTDA were added to the flask while stirring the contents of the flask. The contents of the flask were then stirred for 30 minutes.

[0152] (2nd sequential polymerization step)

[0153] Then, while stirring the contents of the flask, 16.85g of a pre-prepared PDA solution (solvent: DMF, PDA concentration: 20% by weight) and 4.97g of TPE-R were slowly added to the flask. After visually confirming that the TPE-R had dissolved, 14.17g of BPDA was added to the flask while stirring the contents of the flask, and the contents of the flask were stirred for 30 minutes. Next, the pre-prepared PMDA solution (solvent: DMF, PMDA dissolution amount: 0.93g, PMDA concentration: 7.2% by weight) was continuously added to the flask for a prescribed time at a rate such that the viscosity of the contents of the flask would not rise sharply. Then, the addition of the PMDA solution was stopped at a time point when the viscosity of the contents of the flask reached 1500 poise at a temperature of 23°C, and the contents of the flask were stirred for 1 hour to obtain a polyamic acid solution. The solid content concentration of the obtained polyamic acid solution is 15% by weight. The viscosity of the obtained polyamic acid solution at a temperature of 23° C. was 1500 to 2000 poise.

[0154] (Film-making process)

[0155] Next, 27.5 g of an imidization accelerator (weight ratio: AA / IQ / DMF=42 / 21 / 37) containing a mixture of AA, IQ and DMF was added to 55 g of a polyamic acid solution (the polyamic acid solution obtained according to the above preparation method) to prepare a doping solution. Next, in an atmosphere at a temperature below 0°C, the doping solution was stirred while degassing, and then the doping solution was coated on an aluminum foil using a notch wheel coater to form a coating film. Next, a self-supporting gel film was obtained by heating the coating film at a heating temperature of 110°C for 160 seconds. The obtained gel film was peeled off from the aluminum foil, fixed on a metal fixing frame, placed in a hot air circulation oven preheated to a temperature of 300°C, and heated at a heating temperature of 300°C for 56 seconds. Next, the heated film was placed in a far infrared (IR) oven preheated to 380°C and heated at 380°C for 49 seconds to imidize the polyamic acid in the gel film. The film was then cut from a metal fixing frame to obtain a polyimide film of Example 1 (thickness: 17 μm).

[0156] In addition, the polyimide film obtained by the same steps as above was fixed on a metal fixing frame and heated at a heating temperature of 380°C for 1 minute using an IR oven. As a result, it was found that the shape of the polyimide film (film shape) was maintained. Therefore, the polyimide contained in the polyimide film of Example 1 is a non-thermoplastic polyimide. In other words, the polyimide film of Example 1 is a non-thermoplastic polyimide film. Regarding the polyimide films of Examples 2 to 12 described below, the polyimide films obtained by the same steps as below were also fixed on a metal fixing frame, and heated at a heating temperature of 380°C for 1 minute using an IR oven. As a result, it was found that the shape of the polyimide film (film shape) was maintained. Therefore, the polyimide contained in the polyimide films of Examples 2 to 12 are all non-thermoplastic polyimide. In other words, the polyimide films of Examples 2 to 12 are all non-thermoplastic polyimide.

[0157] [Examples 2 to 12]

[0158] The types and ratios (input ratios) of monomers used in the 1st sequential polymerization step and the types and ratios (input ratios) of monomers used in the 2nd sequential polymerization step were as shown in Tables 1 and 2 below, and polyimide films (thickness: all 17 μm) of Examples 2 to 12 were obtained in the same manner as in Example 1. In addition, the total amount of acid dianhydride and diamine in any of Examples 2 to 12 was the same as in Example 1.

[0159] [Comparative Example 1]

[0160] A polyimide film (thickness: 17 μm) of Comparative Example 1 was obtained in the same manner as in Example 1 except that the 1st sequential polymerization step and the 2nd sequential polymerization step were changed as shown below.

[0161] (1st sequential polymerization step of Comparative Example 1)

[0162] After adding 315.40 g of DMF and 9.78 g of PDA to a 2000 mL glass flask, 15.72 g of BPDA, 1.49 g of PMDA, and 8.39 g of BTDA were added to the flask while stirring the contents in the flask. The contents in the flask were then stirred for 30 minutes.

[0163] (2nd sequential polymerization step of Comparative Example 1)

[0164] Next, while stirring the contents of the flask, 16.30 g of a pre-prepared PDA solution (solvent: DMF, PDA concentration: 20% by weight) and 6.75 g of BAPP were slowly added to the flask. After visually confirming that BAPP had dissolved, 13.71 g of BPDA was added to the flask while stirring the contents of the flask, and the contents of the flask were stirred for 30 minutes. Next, the pre-prepared PMDA solution (solvent: DMF, PMDA dissolution amount: 0.90 g, PMDA concentration: 7.2% by weight) was continuously added to the flask for a specified time at a rate such that the viscosity of the contents of the flask would not rise sharply. Then, the addition of the PMDA solution was stopped at a time point when the viscosity of the contents of the flask at a temperature of 23°C reached 1500 poise, and the contents of the flask were stirred for 1 hour to obtain a polyamic acid solution. The solid content concentration of the obtained polyamic acid solution was 15% by weight. In addition, the viscosity of the obtained polyamic acid solution at a temperature of 23°C was 1500 to 2000 poise.

[0165] [Comparative Example 2]

[0166] A polyimide film (thickness: 17 μm) of Comparative Example 2 was obtained in the same manner as in Example 1 except that the polyamic acid solution was prepared by the method shown below (random polymerization).

[0167] (Preparation method of polyamic acid solution of Comparative Example 2)

[0168] After adding 165.61g of DMF, 2.08g of TPE-R and 6.71g of PDA to a glass flask of 500mL, 20.98g of BPDA was added to the flask while stirring the contents of the flask. Then, the contents of the flask were stirred for 60 minutes to obtain a polyamic acid solution. The solid content concentration of the obtained polyamic acid solution was 15% by weight. In addition, the viscosity of the obtained polyamic acid solution at a temperature of 23°C was 1500 poise.

[0169] [Comparative Example 3]

[0170] A polyimide film (thickness: 17 μm) of Comparative Example 3 was obtained in the same manner as in Example 1 except that the polyamic acid solution was prepared by the method shown below (random polymerization).

[0171] (Preparation method of polyamic acid solution of Comparative Example 3)

[0172] After adding 160.84g of DMF and 7.95g of PDA to a glass flask with a capacity of 500mL, 17.31g of BPDA and 4.03g of BTDA were added to the flask while stirring the contents of the flask. Then, the contents of the flask were stirred for 30 minutes. Next, the pre-prepared BTDA solution (solvent: DMF, BTDA dissolution amount: 0.71g, BTDA concentration: 7.2 wt%) was added to the flask continuously for a specified time at a rate such that the viscosity of the contents of the flask would not rise sharply. Then, the addition of the BTDA solution was stopped at the time point when the viscosity of the contents of the flask at a temperature of 23°C reached 1500 poise, and the contents of the flask were stirred for 1 hour to obtain a polyamic acid solution. The solid content concentration of the obtained polyamic acid solution was 15 wt%. In addition, the viscosity of the obtained polyamic acid solution at a temperature of 23°C was 1500 to 2000 poise.

[0173] [Comparative Example 4]

[0174] A polyimide film (thickness: 17 μm) of Comparative Example 4 was obtained in the same manner as in Example 1 except that the polyamic acid solution was prepared by the method shown below (random polymerization).

[0175] (Preparation method of polyamic acid solution of Comparative Example 4)

[0176] After adding 163.95g of DMF, 6.59g of PDA and 3.14g of TPE-R to a glass flask with a capacity of 500mL, 15.57g of ODPA and 4.22g of PMDA were added to the flask while stirring the contents of the flask. Then, the contents of the flask were stirred for 30 minutes. Then, the pre-prepared PMDA solution (solvent: DMF, PMDA dissolution amount: 0.47g, PMDA concentration: 7.2 wt%) was added to the flask continuously for a specified time at a rate such that the viscosity of the flask contents would not rise sharply. Then, the addition of PMDA solution was stopped at a time point when the viscosity of the flask contents at a temperature of 23°C reached 1500 poise, and the flask contents were stirred for 1 hour to obtain a polyamic acid solution. The solid content concentration of the obtained polyamic acid solution was 15 wt%. In addition, the viscosity of the obtained polyamic acid solution at a temperature of 23°C was 1500 to 2000 poise.

[0177] [Comparative Example 5]

[0178] A polyimide film (thickness: 17 μm) of Comparative Example 5 was obtained in the same manner as in Example 1 except that the polyamic acid solution was prepared by the method shown below (random polymerization).

[0179] (Preparation method of polyamic acid solution of Comparative Example 5)

[0180] After adding 163.88g of DMF, 7.07g of PDA and 2.12g of TPE-R to a glass flask with a capacity of 500mL, 19.23g of BPDA and 1.11g of PMDA were added to the flask while stirring the contents of the flask. Then, the contents of the flask were stirred for 30 minutes. Then, the pre-prepared PMDA solution (solvent: DMF, PMDA dissolution amount: 0.48g, PMDA concentration: 7.2% by weight) was continuously added to the flask for a predetermined time at a rate such that the viscosity of the flask contents would not rise sharply. Then, the addition of PMDA solution was stopped at a time point when the viscosity of the flask contents at a temperature of 23°C reached 1500 poise, and the flask contents were stirred for 1 hour to obtain a polyamic acid solution. The solid content concentration of the obtained polyamic acid solution was 15% by weight. In addition, the viscosity of the obtained polyamic acid solution at a temperature of 23°C was 1500 to 2000 poise.

[0181] <Results>

[0182] Regarding Examples 1 to 12 and Comparative Examples 1 to 5, the types of monomers used in the 1st sequential polymerization step and their ratios (input ratios), the types of monomers used in the 2nd sequential polymerization step and their ratios (input ratios), the relative dielectric constant, the dielectric loss tangent and the CTE are shown in Tables 1 and 2.

[0183] In Tables 1 and 2, "1st" and "2nd" refer to "1st sequential polymerization step" and "2nd sequential polymerization step", respectively. Comparative Examples 2 to 5 are random polymerizations, so the types of monomers used and their ratios (charging ratios) are described in the "1st" column.

[0184] In addition, in Tables 1 and 2, the numerical value in the "Diamine" column is the content rate (unit: mol%) of each diamine relative to the total amount of diamines used (in the case of sequential polymerization, the total amount of diamines used in the 1st sequential polymerization step and the total amount of diamines used in the 2nd sequential polymerization step). In Tables 1 and 2, the numerical value in the "Acid Dianhydride" column is the content rate (unit: mol%) of each acid dianhydride relative to the total amount of acid dianhydrides used (in the case of sequential polymerization, the total amount of acid dianhydrides used in the 1st sequential polymerization step and the total amount of acid dianhydrides used in the 2nd sequential polymerization step).

[0185] In addition, with respect to any one of Examples 1 to 12 and Comparative Examples 1 to 5, the molar fraction of each residue in the polyamic acid contained in the prepared polyamic acid solution is consistent with the molar fraction of each monomer (diamine and tetracarboxylic dianhydride) used. In addition, with respect to any one of Examples 1 to 12 and Comparative Examples 1 to 5, the total amount of tetracarboxylic dianhydride residues constituting the polyimide film obtained is divided by the total amount of diamine residues constituting the above-mentioned polyimide. The amount ratio is 0.99 or more and 1.01 or less. In addition, in Table 2, the "-" in the CTE column means that no measurement was performed.

[0186] [Table 1]

[0187]

[0188] [Table 2]

[0189]

[0190] The polyamic acid contained in the polyamic acid solutions prepared in Examples 1 to 12 has a BPDA residue, a BTDA residue, a PDA residue, and a TPE-R residue.

[0191] In Examples 1 to 12, the dielectric loss tangent was 0.0030 or less. Therefore, the polyimide films of Examples 1 to 12 can reduce the dielectric loss tangent.

[0192] The polyamic acid contained in the polyamic acid solutions prepared in Comparative Examples 1 and 3 does not have a TPE-R residue. The polyamic acid contained in the polyamic acid solutions prepared in Comparative Examples 2, 4, and 5 does not have a BTDA residue. The polyamic acid contained in the polyamic acid solution prepared in Comparative Example 4 does not have a BPDA residue.

[0193] In Comparative Examples 1 to 5, the dielectric loss tangent exceeded 0.0030. Therefore, the polyimide films of Comparative Examples 1 to 5 failed to reduce the dielectric loss tangent.

[0194] The above results show that according to the present invention, a non-thermoplastic polyimide film capable of reducing the dielectric loss tangent can be provided.

[0195] Description of Reference Numerals

[0196] 10: Multilayer polyimide film

[0197] 11: Non-thermoplastic polyimide film

[0198] 12: Adhesive layer

[0199] 13: Metal layer

[0200] 20: Metal-clad laminate

Claims

1. A polyamic acid having a tetracarboxylic dianhydride residue and a diamine residue, The tetracarboxylic dianhydride residues include 3,3',4,4'-biphenyltetracarboxylic dianhydride residues and 3,3',4,4'-benzophenonetetracarboxylic dianhydride residues. The diamine residue includes a p-phenylenediamine residue and a 1,3-bis(4-aminophenoxy)benzene residue.

2. The polyamic acid according to claim 1, wherein The content of the p-phenylenediamine residue is 75 mol% or more and 95 mol% or less relative to the total amount of the diamine residues.

3. The polyamic acid according to claim 1, wherein The content of the 3,3′,4,4′-biphenyltetracarboxylic dianhydride residue is 55 mol % or more and 85 mol % or less relative to the total amount of the tetracarboxylic dianhydride residues, The content of the 3,3′,4,4′-benzophenonetetracarboxylic dianhydride residue is 10 mol % or more and 30 mol % or less relative to the total amount of the tetracarboxylic dianhydride residues.

4. The polyamic acid according to claim 3, wherein The tetracarboxylic dianhydride residues further include pyromellitic dianhydride residues, The content of the pyromellitic dianhydride residue is 3 mol % or more and 15 mol % or less relative to the total amount of the tetracarboxylic dianhydride residues. A polyimide, which is an imide of the polyamic acid according to claim 1. A non-thermoplastic polyimide film comprising the polyimide according to claim 5. 7 . A multilayer polyimide film comprising the non-thermoplastic polyimide film according to claim 6 and an adhesive layer, wherein the adhesive layer is disposed on at least one surface of the non-thermoplastic polyimide film and contains thermoplastic polyimide.

8. The multilayer polyimide film according to claim 7, wherein: The adhesive layer is disposed on both sides of the non-thermoplastic polyimide film. 9 . A metal-clad laminate comprising the multilayer polyimide film according to claim 7 and a metal layer, wherein the metal layer is disposed on a main surface of at least one of the adhesive layers of the multilayer polyimide film.

Citation Information

Patent Citations

  • Flexible copper clad laminate

    JP2009246201A

  • Fluororesin-containing flexible metal laminate

    JP2014526399A

  • Multilayer adhesive film and flexible metal-clad laminate

    WO2016159060A1

  • Polyimide film for metal lamination and polyimide metal laminate using same

    WO2018079710A1