Resin composition, cured product, electronic component, and display device
By using soluble resin, organic salts with specific structures and photosensitizers in the resin composition, the problems of increased viscosity and poor adhesion caused by the reaction of the resin composition at room temperature are solved, and the substrate adhesion and storage stability are improved. , and has fine pattern processing performance, suitable for the manufacture of electronic parts and display devices.
Patent Information
- Application Number
- CN202380023236.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-14
- Publication Date
- 2024-10-08
AI Technical Summary
The existing resin composition reacts at room temperature, resulting in an increase in viscosity, poor storage stability, and poor adhesion to the metal layer, making it difficult to meet the high integration requirements of electronic parts.
A resin composition containing a soluble resin, an organic salt with a carboxyl group, and an organic salt of an amino group is used to improve the substrate adhesion and storage stability of the resin through a specific structure and ratio combination, and a photosensitizer is added to the combination to achieve fine patterns. Processability.
The resin composition achieves excellent substrate adhesion and good storage stability, and also has fine pattern processing performance, making it suitable for the manufacture of electronic parts and display devices.
Smart Images

Figure BDA0005005969110000021 
Figure BDA0005005969110000031 
Figure BDA0005005969110000032
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition containing a soluble resin, an organic salt and a solvent, a cured product obtained by curing the resin composition, an electronic component including the cured product, and a display device including the cured product. Background Art
[0002] In the surface protection film or interlayer insulating film of electronic parts, polyimide materials or polybenzoxazole materials with excellent heat resistance, electrical insulation and mechanical properties are widely used. In the manufacturing process of electronic parts, a metal layer is sometimes formed on the insulating film, but if the adhesion between the two is insufficient, peeling occurs at the interface, and the reliability of the electronic parts is poor. Therefore, the material used for the insulating film is required to have excellent adhesion to the metal layer, and excellent adhesion to the metal substrate is required in the evaluation of the development stage.
[0003] To address the above problems, resin compositions containing a basic nitrogen-containing compound or a thiol derivative as an additive have been disclosed (see Patent Documents 1 to 3).
[0004] In addition, in order to meet the requirements of fine processing required for high integration of electronic parts, a resin composition that can be patterned using photolithography by containing a photosensitizer in the insulating film is sometimes used. In such a case, it is preferable to use a resin composition with fine pattern processability of several μm to tens of μm.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2007-39486
[0008] Patent Document 2: Japanese Patent Application Publication No. 2003-5369
[0009] Patent Document 3: International Publication No. 2014 / 115233 Summary of the invention
[0010] Problems to be solved by the invention
[0011] The resin compositions described in Patent Documents 1 and 3 promote the reaction of the resin when stored at room temperature, causing the viscosity to increase; the resin composition described in Patent Document 2 has poor compatibility with the additives, so both have problems in terms of storage stability.
[0012] Therefore, an object of the present invention is to provide a resin composition having excellent substrate adhesion and excellent storage stability.
[0013] Technical means of solving problems
[0014] In order to solve the above-mentioned problems, the present invention has the following structure.
[0015] [1] A resin composition comprising (A) a soluble resin, (B) an organic salt and (C) a solvent, wherein the organic salt (B) is an organic salt formed from an organic compound having a carboxyl group and an organic compound having an amino group, and the amount of the organic salt (B) is 0.01 to 10 parts by mass based on 100 parts by mass of the soluble resin (A).
[0016] [2] The resin composition according to [1], wherein the (B) organic salt contains an organic salt having a structure represented by formula (6) or formula (7).
[0017] [Chemistry 1]
[0018]
[0019] (In formula (6), R 14 represents a tetravalent organic group having 4 to 40 carbon atoms; R 15 represents a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms; R 16 represents a divalent organic group having 1 to 40 carbon atoms)
[0020] (In formula (7), R 17 represents a divalent organic group having 1 to 40 carbon atoms; wherein R 17 Does not contain carboxyl or carboxylate groups; R 18 represents a divalent organic group having 1 to 40 carbon atoms)
[0021] [3] The resin composition according to [1] or [2], wherein the (A) soluble resin contains at least one soluble resin selected from the group consisting of polyimide, polybenzoxazole, precursors thereof, and copolymers thereof.
[0022] [4] The resin composition according to any one of [1] to [3], further comprising (D) a photosensitizer.
[0023] [5] The resin composition according to any one of [1] to [4], wherein the (A) soluble resin contains a
[0024] A polyimide having a structure represented by formula (1),
[0025] A polybenzoxazole having a structure represented by formula (3),
[0026] A polyimide precursor having a structure represented by formula (4) wherein g in formula (4) is 2,
[0027] A polybenzoxazole precursor having a structure represented by formula (4) wherein g in formula (4) is 0,
[0028] and at least one soluble resin selected from the group consisting of copolymers thereof.
[0029] [Chemistry 2]
[0030]
[0031] (In formula (1), R 1 represents a tetravalent organic group having 4 to 40 carbon atoms; R 2 The structure represented by expression (2)
[0032] (In formula (2), R 3 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates that R 4 and R 5 represents a monovalent organic group having 1 to 20 carbon atoms; a and b each independently represent an integer of 1 to 4, c and d each independently represent an integer of 0 to 1; * represents a chemical bond)
[0033] [Chemistry 3]
[0034]
[0035] (In formula (3), R 6 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates; R 7 represents a divalent organic group having 4 to 40 carbon atoms)
[0036] [Chemistry 4]
[0037]
[0038] (In formula (4), R 8 represents a divalent to tetravalent organic group having 4 to 40 carbon atoms; R 9 The structure represented by formula (5); R 10 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms; g represents 0 or 2)
[0039] (In formula (5), R 11 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates that R12 and R 13 represents a monovalent organic group having 1 to 20 carbon atoms; k and l each independently represent an integer of 1 to 4, m and n each independently represent an integer of 0 to 1; * represents a chemical bond)
[0040] [6] The resin composition according to any one of [1] to [5], wherein R in the formula (6) 16 And R in the formula (7) 18 It is the structure represented by formula (8).
[0041] [Chemistry 5]
[0042]
[0043] (In formula (8), R 19 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates that R 20 and R 21 represents a monovalent organic group having 1 to 20 carbon atoms; o and p each independently represent an integer of 1 to 4, q and r each independently represent an integer of 0 to 1; * represents a chemical bond)
[0044] [7] The resin composition according to [6], wherein R in the formula (8) 19 -C(CF 3 ) 2 -.
[0045] [8] A cured product obtained by curing the resin composition according to any one of [1] to [7].
[0046] [9] An electronic component comprising the hardened material according to [8].
[0047]
[10] A display device comprising the hardened material according to [8].
[0048] Effects of the Invention
[0049] The present invention provides a resin composition having excellent substrate adhesion and excellent storage stability. In a form further containing a photosensitizer, the present invention provides a resin composition having fine pattern processability. DETAILED DESCRIPTION
[0050] Hereinafter, the present invention will be described in detail.
[0051] <(A) Soluble resin>
[0052] The resin composition of the present invention contains (A) a soluble resin. The soluble resin in the present invention refers to a resin that dissolves 0.1 g or more in 100 g of an organic solvent or an alkaline aqueous solution at 25°C.
[0053] Examples of the organic solvent include γ-butyrolactone, γ-valerolactone, δ-valerolactone, dimethyl sulfoxide, tetrahydrofuran, dioxane, propylene glycol monomethyl ether, propylene glycol monoethyl ether, acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl acetate, butyl acetate, isobutyl acetate, propyl acetate, propylene glycol monomethyl ether acetate, 3-methyl-3-methoxybutyl acetate, methyl lactate, ethyl lactate, diacetone alcohol, 3-methyl-3-methoxybutanol, toluene, xylene, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, 1,3-dimethyl-2-imidazolidinone, N,N'-dimethylpropyleneurea, 1,3-dimethylisobutylamide, methoxy-N,N-dimethylpropionamide, butoxy-N,N-dimethylpropionamide, and the like.
[0054] Examples of the alkaline aqueous solution include aqueous solutions of tetramethyl ammonium hydroxide (TMAH), diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, and hexamethylenediamine.
[0055] As (A) soluble resin, there can be listed: polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, polyamide, polyamide-imide, phenolic resin, acrylic resin, polyurea, polyester, polysiloxane, etc. In addition, two or more of these resins may be contained. Among these, in terms of excellent heat resistance, strength, and substrate adhesion, it is preferred to include at least one soluble resin selected from the group consisting of polyimide, polybenzoxazole, their precursors, and their copolymers.
[0056] Polyimide and polybenzoxazole are resins having a cyclic structure of an imide ring or an oxazole ring in the main chain structure. In addition, the polyimide precursor and polybenzoxazole precursor as their precursors are resins that form an imide ring or a benzoxazole ring structure by undergoing dehydration ring closure.
[0057] Polyimide is obtained by reacting tetracarboxylic acid or corresponding tetracarboxylic dianhydride, tetracarboxylic diester dichloride, etc. with diamine or corresponding diisocyanate compound, trimethyl silylated diamine, etc., and has an organic group that is active from tetracarboxylic acid and an organic group derived from diamine. For example, polyamic acid, which is one of the polyimide precursors obtained by reacting tetracarboxylic dianhydride with diamine, is obtained by dehydration and ring closure by heat treatment. During the heat treatment, a solvent that azeotropes with water such as m-xylene may also be added. Alternatively, a dehydration condensation agent such as carboxylic anhydride or dicyclohexylcarbodiimide or a ring closure catalyst such as a base such as triethylamine is added, and dehydration and ring closure are obtained by chemical heat treatment. Alternatively, a weakly acidic carboxylic acid compound is added and dehydration and ring closure are obtained by heat treatment at a low temperature below 100°C.
[0058] Polybenzoxazole is obtained by reacting a bisaminophenol compound with a dicarboxylic acid or a corresponding dicarboxylic acid chloride, a dicarboxylic acid active ester, etc., and has an organic group that is actively derived from the dicarboxylic acid and an organic group that is derived from the bisaminophenol. For example, polyhydroxyamide, which is one of the precursors of polybenzoxazole, obtained by reacting a bisaminophenol compound with a dicarboxylic acid, is obtained by dehydration and ring closure by heat treatment. Alternatively, phosphoric anhydride, alkali, carbodiimide compounds, etc. are added and dehydration and ring closure are obtained by chemical treatment.
[0059] The (A) soluble resin preferably contains at least one soluble resin selected from the group consisting of a polyimide having a structure represented by formula (1), a polybenzoxazole having a structure represented by formula (3), a polyimide precursor having a structure represented by formula (4) wherein g in formula (4) is 2, a polybenzoxazole precursor having a structure represented by formula (4) wherein g in formula (4) is 0, and copolymers thereof. By containing at least one soluble resin selected from the group consisting of a polyimide having a structure represented by formula (1), a polybenzoxazole having a structure represented by formula (3), a polyimide precursor having a structure represented by formula (4) wherein g in formula (4) is 2, a polybenzoxazole precursor having a structure represented by formula (4) wherein g in formula (4) is 0, and copolymers thereof, the resin composition has excellent heat resistance, strength, and substrate adhesion, and its dissolution rate in an alkaline aqueous solution as a developer becomes faster, and the difference between the dissolution rate of a cured portion of the resin composition coating film in the developer and the dissolution rate of an uncured portion in the developer (hereinafter referred to as dissolution contrast) becomes larger, thereby achieving fine pattern processability.
[0060] [Chemistry 6]
[0061]
[0062] (In formula (1), R 1 represents a tetravalent organic group having 4 to 40 carbon atoms; R 2The structure represented by expression (2)
[0063] (In formula (2), R 3 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates that R 4 and R 5 represents a monovalent organic group having 1 to 20 carbon atoms; a and b each independently represent an integer of 1 to 4, c and d each independently represent an integer of 0 to 1; * represents a chemical bond)
[0064] [Chemistry 7]
[0065]
[0066] (In formula (3), R 6 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates; R 7 represents a divalent organic group having 4 to 40 carbon atoms)
[0067] [Chemistry 8]
[0068]
[0069] (In formula (4), R 8 represents a divalent to tetravalent organic group having 4 to 40 carbon atoms; R 9 The structure represented by formula (5); R 10 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms; g represents 0 or 2)
[0070] (In formula (5), R 11 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates that R 12 and R 13 represents a monovalent organic group having 1 to 20 carbon atoms; k and l each independently represent an integer of 1 to 4, m and n each independently represent an integer of 0 to 1; * represents a chemical bond)
[0071] R in formula (1) 1It is an organic group derived from a tetravalent carboxylic acid having 4 to 40 carbon atoms or a derivative thereof, and is preferably an organic group derived from a tetracarboxylic dianhydride. Examples of the tetracarboxylic dianhydride include pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, and bis(3,4-dicarboxyphenyl)ethane dianhydride. Aromatic tetracarboxylic acid dianhydrides such as bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, 4,4'-oxydiphthalic anhydride, 1,2,5,6-naphthalenetetracarboxylic acid dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene dianhydride, 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 2,3,5,6-pyridinetetracarboxylic acid dianhydride, 3,4,9,10-perylenetetracarboxylic acid dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, 3,3',4,4' -diphenylsulfone tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 1,2,4,5-cyclohexane tetracarboxylic dianhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic dianhydride, 2,3,5-tricarboxy-2-cyclopentaneacetic dianhydride, 2,3,4,5-tetrahydrofuran tetracarboxylic dianhydride, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic dianhydride, 4-(2,5-dioxotetrahydrofuran-3-yl)-4-methyl-1, 2,3,4-tetrahydronaphthalene-1,2-dicarboxylic dianhydride, 4-(2,5-dioxotetrahydrofuran-3-yl)-7-methyl-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic dianhydride, norbornane-2-spiro-2'-cyclopentanone-5'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride, norbornane-2-spiro-2'-cyclohexanone-6'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride, or compounds obtained by replacing a part of hydrogen atoms of aromatic rings or hydrocarbons thereof with an alkyl group or fluoroalkyl group having 1 to 10 carbon atoms, a halogen atom, or the like. In addition, two or more of these tetracarboxylic dianhydrides may be used in combination.
[0072] R in formula (1) 2The structure represented by formula (2) is as follows. Examples of the diamine having the structure represented by formula (2) include bis(3-amino-4-hydroxyphenyl)ether, bis(3-amino-4-hydroxyphenyl)methylene, bis[N-(3-aminobenzoyl)-3-amino-4-hydroxyphenyl]sulfone, bis[N-(4-aminobenzoyl)-3-amino-4-hydroxyphenyl]sulfone, bis(3-amino-4-hydroxyphenyl)sulfone, bis(3-amino-4-hydroxyphenyl)propane, 2- ,2'-bis[N-(3-aminobenzoyl)-3-amino-4-hydroxyphenyl]propane, 2,2'-bis[N-(4-aminobenzoyl)-3-amino-4-hydroxyphenyl]propane, 9,9-bis(3-amino-4-hydroxyphenyl)fluorene, 9,9-bis[N-(3-aminobenzoyl)-3-amino-4-hydroxyphenyl]fluorene, 9,9-bis[N-(4-aminobenzoyl)-3-amino-4-hydroxyphenyl]fluorene, N,N'-bis[N-(3-aminobenzoyl)-3-amino-4-hydroxyphenyl]fluorene (3-aminobenzoyl)-2,5-diamino-1,4-dihydroxybenzene, N,N'-bis(4-aminobenzoyl)-2,5-diamino-1,4-dihydroxybenzene, N,N'-bis(4-aminobenzoyl)-4,4'-diamino-3,3-dihydroxybiphenyl, N,N'-bis(3-aminobenzoyl)-3,3'-diamino-4,4-dihydroxybiphenyl, N,N'-bis(4-aminobenzoyl)-3,3'-diamino- 4,4-dihydroxybiphenyl, 3,3'-diamino-4,4'-biphenol, bis(3-amino-4-hydroxyphenyl)methane, 1,1-bis(3-amino-4-hydroxyphenyl)ethane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, or compounds obtained by replacing a portion of hydrogen atoms of aromatic rings or hydrocarbons thereof with alkyl or fluoroalkyl groups having 1 to 10 carbon atoms, halogen atoms, etc. In addition, two or more of the diamines having the structure represented by formula (2) may be used in combination.
[0073] R in formula (3) 6 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 -express.
[0074] R in formula (3) 7 represents a divalent organic group having 4 to 40 carbon atoms. 7 It is an organic group derived from a divalent carboxylic acid having 4 to 40 carbon atoms or a derivative thereof, and is preferably an organic group derived from a dicarboxylic acid.
[0075] Examples of the dicarboxylic acid include phthalic acid, isophthalic acid, terephthalic acid, 2,2'-biphenyl dicarboxylic acid, 3,4'-biphenyl dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, benzophenone-2,4'-dicarboxylic acid, benzophenone-4,4'-dicarboxylic acid, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 3,3'-dicarboxy diphenyl ether, 3,4'-dicarboxy diphenyl ether, 4,4'-dicarboxy diphenyl ether, Phenyl ether, 3,3'-dicarboxydiphenylmethane, 3,4'-dicarboxydiphenylmethane, 4,4'-dicarboxydiphenylmethane, 3,3'-dicarboxydiphenyldifluoromethane, 3,4'-dicarboxydiphenyldifluoromethane, 4,4'-dicarboxydiphenyldifluoromethane, 3,3'-dicarboxydiphenyl sulfone, 3,4'-dicarboxydiphenyl sulfone, 4,4'-dicarboxydiphenyl sulfone, 3,3'-dicarboxy Diphenyl sulfide, 3,4'-dicarboxydiphenyl sulfide, 4,4'-dicarboxydiphenyl sulfide, 3,3'-dicarboxydiphenyl ketone, 3,4'-dicarboxydiphenyl ketone, 4,4'-dicarboxydiphenyl ketone, 2,2-bis(3-carboxyphenyl)propane, 2,2-bis(3,4'-dicarboxyphenyl)propane, 2,2-bis(4-carboxyphenyl)propane, 2,2-bis(3-carboxyphenyl)hexafluoro Propane, 2,2-bis(3,4'-carboxyphenyl)hexafluoropropane, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 1,3-bis(3-carboxyphenoxy)benzene, 1,4-bis(3-carboxyphenoxy)benzene, 1,3-bis(4-carboxyphenoxy)benzene, or compounds obtained by replacing a portion of hydrogen atoms of aromatic rings or hydrocarbons thereof with alkyl or fluoroalkyl groups having 1 to 10 carbon atoms, halogen atoms, etc. In addition, two or more of these dicarboxylic acids may be used in combination.
[0076] R in formula (4) 8 represents a divalent to tetravalent organic group having 4 to 40 carbon atoms. 8 When g is 0, it is an organic group derived from a divalent carboxylic acid having 4 to 40 carbon atoms or a derivative thereof, and is preferably an organic group derived from a dicarboxylic acid.
[0077] Examples of the dicarboxylic acid include those having the same R as in formula (3). 7 Same dicarboxylic acid.
[0078] R in formula (4) 8 When g is 2, it is an organic group derived from a tetravalent carboxylic acid having 4 to 40 carbon atoms or a derivative thereof, and is preferably an organic group derived from tetracarboxylic dianhydride.
[0079] Examples of tetracarboxylic dianhydride include 1 Same tetracarboxylic dianhydride.
[0080] R in formula (4) 9It is a structure represented by formula (5). As a diamine which has a structure represented by formula (5), the same diamine as the structure represented by formula (2) can be mentioned.
[0081] The (A) soluble resin is preferably blocked at the end with one or more of a monoamine, an acid anhydride, an acid chloride, and a monocarboxylic acid. By blocking the end with one or more of a monoamine, an acid anhydride, an acid chloride, and a monocarboxylic acid, the storage stability of the resin composition is excellent.
[0082] The amount of monoamine when the terminal is blocked by a monoamine is preferably in the range of 0.1 mol% to 60 mol% relative to the total amine components, and more preferably 5 mol% to 50 mol%. When it is 5 mol% or more, excellent storage stability is achieved, and when it is 50 mol% or less, sufficient weight average molecular weight can be obtained, which is preferred in this respect.
[0083] Examples of the monoamine include 5-amino-8-hydroxyquinoline, 1-hydroxy-7-aminonaphthalene, 1-hydroxy-6-aminonaphthalene, 1-hydroxy-5-aminonaphthalene, 1-hydroxy-4-aminonaphthalene, 2-hydroxy-7-aminonaphthalene, 2-hydroxy-6-aminonaphthalene, 2-hydroxy-5-aminonaphthalene, 1-carboxy-7-aminonaphthalene, 1-carboxy-6-aminonaphthalene, 1-carboxy-5-aminonaphthalene, 2-carboxy-7-aminonaphthalene, 2-carboxy-6-aminonaphthalene, 2-carboxy-5-aminonaphthalene, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 3-amino-4,6-dihydroxypyrimidine, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2-aminothiophenol, 3-aminothiophenol, and 4-aminothiophenol. Two or more of these monoamines may be used in combination.
[0084] The amount of each compound when the terminal is blocked by anhydride, acid chloride, or monocarboxylic acid is preferably in the range of 0.1 mol% to 60 mol% relative to the total acid components, and more preferably 5 mol% to 50 mol%. When it is 5 mol% or more, excellent storage stability is achieved, and when it is 50 mol% or less, sufficient weight average molecular weight can be obtained, which is preferred in this respect.
[0085] Examples of the acid anhydride, acid chloride, and monocarboxylic acid include anhydrides such as phthalic anhydride, maleic anhydride, naphthalic anhydride, cyclohexanedicarboxylic anhydride, and 3-hydroxyphthalic anhydride; monocarboxylic acids such as 3-carboxyphenol, 4-carboxyphenol, 3-carboxythiophenol, 4-carboxythiophenol, 1-hydroxy-7-carboxynaphthalene, 1-hydroxy-6-carboxynaphthalene, 1-hydroxy-5-carboxynaphthalene, 1-mercapto-7-carboxynaphthalene, 1-mercapto-6-carboxynaphthalene, and 1-mercapto-5-carboxynaphthalene; and Monoacyl chloride compounds obtained by chlorinating their carboxyl groups, monoacyl chloride compounds obtained by chlorinating only one carboxyl group of dicarboxylic acids such as terephthalic acid, phthalic acid, maleic acid, cyclohexanedicarboxylic acid, 1,5-dicarboxynaphthalene, 1,6-dicarboxynaphthalene, 1,7-dicarboxynaphthalene, and 2,6-dicarboxynaphthalene, and active ester compounds obtained by reacting monoacyl chloride compounds with N-hydroxybenzotriazole or N-hydroxy-5-norbornene-2,3-dicarboximide, etc. Two or more of these acid anhydrides, acid chlorides, and monocarboxylic acids may also be used in combination.
[0086] (A) The weight average molecular weight of the soluble resin is preferably 1,000 or more and 200,000 or less, more preferably 5,000 or more and 100,000 or less, and further preferably 10,000 or more and 50,000 or less. By having a weight average molecular weight in the above range, fine pattern processability, heat resistance, and strength can be obtained. The weight average molecular weight is measured by gel permeation chromatography (GPC method) and calculated in terms of polystyrene.
[0087] <(B) Organic salt>
[0088] The resin composition of the present invention contains (B) an organic salt. The organic salt in the present invention refers to a salt formed by an organic compound having an acidic functional group and an organic compound having a basic functional group. Examples of the acidic functional group include a carboxyl group, a sulfonic acid group, a phosphoric acid group, and a phenolic hydroxyl group. Examples of the basic functional group include an amino group, specifically a primary amino group, a secondary amino group, and the like.
[0089] The organic salt (B) is preferably an organic salt having a structure represented by formula (6) or formula (7). By making the organic salt (B) contain an organic salt having a structure represented by formula (6) or formula (7), the adhesion between the resin composition and the Si substrate and SiO 2 Adhesion to substrates such as SiN substrates, Al substrates, Cu substrates, Ti substrates, and indium tin oxide (ITO) substrates.
[0090] [Chemistry 9]
[0091]
[0092] (In formula (6), R 14 represents a tetravalent organic group having 4 to 40 carbon atoms; R 15 represents a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms; R 16 represents a divalent organic group having 1 to 40 carbon atoms)
[0093] (In formula (7), R 17 represents a divalent organic group having 1 to 40 carbon atoms; wherein R 17 Does not contain carboxyl or carboxylate groups; R 18 represents a divalent organic group having 1 to 40 carbon atoms)
[0094] R in formula (6) 14 It is an organic group derived from a tetravalent carboxylic acid having 4 to 40 carbon atoms or a derivative thereof, and is preferably an organic group derived from a tetracarboxylic acid.
[0095] Examples of the tetracarboxylic acid include pyromellitic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 2,2',3,3'-biphenyltetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,2',3,3'-benzophenonetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)propane, 2,2-bis(2,3-dicarboxyphenyl)propane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3-dicarboxyphenyl)ethane, and bis(3,4-dicarboxyphenyl)methane. , bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)sulfone, 4,4'-oxydiphthalic acid, 1,2,5,6-naphthalenetetracarboxylic acid, 9,9-bis(3,4-dicarboxyphenyl)fluorene acid, 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,5,6-pyridinetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane and other aromatic tetracarboxylic acids, 3,3',4,4'-diphenylsulfonetetracarboxylic acid, 1, 2,3,4-cyclobutanetetracarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic acid, 2,3,5-tricarboxy-2-cyclopentaneacetic acid, 2,3,4,5-tetrahydrofurantetracarboxylic acid, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid, 4-(2,5-dioxotetrahydrofuran-3-yl)-4-methyl-1,2,3,4-tetrahydronaphthalene- 1,2-dicarboxylic acid, 4-(2,5-dioxotetrahydrofuran-3-yl)-7-methyl-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid, norbornane-2-spiro-2'-cyclopentanone-5'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic acid, norbornane-2-spiro-2'-cyclohexanone-6'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic acid, or compounds obtained by replacing part of the hydrogen atoms of the aromatic ring or hydrocarbon thereof with an alkyl group or fluoroalkyl group having 1 to 10 carbon atoms, a halogen atom, or the like. In addition, two or more of these tetracarboxylic acids may be used in combination.
[0096] R in formula (6) 16 It is an organic group derived from a divalent diamine having 1 to 40 carbon atoms or a derivative thereof, and is preferably a divalent organic group obtained by removing two amino groups from a diamine.
[0097] Examples of the diamine include 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 1,4-bis(4-aminophenoxy)benzene, benzidine, m-phenylenediamine, p-phenylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, bis(4-aminophenoxyphenyl)sulfone, bis(3-aminophenoxyphenyl)sulfone, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl Aromatic diamines such as -4,4'-biaminobiphenyl, 2,2'-diethyl-4,4'-biaminobiphenyl, 3,3'-dimethyl-4,4'-biaminobiphenyl, 3,3'-diethyl-4,4'-biaminobiphenyl, 2,2',3,3'-tetramethyl-4,4'-biaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-biaminobiphenyl, and 2,2'-bis(trifluoromethyl)-4,4'-biaminobiphenyl, or compounds obtained by replacing a portion of hydrogen atoms of the aromatic ring or hydrocarbon thereof with an alkyl group having 1 to 10 carbon atoms or a fluoroalkyl group, a halogen atom, or the like, bis(3-amino-4-hydroxyphenyl)ether, bis(3-amino-4-hydroxyphenyl)methylene, bis[N-(3-aminophenyl)] 2,2'-Bis[N-(3-aminobenzoyl)-3-amino-4-hydroxyphenyl]propane, 2,2'-Bis[N-(4-aminobenzoyl)-3-amino-4-hydroxyphenyl]propane, 9,9-Bis[N-(3-aminobenzoyl)-3-amino-4-hydroxyphenyl]fluorene, 9,9-Bis[N-(4-aminobenzoyl)-3-amino-4-hydroxyphenyl]fluorene, N,N'-Bis(3-amino-4-hydroxyphenyl)-3-amino-4-hydroxyphenyl]fluorene, bis[N-(3-aminobenzoyl)-3-amino-4-hydroxyphenyl]sulfone, bis[3-amino-4-hydroxyphenyl]sulfone, bis[3-amino-4-hydroxyphenyl]propane, 2,2'-Bis[N-(4-aminobenzoyl)-3-amino-4-hydroxyphenyl]propane, 9,9-Bis[N-(3-aminobenzoyl)-3-amino-4-hydroxyphenyl]fluorene, 9,9-Bis[N-(4-aminobenzoyl)-3-amino-4-hydroxyphenyl]fluorene, N,N'-Bis(3-amino-4-hydroxyphenyl)-3-amino-4-hydroxyphenyl] N,N'-bis(4-aminobenzoyl)-2,5-diamino-1,4-dihydroxybenzene, N,N'-bis(4-aminobenzoyl)-2,5-diamino-1,4-dihydroxybenzene, N,N'-bis(4-aminobenzoyl)-4,4'-diamino-3,3-dihydroxybiphenyl, N,N'-bis(3-aminobenzoyl)-3,3'-diamino-4,4-dihydroxybiphenyl, N,N'-bis(4-aminobenzoyl)-3,3'-diamino-4,4-dihydroxybiphenyl, 3,3'-diamino-4,4'-biphenol, bis(3-amino-4-hydroxyphenyl)methane, 1,1-bis(3-amino-4-hydroxyphenyl)ethane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, or compounds obtained by replacing part of the hydrogen atoms of the aromatic ring or hydrocarbon thereof with an alkyl group or a fluoroalkyl group having 1 to 10 carbon atoms, a halogen atom, or the like.
[0098] R in formula (7) 17 represents a divalent organic group having 1 to 40 carbon atoms. 17 It is an organic group derived from a divalent carboxylic acid having 1 to 40 carbon atoms or a derivative thereof, and is preferably an organic group derived from a dicarboxylic acid.
[0099] Examples of the dicarboxylic acid include phthalic acid, isophthalic acid, terephthalic acid, 2,2'-biphenyl dicarboxylic acid, 3,4'-biphenyl dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, benzophenone-2,4'-dicarboxylic acid, benzophenone-4,4'-dicarboxylic acid, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 3,3'-dicarboxy diphenyl ether, 3,4'-dicarboxy diphenyl ether, 4,4'-dicarboxy diphenyl ether, Phenyl ether, 3,3'-dicarboxydiphenylmethane, 3,4'-dicarboxydiphenylmethane, 4,4'-dicarboxydiphenylmethane, 3,3'-dicarboxydiphenyldifluoromethane, 3,4'-dicarboxydiphenyldifluoromethane, 4,4'-dicarboxydiphenyldifluoromethane, 3,3'-dicarboxydiphenyl sulfone, 3,4'-dicarboxydiphenyl sulfone, 4,4'-dicarboxydiphenyl sulfone, 3,3'-dicarboxy Diphenyl sulfide, 3,4'-dicarboxydiphenyl sulfide, 4,4'-dicarboxydiphenyl sulfide, 3,3'-dicarboxydiphenyl ketone, 3,4'-dicarboxydiphenyl ketone, 4,4'-dicarboxydiphenyl ketone, 2,2-bis(3-carboxyphenyl)propane, 2,2-bis(3,4'-dicarboxyphenyl)propane, 2,2-bis(4-carboxyphenyl)propane, 2,2-bis(3-carboxyphenyl)hexafluoro Propane, 2,2-bis(3,4'-carboxyphenyl)hexafluoropropane, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 1,3-bis(3-carboxyphenoxy)benzene, 1,4-bis(3-carboxyphenoxy)benzene, 1,3-bis(4-carboxyphenoxy)benzene, or compounds obtained by replacing a portion of hydrogen atoms of aromatic rings or hydrocarbons thereof with alkyl or fluoroalkyl groups having 1 to 10 carbon atoms, halogen atoms, etc. In addition, two or more of these dicarboxylic acids may be used in combination.
[0100] R in formula (7) 18 It is an organic group derived from a divalent diamine having 1 to 40 carbon atoms or a derivative thereof, and is preferably a divalent organic group obtained by removing two amino groups from a diamine.
[0101] Examples of the diamine include those having the same R as in formula (6) 16 Same diamine.
[0102] R in formula (6) 16, R in formula (7) 18 The structure represented by formula (8) is preferred. The structure represented by formula (8) increases the dissolution rate in an alkaline aqueous solution as a developer, increases the dissolution contrast between the cured part and the uncured part of the resin composition coating film, and facilitates fine pattern processability.
[0103] [Chemistry 10]
[0104]
[0105] (In formula (8), R 19 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates that R 20 and R 21 represents a monovalent organic group having 1 to 20 carbon atoms; o and p each independently represent an integer of 1 to 4, q and r each independently represent an integer of 0 to 1; * represents a chemical bond)
[0106] Examples of the diamine having a structure represented by formula (8) include bis(3-amino-4-hydroxyphenyl)ether, bis(3-amino-4-hydroxyphenyl)methylene, bis[N-(3-aminobenzoyl)-3-amino-4-hydroxyphenyl]sulfone, bis[N-(4-aminobenzoyl)-3-amino-4-hydroxyphenyl]sulfone, bis(3-amino-4-hydroxyphenyl)sulfone, bis(3-amino-4-hydroxyphenyl)propane, 2,2′-bis[N-( 3-aminobenzoyl)-3-amino-4-hydroxyphenyl]propane, 2,2'-bis[N-(4-aminobenzoyl)-3-amino-4-hydroxyphenyl]propane, 9,9-bis(3-amino-4-hydroxyphenyl)fluorene, 9,9-bis[N-(3-aminobenzoyl)-3-amino-4-hydroxyphenyl]fluorene, 9,9-bis[N-(4-aminobenzoyl)-3-amino-4-hydroxyphenyl]fluorene, N,N'-bis(3-aminobenzoyl)- N,N'-bis(4-aminobenzoyl)-2,5-diamino-1,4-dihydroxybenzene, N,N'-bis(4-aminobenzoyl)-4,4'-diamino-3,3-dihydroxybiphenyl, N,N'-bis(3-aminobenzoyl)-3,3'-diamino-4,4-dihydroxybiphenyl, N,N'-bis(4-aminobenzoyl)-3,3'-diamino-4,4 -dihydroxybiphenyl, 3,3'-diamino-4,4'-biphenol, bis(3-amino-4-hydroxyphenyl)methane, 1,1-bis(3-amino-4-hydroxyphenyl)ethane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, or compounds obtained by replacing part of the hydrogen atoms of the aromatic ring or hydrocarbon thereof with an alkyl group or fluoroalkyl group having 1 to 10 carbon atoms, a halogen atom, or the like.
[0107] R in formula (8) 19 More preferably -C(CF 3 ) 2 -. By R 19 -C(CF 3 ) 2 -, with R 19 For single bonds, -O-, -C(CH 3 ) 2 -, the dissolution rate in the alkaline aqueous solution as a developer becomes faster, the dissolution contrast between the cured part and the uncured part of the resin composition coating film becomes larger, and fine pattern processability is more easily obtained.
[0108] As R in formula (8) 19 -C(CF 3 ) 2Examples of diamines include 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, and compounds in which a part of hydrogen atoms of these aromatic rings or hydrocarbons are substituted with an alkyl group or fluoroalkyl group having 1 to 10 carbon atoms, a halogen atom, or the like.
[0109] The content of the organic salt (B) is set to be 0.01 parts by mass or more and 10 parts by mass or less, preferably 0.05 parts by mass or more and 1 part by mass or less, relative to 100 parts by mass of the soluble resin (A). When the content of the organic salt (B) is less than 0.01 parts by mass, fine pattern processability and substrate adhesion are poor. When the content of the organic salt (B) exceeds 10 parts by mass, storage stability is poor.
[0110] (B) The organic salt having a structure represented by formula (6) can be obtained, for example, by stirring equimolar amounts of the tetracarboxylic acid and diamine in a solvent, and the organic salt having a structure represented by formula (7) can be obtained, for example, by stirring equimolar amounts of the dicarboxylic acid and diamine in a solvent.
[0111] As the solvent, the organic solvent or water exemplified in the item of <(A) soluble resin> can be cited, and water is more preferred from the viewpoint of reaction yield. The reaction temperature is preferably 0°C or more and 150°C or less, more preferably 10°C or more and 120°C or less, and particularly preferably 30°C or more and 80°C or less. By making the reaction temperature within the preferred range, the tetracarboxylic acid and the diamine react sufficiently to obtain the organic salt having the structure represented by formula (6) in the organic salt (B), and overreaction can be suppressed. In addition, the dicarboxylic acid and the diamine react sufficiently to obtain the organic salt having the structure represented by formula (7) in the organic salt (B), and overreaction can be suppressed. The reaction time is preferably 0.5 hours or more and 30 hours or less, more preferably 1 hour or more and 20 hours or less, and particularly preferably 2 hours or more and 10 hours or less. By making the reaction time within the preferred range, the tetracarboxylic acid and the diamine react sufficiently to obtain the organic salt having the structure represented by formula (6) in the organic salt (B), and overreaction can be suppressed. In addition, the dicarboxylic acid and the diamine react sufficiently to obtain the organic salt having the structure represented by the formula (7) among the organic salts (B), and overreaction can be suppressed.
[0112] As a second method for obtaining an organic salt having a structure represented by formula (6) in an organic salt (B), a method of stirring a tetracarboxylic anhydride as the tetracarboxylic acid derivative in water to hydrolyze it, and then adding an equimolar amount of the diamine to stir. The reaction temperature of the hydrolysis is preferably above 0°C and below 150°C, more preferably above 10°C and below 120°C, and particularly preferably above 30°C and below 80°C. By making the reaction temperature within the preferred range, hydrolysis can be fully carried out to suppress overreaction. The reaction time is preferably above 0.5 hours and below 30 hours, more preferably above 1 hour and below 20 hours, and particularly preferably above 2 hours and below 10 hours. By making the reaction temperature within the preferred range, hydrolysis can be fully carried out to suppress overreaction.
[0113] <(C) Solvent>
[0114] The resin composition of the present invention contains (C) a solvent. The solvent in the present invention refers to a component that can dissolve (A) a soluble resin, (B) an organic salt, (D) a photosensitizer, and other components.
[0115] The content of the (C) solvent is not particularly limited, but is preferably 100 parts by mass or more and 10,000 parts by mass or less, more preferably 100 parts by mass or more and 5,000 parts by mass or less, and still more preferably 100 parts by mass or more and 2,000 parts by mass or less, relative to 100 parts by mass of the (A) soluble resin. By setting the content of the (C) solvent to be within the preferred range, excellent coating properties and flatness of the coating film can be achieved, and a coating film having a film thickness of 1 μm or more can be formed.
[0116] The boiling point of the solvent (C) under atmospheric pressure is preferably 50° C. to 250° C., more preferably 100° C. to 210° C. By setting the boiling point under atmospheric pressure to the above range, the solvent can be removed from the coating film in a short time during the drying step of the coating film of the resin composition, and the step embedding property of the patterned substrate is excellent. Examples of the solvent having a boiling point in the above range under atmospheric pressure include ethyl lactate (boiling point 154° C.), butyl lactate (boiling point 186° C.), dipropylene glycol dimethyl ether (boiling point 171° C.), diethylene glycol dimethyl ether (boiling point 162° C.), diethylene glycol ethyl methyl ether (boiling point 176° C.), diethylene glycol diethyl ether (boiling point 189° C.), 3-methoxybutyl acetate (boiling point 171° C.), ethylene glycol monoethyl ether acetate (boiling point 160° C.), γ-butyrolactone (boiling point 203° C.), N-methyl-2-pyrrolidone (boiling point 204° C.), diacetone alcohol (boiling point 166° C.), N-cyclohexyl-2-pyrrolidone (boiling point 154° C.), N,N-dimethylformamide Alkyl glycol monoalkyl ethers such as amide (boiling point 153°C), N,N-dimethylacetamide (boiling point 165°C), dimethyl sulfoxide (boiling point 189°C), propylene glycol monomethyl ether acetate (boiling point 146°C), N,N-dimethylisobutyric acid amide (boiling point 175°C), ethylene glycol monomethyl ether (boiling point 124°C), propylene glycol monomethyl ether (boiling point 120°C), alkyl acetates such as propyl acetate (boiling point 102°C), butyl acetate (boiling point 125°C), isobutyl acetate (boiling point 118°C), ketones such as methyl isobutyl ketone (boiling point 116°C), methyl propyl ketone (boiling point 102°C), alcohols such as butanol (boiling point 117°C), isobutyl alcohol (boiling point 108°C), etc. Two or more solvents having a boiling point of 100°C to 210°C at atmospheric pressure may be used in combination.
[0117] The solubility parameter (SP value) of the (C) solvent is preferably greater than or equal to 7.0 and less than or equal to 13.0. By setting the SP value to the above range, the precipitation of solid components can be suppressed, and the (A) soluble resin can be easily dissolved. The SP value is more preferably less than or equal to 12.5. In the present invention, the solubility parameter (SP value) uses the literature value recorded in "Basic Science of Coating" (page 65, written by Yuji Harazaki, Maki Bookstore). In addition, if the SP value is not recorded, the value calculated based on Fedors on page 55 of the book from the evaporation energy and molar volume of atoms and atomic groups is used. Examples of the solvent having an SP value of 7.0 or more and 13.0 or less include ethyl lactate (SP value 10.6, literature value), butyl lactate (SP value 9.7, literature value), dipropylene glycol dimethyl ether (SP value 7.9, calculated value), diethylene glycol dimethyl ether (SP value 8.1, calculated value), diethylene glycol ethyl methyl ether (SP value 8.1, calculated value), diethylene glycol diethyl ether (SP value 8.2, calculated value), 3-methoxybutyl acetate (SP value 8.7, calculated value), ethylene glycol monoethyl ether acetate (SP value 9.0, calculated value), γ-butyrolactone (SP value 12.8, literature value), N-methyl-2-pyrrolidone (SP value 11.2, literature value), diacetone alcohol (SP value 10.2, literature value), N-cyclohexyl-2-pyrrolidone (SP value 10.8, literature value), N ,N-dimethylformamide (SP value 12.1, literature value), N,N-dimethylacetamide (SP value 11.1, literature value), dimethyl sulfoxide (SP value 12.9, literature value), propylene glycol monomethyl ether acetate (SP value 8.7, calculated value), N,N-dimethylisobutyric acid amide (SP value 9.9, calculated value), ethylene glycol monomethyl ether (SP value 10.8, calculated value), propylene glycol monomethyl ether (SP value 10.2, calculated value), propyl acetate (SP value 8.7, calculated value), butyl acetate (SP value 8.5, literature value), isobutyl acetate (SP value 8.4, literature value), methyl isobutyl ketone (SP value 8.6, literature value), methyl propyl ketone (SP value 8.9, calculated value), butanol (SP value 11.3, literature value), isobutyl alcohol (SP value 11.1, literature value), etc. Two or more of these solvents having an SP value of 7.0 or more and 13.0 or less may be used in combination.
[0118] <(D) Photosensitizer>
[0119] The resin composition of the present invention contains (D) a photosensitizer. The photosensitizer in the present invention refers to a component that generates reactive species upon exposure to light, and examples thereof include (D-1) a photoacid generator and (D-2) a photopolymerization initiator.
[0120] The (D-1) photoacid generator is a component that generates an acid by exposure. The dissolution rate of the exposed part relative to the alkaline aqueous solution becomes faster, resulting in a dissolution contrast with the unexposed part, thereby obtaining a positive relief pattern in which the exposed part is soluble. In applications that particularly require high resolution, the positive type is preferably selected. In addition, by containing the (D-1) photoacid generator and the cross-linking agent described later, the acid generated in the exposed part causes the cross-linking agent to undergo a cross-linking reaction, thereby obtaining a negative relief pattern in which the exposed part is insoluble. In applications that particularly require high exposure sensitivity and / or thick film processing, the negative type is preferably selected.
[0121] Examples of the photoacid generator (D-1) include quinonediazide compounds, sulfonium salts, phosphonium salts, diazonium salts, and iodonium salts.
[0122] Examples of the quinonediazide compound include compounds obtained by ester-bonding a polyhydroxy compound to a sulfonyl group of quinonediazide, compounds obtained by sulfonamide-bonding a polyamino compound to a sulfonyl group of quinonediazide, and compounds obtained by ester-bonding and / or sulfonamide-bonding a polyhydroxypolyamino compound to a sulfonyl group of quinonediazide.
[0123] As the sulfonyl group of the quinonediazide compound, 4-naphthoquinonediazidesulfonyl group and 5-naphthoquinonediazidesulfonyl group can be preferably used. The 4-naphthoquinonediazidesulfonyl ester compound has absorption in the i-ray region of the mercury lamp and is suitable for i-ray exposure. The 5-naphthoquinonediazidesulfonyl ester compound has absorption in the g-ray region of the mercury lamp and is suitable for g-ray exposure. In the present invention, it is preferred to select the 4-naphthoquinonediazidesulfonyl ester compound and the 5-naphthoquinonediazidesulfonyl ester compound according to the wavelength of the light used for exposure. In addition, the naphthoquinonediazidesulfonyl ester compound having the 4-naphthoquinonediazidesulfonyl group and the 5-naphthoquinonediazidesulfonyl group in the same molecule may be contained, and the 4-naphthoquinonediazidesulfonyl ester compound and the 5-naphthoquinonediazidesulfonyl ester compound may also be contained.
[0124] (D-1) Among the photoacid generators, sulfonium salts, phosphonium salts, diazonium salts, and iodonium salts are preferred in terms of appropriately stabilizing the acid generated by light exposure. Among them, sulfonium salts are more preferred in terms of preventing wiring corrosion.
[0125] Examples of the cation forming the sulfonium salt include triphenylsulfonium, tri-p-tolylsulfonium, tri-o-tolylsulfonium, tri(4-methoxyphenyl)sulfonium, 1-naphthyldiphenylsulfonium, 2-naphthyldiphenylsulfonium, tri(4-fluorophenyl)sulfonium, tri-1-naphthylsulfonium, tri-2-naphthylsulfonium, tri(4-hydroxyphenyl)sulfonium, 4-(phenylthio)phenyldiphenylsulfonium, 4-(p-tolylsulfonium)phenyldi-p-tolylsulfonium, 4-(4-methoxyphenylthio)phenylbis(4-methoxyphenyl)sulfonium, 4-(phenylthio)phenylbis(4-fluorophenyl)sulfonium, 4-(phenylthio)phenylbis(4-methoxyphenyl)sulfonium, 4-(phenylthio)phenylbis(4-methoxyphenyl)sulfonium, )phenyl di-p-tolylsulfonium, [4-(4-biphenylthio)phenyl]-4-biphenylphenylsulfonium, [4-(2-thioxanthonethio)phenyl]diphenylsulfonium, bis[4-(diphenylsulfonyl)phenyl]sulfide, bis[4-{bis[4-(2-hydroxyethoxy)phenyl]sulfonyl}phenyl]sulfide, bis{4-[bis(4-fluorophenyl)sulfonyl]phenyl}sulfide, bis{4-[bis(4-methylphenyl)sulfonyl]phenyl}sulfide, bis{4-[bis(4-methoxyphenyl)sulfonyl]phenyl}sulfide, 4-(4-benzoyl-2-chlorophenylthio)phenylbis(4-fluorophenyl)sulfonium, 4-(4-benzoyl- 2-chlorophenylthio)phenyl diphenylsulfonium, 4-(4-benzoylphenylthio)phenylbis(4-fluorophenyl)sulfonium, 4-(4-benzoylphenylthio)phenyl diphenylsulfonium, 7-isopropyl-9-oxo-10-thia-9,10-dihydroanthracen-2-yldi-p-tolylsulfonium, 7-isopropyl-9-oxo-10-thia-9,10-dihydroanthracen-2-yldiphenylsulfonium, 2-[(di-p-tolyl)sulfonyl]thioxanthone, 2-[(diphenyl)sulfonyl]thioxanthone, 4-(9-oxo-9H-thioxanthen-2-yl)thiophenyl-9-oxo-9H-thioxanthen-2-ylphenylsulfonium, 4-[4-( triarylsulfoniums such as 4-tert-butylbenzoyl)phenylthio]phenyldi-p-tolylsulfonium, 4-[4-(4-tert-butylbenzoyl)phenylthio]phenyldiphenylsulfonium, 4-[4-(benzoylphenylthio)]phenyldi-p-tolylsulfonium, 4-[4-(benzoylphenylthio)]phenyldiphenylsulfonium, 5-(4-methoxyphenyl)thianthrenium, 5-phenylthianthrenium, 5-tolylthianthrenium, 5-(4-ethoxyphenyl)thianthrenium, and 5-(2,4,6-trimethylphenyl)thianthrenium; diarylsulfoniums such as diphenylphenacylsulfonium, diphenyl 4-nitrophenacylsulfonium, diphenylbenzylsulfonium, and diphenylmethylsulfonium;Monoarylsulfonium such as phenylmethylbenzylsulfonium, 4-hydroxyphenylmethylbenzylsulfonium, 4-methoxyphenylmethylbenzylsulfonium, 4-acetylcarbonyloxyphenylmethylbenzylsulfonium, 4-hydroxyphenyl(2-naphthylmethyl)methylsulfonium, 2-naphthylmethylbenzylsulfonium, 2-naphthylmethyl(1-ethoxycarbonyl)ethylsulfonium, phenylmethylphenacylsulfonium, 4-hydroxyphenylmethylphenacylsulfonium, 4-methoxyphenylmethylphenacylsulfonium, 4-acetylcarbonyloxyphenylmethylphenacylsulfonium, 2-naphthylmethylphenacylsulfonium, 2-naphthyloctadecylphenacylsulfonium, 9-anthrylmethylphenacylsulfonium; dimethylphenacylsulfonium, phenacyltetrahydrothiophenium, dimethylbenzylsulfonium, benzyltetrahydrothiophenium, octadecylmethylphenacylsulfonium, etc.;
[0126] As the anion forming the sulfonium salt, it is preferable to contain at least one selected from the group consisting of borate ions, phosphate ions, and gallate ions.
[0127] Examples of the borate ion include pentafluorophenyl borate, trifluorophenyl borate, tetrafluorophenyl borate, trifluoromethylphenyl borate, bis(trifluoromethyl)phenyl borate, pentafluoroethylphenyl borate, bis(pentafluoroethyl)phenyl borate, fluoro-bis(trifluoromethyl)phenyl borate, fluoro-pentafluoroethylphenyl borate, and fluoro-bis(pentafluoroethyl)phenyl borate.
[0128] Examples of the phosphate ion include hexafluorophosphate and tris(pentafluoroethyl)trifluorophosphate.
[0129] Examples of the gallate ion include tetrakis(pentafluorophenyl)gallate and tetrakis(3,5-bis(trifluoromethyl)phenyl)gallate.
[0130] The content of the photoacid generator (D-1) is preferably 0.01 parts by mass or more and 50 parts by mass or less relative to 100 parts by mass of the soluble resin (A). The content within the above range is preferred in terms of good sensitivity and excellent storage stability.
[0131] The (D-2) photopolymerization initiator is a component that generates free radicals by bond cleavage and / or reaction upon exposure. By containing the (D-2) photopolymerization initiator and the free radical polymerizable compound described later, a free radical polymerization reaction is carried out in the exposed part to obtain a negative relief pattern in which the exposed part is insoluble. In applications requiring particularly high exposure sensitivity and / or thick film processing, the negative type is preferably selected.
[0132] Examples of the photopolymerization initiator (D-2) include benzyl ketal photopolymerization initiators, α-hydroxy ketone photopolymerization initiators, α-amino ketone photopolymerization initiators, acyl phosphine oxide photopolymerization initiators, oxime ester photopolymerization initiators, acridine photopolymerization initiators, titanocene photopolymerization initiators, benzophenone photopolymerization initiators, acetophenone photopolymerization initiators, aromatic ketoester photopolymerization initiators, and benzoate photopolymerization initiators. Among them, α-amino ketone photopolymerization initiators, acyl phosphine oxide photopolymerization initiators, and oxime ester photopolymerization initiators are preferred from the viewpoint of sensitivity.
[0133] Examples of the α-aminoketone-based photopolymerization initiator include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butane-1-one, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholinophenyl)-butane-1-one, and 3,6-bis(2-methyl-2-morpholinopropionyl)-9-octyl-9H-carbazole.
[0134] Examples of the acylphosphine oxide-based photopolymerization initiator include 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-(2,4,4-trimethylpentyl)phosphine oxide.
[0135] Examples of the oxime ester photopolymerization initiator include 1-phenylpropane-1,2-dione-2-(O-ethoxycarbonyl)oxime, 1-phenylbutane-1,2-dione-2-(O-methoxycarbonyl)oxime, 1,3-diphenylpropane-1,2,3-trione-2-(O-ethoxycarbonyl)oxime, 1-[4-(phenylthio)phenyl]octane-1,2-dione-2-(O-benzoyl)oxime, 1-[4-[4-(carboxyphenyl)thio]phenyl]propane-1,2-dione-2-(O-acetyl)oxime, 1-[9-ethoxy]phenyl]propane-1,2-dione-2-(O-ethoxycarbonyl)oxime, and 1-[4-[4-(carboxyphenyl)thio]phenyl]propane-1,2-dione-2-(O-acetyl)oxime. 1-[9-ethyl-6-[2-methyl-4-[1-(2,2-dimethyl-1,3-dioxolan-4-yl)methyloxy]benzoyl]-9H-carbazol-3-yl]ethanone-1-(O-acetyl)oxime, 1-(9-ethyl-6-nitro-9H-carbazol-3-yl)-1-[2-methyl-4-(1-methoxypropane-2-yloxy)phenyl]methanone-1-(O-acetyl)oxime, and the like.
[0136] The content of the photopolymerization initiator (D-2) is preferably 1 part by mass or more and 25 parts by mass or less relative to 100 parts by mass of the soluble resin (A). The content within the above range is preferred in terms of good sensitivity and excellent resolution.
[0137] The (D-1) photoacid generator and the (D-2) photopolymerization initiator in the (D) photosensitive agent may be used alone or in combination. The content of the (D) photosensitive agent is preferably 0.01 parts by mass or more and 50 parts by mass or less relative to 100 parts by mass of the (A) soluble resin. By making the content within the above range, it is preferred in terms of good sensitivity, excellent resolution and excellent storage stability.
[0138] <Cross-linking agent>
[0139] The resin composition of the present invention may further contain a crosslinking agent. The crosslinking agent in the present invention refers to a component that crosslinks (A) a soluble resin or other components, and examples thereof include compounds having at least two functional groups such as alkoxymethyl, methylol, epoxy, and oxetane. By containing a crosslinking agent, (A) a soluble resin or other components can be crosslinked to improve the heat resistance, strength, and chemical resistance of the cured film. In addition, by containing a crosslinking agent and the (D-1) photoacid generator, the acid generated in the exposure portion causes the crosslinking agent to undergo a crosslinking reaction, thereby obtaining a negative relief pattern in which the exposure portion is insoluble.
[0140] Examples of the compound having at least two alkoxymethyl groups or hydroxymethyl groups include DML-PC, DML-PEP, DML-OC, DML-OEP, DML-34X, DML-PTBP, DML-PCHP, DML-OCHP, DML-PFP, DML-PSBP, DML-POP, DML-MBOC, DML-MBPC, DML-MTrisPC, DML-BisOC-Z, DML-BisOCHP-Z, DML-BPC, DML-BisOC-P, DMOM-PC, DMOM-PTBP, DMOM-MBPC, TriML-P, TriML-35XL, TML-HQ, TML-BP, TML-pp-BPF, TML-BPE, TML-BPA, TML- BPAF, TML-BPAP, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP (these are trade names, manufactured by Honshu Chemical Industry Co., Ltd.), "NIKALAC" (registered trademark) MX-290, "NIKALAC" MX-280, "NIKALAC" MX-270, "NIKALAC" MX-279, "NIKALAC" MW-100LM, "NIKALAC" MX-750LM (these are trade names, manufactured by Sanwa Chemical Co., Ltd.), etc. Two or more of these compounds having at least two alkoxymethyl groups or hydroxymethyl groups may be used in combination.
[0141] Examples of the compound having at least two epoxy groups include: "Epolight" (registered trademark) 40E, "Epolight" 100E, "Epolight" 200E, "Epolight" 400E, "Epolight" 70P, "Epolight" 200P, "Epolight" 400P, and "Epolight" 1500N. P, "Epolight" 80MF, "Epolight" 4000, "Epolight" 3002 (all manufactured by Kyoeisha Chemical Co., Ltd.), "Denacol" (registered trademark) EX-212L, "Denacol" EX-214L, "Denacol" EX-216L, "Denacol" EX-850L (all manufactured by Nagase Chemical Co., Ltd. Chemtex (manufactured by Co., Ltd.), GAN, GOT (manufactured by Nippon Kayaku Co., Ltd.), "Epikote" (registered trademark) 828, "Epikote" 1002, "Epikote" 1750, "Epikote" 1007, YX8100-BH30, E1256, E4250, E4275 (manufactured by Nippon Epoxy Resin Co., Ltd.), " "Epiclon" (registered trademark) EXA-9583, HP4032 (all manufactured by DIC), VG3101 (manufactured by Mitsui Chemicals), "TEPIC" (registered trademark) S, "TEPIC" G, "TEPIC" P (all manufactured by Nissan Chemical Industries, Ltd.), "Denacol" EX-321L (manufactured by Nagase Chemtex), NC6000 (manufactured by Nippon Kayaku), "Epotohto" (registered trademark) YH-434L (manufactured by Tohto Kasei), EPPN502H, NC3000 (manufactured by Nippon Kayaku), "Epiclon" (registered trademark) N695, HP7200 (all manufactured by DIC), etc. Two or more of these compounds having at least two epoxy groups may be used in combination.
[0142] Examples of the compound having at least two oxetane groups include: Eternacoll EHO, OXBP, OXTP, OXMA (all manufactured by Ube Industries, Ltd.), etc. Two or more of these compounds having at least two oxetane groups may be used in combination.
[0143] The content of the crosslinking agent is preferably 5 parts by mass or more and 100 parts by mass or less, more preferably 10 parts by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the soluble resin (A). By setting the content within the preferred range, chemical resistance is good, and heat resistance and strength are excellent.
[0144] <Radical polymerizable compounds>
[0145] The resin composition of the present invention may further contain a free radical polymerizable compound. The free radical polymerizable compound in the present invention refers to a component that undergoes polymerization reaction under a free radical mechanism. By containing the free radical polymerizable compound and the (D-2) photopolymerization initiator, a free radical polymerization reaction is carried out in the exposed part to obtain a negative relief pattern in which the exposed part is insoluble.
[0146] Examples of the radical polymerizable compound include trimethylolpropane tri(meth)acrylate, di-trimethylolpropane tri(meth)acrylate, di-trimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, 2,2-bis[4-(3-(meth)acrylate]propane
[0063] The invention also includes 1,3,5-tris((meth)acryloyloxyethyl)isocyanuric acid, 1,3-bis((meth)acryloyloxyethyl)isocyanuric acid, 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene, 9,9-bis[4-(3-(meth)acryloyloxypropoxy)phenyl]fluorene, 9,9-bis(4-(meth)acryloyloxyphenyl)fluorene or their acid-modified forms, ethylene oxide-modified forms, propylene oxide-modified forms, and the like. Two or more of these radical polymerizable compounds may be used in combination.
[0147] The content of the radical polymerizable compound is preferably 10 parts by mass to 90 parts by mass, more preferably 20 parts by mass to 80 parts by mass, relative to 100 parts by mass of the soluble resin (A). When the content is within the preferred range, good sensitivity, excellent heat resistance and strength are achieved.
[0148] <Dissolution accelerator>
[0149] The resin composition of the present invention may further contain a dissolution accelerator. The dissolution accelerator in the present invention refers to a component that improves the solubility of the resin composition in an alkaline aqueous solution. By containing a dissolution accelerator, the dissolution rate in an alkaline aqueous solution as a developer becomes faster, the dissolution contrast between the hardened part and the unhardened part of the resin composition coating film becomes larger, and fine pattern processability is easily obtained.
[0150] Examples of the dissolution accelerator include Bis-Z, BisOC-Z, BisOPP-Z, BisP-CP, Bis26X-Z, BisOTBP-Z, BisOCHP-Z, BisOCR-CP, BisP-MZ, BisP-EZ, Bis26X-CP, BisP-PZ, BisP-IPZ, BisCRIPZ, BisOCP-IPZ, BisOIPP-CP, Bis26X-IPZ, BisOTBP-CP, TekP-4HBPA (tetrakis P-DO-BPA), tris P-HAP, TrisP-PA, TrisP-PHBA, TrisP-SA, TrisOCR-PA, BisOFP-Z, BisRS-2P, BisPG-26X, BisRS-3P, BisOC-OCHP, BisPC-OCHP, Bis25X-O CHP, Bis26X-OCHP, BisOCHP-OC, Bis236T-OCHP, Methylenetris-FR-CR, BisRS-26X, BisRS-OCHP (these are trade names, manufactured by Honshu Chemical Industry Co., Ltd.), BIR-OC, BIP-PCBIR-PC, BIR-PTBP, BIR-PCHP, BIP-BIOC-F, 4PC, BIR-B IPC-F, TEP-BIP-A (the above are trade names, manufactured by Asahi Organic Materials Industries, Ltd.), 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 2,4-dihydroxyquinoline, 2,6-dihydroxyquinoline, 2,3-dihydroxyquinoxaline, anthracene-1,2,10-triol, anthracene-1,8,9-triol, phenolic compounds such as 8-quinolinol, etc. Two or more of these dissolution accelerators may be used in combination.
[0151] The content of the dissolution accelerator is preferably 1 part by mass or more and 20 parts by mass or less relative to 100 parts by mass of the (A) soluble resin. When the content is within the above-described preferred range, heat resistance is improved and fine pattern processability can be obtained.
[0152] <Adhesion improving agent>
[0153] The resin composition of the present invention may further contain an adhesion improver. The adhesion improver in the present invention refers to a component that improves the adhesion between the resin composition film and the substrate.
[0154] Examples of the substrate include Si substrates, SiO 2 Substrate, SiN substrate, Al substrate, Cu substrate, Ti substrate, ITO substrate, etc.
[0155] Examples of the adhesion improver include vinyl trimethoxysilane, vinyl triethoxysilane, epoxy cyclohexyl ethyl trimethoxysilane, 3-glycidyloxypropyl trimethoxysilane, 3-glycidyloxypropyl triethoxysilane, p-phenylyl trimethoxysilane, 3-aminopropyl trimethoxysilane, 3-aminopropyl triethoxysilane, N-phenyl-3-aminopropyl trimethoxysilane and other silane coupling agents, titanium chelating agents, aluminum chelating agents, compounds obtained by reacting aromatic amine compounds with alkoxy-containing silicon compounds, etc. Two or more of these adhesion improvers may be used in combination.
[0156] The content of the adhesion improver is preferably 0.1 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the total amount of the resin composition excluding the (C) solvent.
[0157] <Surfactant>
[0158] The resin composition of the present invention may further contain a surfactant. The surfactant in the present invention refers to a component that improves the wettability of the resin composition and the base substrate. Examples of surfactants include: SH series, SD series, ST series of Dow Corning Toray (stock), BYK series of BYK-Chemie Japan (stock), KP series of Shin-Etsu Chemical (stock), DISFOAM series of NOF (stock), "MEGAFAC" (registered trademark) series of DIC (stock), FLUORAD series of Sumitomo 3M (stock), "SURFLON" (registered trademark) series of Asahi Glass (stock), "AsahiGuard" (registered trademark) series, OMNOVA solutions (Omnivolum) Fluorochemical surfactants such as the PolyFox series of KONOEX CHEMICAL CO., LTD., POLYFLOW series of KYOEISH Chemical Co., Ltd., and DISPARLON (registered trademark) series of Kusumoto Chemical Co., Ltd. are acrylic acid and / or methacrylic acid surfactants.
[0159] The content of the surfactant is preferably 0.001 part by mass or more and 1 part by mass or less relative to 100 parts by mass of the total amount of the resin composition excluding the (C) solvent.
[0160] <Hardened material>
[0161] The cured product of the present invention is a cured product obtained by curing the resin composition, and may be in any form as long as the resin composition is cured by light or heat. As a method of curing by light, a method of curing by exposure to 50 mJ or more and 3,000 mJ or less using 365 nm i-rays, 405 nm h-rays, or 432 nm g-rays of a high pressure mercury lamp, etc., and as a method of curing by heat, a method of curing by heating at 150° C. or more and 500° C. or less for 5 minutes or more and 5 hours or less, etc., may be mentioned.
[0162] The method for producing the cured product includes: a step of applying the resin composition on a substrate and drying it to form a resin film on the substrate; a step of exposing the resin composition film to light; a step of removing the unexposed portion or unexposed portion of the resin composition film with a developer and developing it; and a step of heating the developed resin composition film to cure it.
[0163] As the process of applying the resin composition on a substrate and drying it to form a resin film on the substrate, there can be listed: using a spin coater, a spray coater, a screen coater, a knife coater, a die coater, a calender coater, a meniscus coater, a rod coater, a roll coater, a notch roll coater, a gravure coater, a slot die coater, etc. to apply the resin composition on a substrate, and drying it in a range of not less than 50° C. and not more than 150° C. for not less than 1 minute and not more than 24 hours to form a resin composition film, etc.
[0164] As a process for exposing the resin composition film, there can be cited a process of exposing the film to 50 mJ or more and 3,000 mJ or less using 365 nm i-rays, 405 nm h-rays, and 432 nm g-rays of a high-pressure mercury lamp through a mask having a desired pattern. The resin composition film exposed by the above process can be baked after exposure. From the viewpoint of curability and adhesion to the substrate, the post-exposure bake is preferably 50° C. or more, and from the viewpoint of resolution, it is preferably 150° C. or less.
[0165] As a process for developing by removing the unexposed part or unexposed part of the resin composition film with a developer, the following can be cited: spraying the developer on the surface of the resin composition film, placing the developer on the surface of the resin composition film, immersing the resin composition film in the developer, or immersing and applying ultrasonic waves. The development conditions such as the development time, the development steps, and the temperature of the developer are sufficient as long as they can remove the unexposed part or the exposed part to form a pattern. It is preferred to perform a rinse treatment after development. The rinse treatment is preferably carried out by adding alcohols such as water, ethanol, isopropanol, ethyl lactate, propylene glycol monomethyl ether acetate, etc., or by combining two or more of these.
[0166] As a process for curing the developed resin composition film by heat treatment, a process of forming a cured product by heat treatment at 150°C or more and 500°C or less for 5 minutes or more and 5 hours or less can be cited. The heat treatment can be selected as follows: a method of stepwise heating by selecting a temperature, or a method of continuously heating by selecting a certain temperature range. As the former, a method of heat treatment at 130°C and 200°C for 30 minutes each can be cited. As the latter, a method of heating from room temperature to 400°C for 2 hours can be cited.
[0167] <Electronic components>
[0168] The electronic component of the present invention includes the hardened material. The hardened material can be used as an insulating film, a protective film, etc. constituting the electronic component.
[0169] As electronic parts, there are active parts with semiconductors such as transistors, diodes, integrated circuits (ICs), and memories, and passive parts such as resistors, capacitors, and inductors. As specific examples of hardened materials in electronic parts, preferably used for semiconductor passivation films, semiconductor elements, surface protection films of thin film transistors (TFTs), interlayer insulation films such as interlayer insulation films between redistribution wiring in multilayer wiring for high-density mounting of 2 to 10 layers, insulation films of touch screen displays, protective films, and insulation layers of organic electroluminescent elements, etc. In addition, various structures can also be used.
[0170] <Display device>
[0171] The display device of the present invention includes the hardened material. The hardened material can be used as a planarization layer or a pixel division layer constituting the display device.
[0172] As a display device, there can be cited: an organic EL display device having a planarization layer, a first electrode, a pixel segmentation layer, an organic electroluminescence (EL) layer and a second electrode on a substrate, and the planarization layer and / or the pixel segmentation layer include a cured product of the present invention. If an active matrix display device is taken as an example, a TFT (thin film transistor) and a wiring located on the side of the TFT and connected to the TFT are provided on a substrate such as a glass or resin film, and a planarization layer is provided thereon in a manner covering the concave and convex, and a display element is further provided on the planarization layer. The display element and the wiring are connected via contact holes formed in the planarization layer. The cured product formed by curing the photosensitive resin composition of the present invention is preferably used for the planarization layer because of its excellent planarization and pattern dimensional stability. In particular, in recent years, the flexibility of organic EL display devices has become mainstream, and it can also be an organic EL display device in which the substrate having the driving circuit includes a resin film.
[0173] Example
[0174] Hereinafter, the present invention will be described with reference to Examples, but the present invention is not limited to these Examples. First, the evaluation method in each Example and Comparative Example will be described.
[0175] (1) Evaluation of fine pattern processability of negative resin composition containing (D-2) photopolymerization initiator
[0176] A negative resin composition containing a photopolymerization initiator (D-2) was applied to a copper substrate using a spin coater (1H-360S manufactured by Mikasa Co., Ltd.), and heated and dried at 100°C for 3 minutes using a hot plate (SCW-636 manufactured by Dainippon Screen Co., Ltd.) to form a coating film of 10 μm. An alignment exposure machine (PLA-501F manufactured by Canon Co., Ltd.) was used through a photomask having a pattern of L / S=30 μm / 30 μm, a pattern of 20 μm / 20 μm, and a pattern of 15 μm / 15 μm, and an ultra-high pressure mercury lamp was used as a light source at 200 mJ / cm 2The copper substrate formed with the coating film is exposed. The exposure amount is calculated by measuring the illumination of 365nm. Then, it is heated at 120°C for 1 minute, and an automatic developer (AD-1200 manufactured by Takizawa Industry (stock)) is used, and a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution is used as a developer, and the developer is developed in a liquid-covering manner twice for 45 seconds, and rinsed with pure water for 30 seconds. Then, a flat panel display (Flat Panel Display, FPD) microscope (MX61 manufactured by Olympus (stock)) is used to observe the pattern processing part, check the minimum pattern size that can be processed, and evaluate the fine pattern processability based on the following benchmarks. Here, being able to process means that the opening size of the pattern after development is more than 95% of the size of the pattern of the photomask. A and B are set to be qualified, and C is set to be unqualified.
[0177] A: The minimum pattern size is 15μm
[0178] B: The smallest pattern size is 20μm
[0179] C: The smallest pattern size is 30 μm.
[0180] (2) Evaluation of fine pattern processability of positive resin composition containing (D-1) photoacid generator
[0181] The positive resin composition containing the photoacid generator (D-1) was applied to a copper substrate using a spin coater (1H-360S manufactured by Mikasa Co., Ltd.), and heated and dried at 100°C for 3 minutes using a hot plate (SCW-636 manufactured by Dainippon Screen Co., Ltd.) to form a coating film of 10 μm. An alignment exposure machine (PLA-501F manufactured by Canon Co., Ltd.) was used through a photomask having a pattern of L / S=15 μm / 15 μm, a pattern of 10 μm / 10 μm, and a pattern of 5 μm / 5 μm, and an ultra-high pressure mercury lamp was used as a light source at 800 mJ / cm 2 The copper substrate formed with the coating film is exposed. The exposure amount is calculated by measuring the illumination of 365nm. Then, an automatic developer (AD-1200 manufactured by Takizawa Industry (stock)) is used, and a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution is used as a developer, and the development is performed in a liquid-covering manner twice for 45 seconds, and then rinsed with pure water for 30 seconds. Then, an FPD microscope (MX61 manufactured by Olympus (stock)) is used to observe the pattern processing part, check the minimum pattern size that can be processed, and evaluate the fine pattern processability based on the following benchmarks. Here, being able to process means that the opening size of the pattern after development is more than 95% of the size of the pattern of the photomask. A and B are set to be qualified, and C is set to be unqualified.
[0182] A: The minimum pattern size is 5μm
[0183] B: The smallest pattern size is 10μm
[0184] C: The smallest pattern size is 15 μm.
[0185] (3) Evaluation of fine pattern processability of negative resin composition containing (D-1) photoacid generator
[0186] A negative resin composition containing a photoacid generator (D-1) was applied to a copper substrate using a spin coater (1H-360S manufactured by Mikasa Co., Ltd.), and heated and dried at 120°C for 3 minutes using a hot plate (SCW-636 manufactured by Dainippon Screen Co., Ltd.) to form a 15 μm coating film. An alignment exposure machine (PLA-501F manufactured by Canon Co., Ltd.) was used through a photomask having a pattern of L / S=15 μm / 15 μm, a pattern of 10 μm / 10 μm, and a pattern of 5 μm / 5 μm, and an ultra-high pressure mercury lamp was used as a light source at 500 mJ / cm 2 The copper substrate formed with the coating film is exposed. The exposure amount is calculated by measuring the illumination of 365nm. Then, it is heated at 100°C for 3 minutes, and an automatic developer (AD-1200 manufactured by Takizawa Industry (Co., Ltd.) is used, and a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution is used as a developer, and the development is performed in a liquid-covering manner twice for 30 seconds, and then rinsed with pure water for 30 seconds. Then, an FPD microscope (MX61 manufactured by Olympus (Co., Ltd.) is used to observe the pattern processing part, check the minimum pattern size that can be processed, and evaluate the fine pattern processability based on the following criteria. Here, being able to process means that the opening size of the pattern after development is more than 95% of the size of the pattern of the photomask. A to C are qualified, and D is unqualified.
[0187] A: The minimum pattern size is 5μm
[0188] B: The smallest pattern size is 10μm
[0189] C: The minimum pattern size is 15μm
[0190] D: Unable to process a pattern size of 15 μm.
[0191] (4) Evaluation of substrate adhesion of non-photosensitive resin composition
[0192] The non-photosensitive resin composition was applied to a copper substrate using a spin coater (1H-360S manufactured by Mikasa Co., Ltd.), and a 10 μm coating film was formed by heating and drying at 100° C. for 3 minutes using a hot plate (SCW-636 manufactured by Dainippon Screen Co., Ltd.). The copper substrate on which the coating film was formed was heated for 1 hour using an inert oven (CLH-21CD-S manufactured by KOYO THERMO SYSTEM Co., Ltd.) at an oxygen concentration of less than 20 ppm and a heating rate of 3.5° C. / min to 280° C. The cured film was subjected to a cross-cutting method according to Japanese Industrial Standards (JIS) K5400-8.5, with a single blade cutting 10 rows and 10 columns at intervals of 2 mm, and a peeling test was performed using a cellophane adhesive tape, and the substrate adhesion was evaluated according to the following criteria. Set A and B as qualified, and set C, D, and E as unqualified.
[0193] A: The number of grids of the cured film in close contact with the substrate after the test is 100
[0194] B: The number of grids of the cured film in close contact with the substrate after the test is 80 or more and less than 100
[0195] C: The number of grids of the cured film in close contact with the substrate after the test is 50 or more and less than 80
[0196] D: The number of grids of the cured film in close contact with the substrate after the test is 20 or more and less than 50
[0197] E: The number of grids of the cured film in close contact with the substrate after the test is less than 20
[0198] (5) Evaluation of substrate adhesion of negative resin composition containing (D-2) photopolymerization initiator
[0199] A negative resin composition containing a photopolymerization initiator (D-2) was applied to a copper substrate using a spin coater (1H-360S manufactured by Mikasa Co., Ltd.), and heated and dried at 100° C. for 3 minutes using a hot plate (SCW-636 manufactured by Dainippon Screen Co., Ltd.) to form a 10 μm coating film. An alignment exposure machine (PLA-501F manufactured by Canon Co., Ltd.) was used through a photomask having a square pattern of 100 μm×100 μm, with an ultra-high pressure mercury lamp as a light source at 200 mJ / cm 2The copper substrate formed with the coating film was exposed. The exposure amount was calculated by measuring the illumination at 365 nm. Then, it was heated at 120°C for 1 minute, and an automatic developer (AD-1200 manufactured by Takizawa Industry Co., Ltd.) was used, and a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution was used as a developer, and the development was performed in a liquid-covering manner twice for 45 seconds, and then rinsed with pure water for 30 seconds. Then, an inert oven (CLH-21CD-S manufactured by KOYO THERMO SYSTEM Co., Ltd.) was used, and the temperature was raised to 280°C at a heating rate of 3.5°C / min at an oxygen concentration of less than 20 ppm, and then a heating treatment was performed for 1 hour. The shear strength of the obtained cured film pattern was measured using a die shear tester (Dage-Series 4000 manufactured by Nordson Co., Ltd.) under the conditions of a 150 μm wide tool, a height of 1 μm from the copper substrate, and a speed of 15 μm / second. The average value of 10 measurements was taken as the shear strength, and the substrate adhesion was evaluated based on the following criteria. A and B were considered qualified, and C was considered unqualified.
[0200] A: Shear strength is 300mN or more
[0201] B: Shear strength is 250mN or more and less than 300mN
[0202] C: Shear strength is less than 250 mN.
[0203] (6) Evaluation of substrate adhesion of positive resin composition containing (D-1) photoacid generator
[0204] The positive resin composition containing the photoacid generator (D-1) was applied to a copper substrate using a spin coater (1H-360S manufactured by Mikasa Co., Ltd.), and heated and dried at 100° C. for 3 minutes using a hot plate (SCW-636 manufactured by Dainippon Screen Co., Ltd.) to form a 10 μm coating film. An alignment exposure machine (PLA-501F manufactured by Canon Co., Ltd.) was used through a photomask having a square pattern of 100 μm×100 μm, with an ultra-high pressure mercury lamp as the light source, at 800 mJ / cm 2The copper substrate formed with the coating film is exposed. The exposure amount is calculated by measuring the illumination at 365 nm. Then, an automatic developer (AD-1200 manufactured by Takizawa Industry Co., Ltd.) is used, and a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution is used as a developer, and the development is performed in a 45-second double-liquid-covering manner, and pure water is rinsed for 30 seconds. Then, an inert oven (CLH-21CD-S manufactured by KOYO THERMO SYSTEM Co., Ltd.) is used to heat the temperature to 280°C at a heating rate of 3.5°C / min at an oxygen concentration below 20 ppm, and then a heating treatment is performed for 1 hour. Using a die shear tester (Dage-Series 4000 manufactured by Nordson Co., Ltd.), the shear strength of the pattern of the obtained cured film is measured under the conditions of a 150 μm wide tool, a height of 1 μm from the copper substrate, and a speed of 15 μm / second. The average value of 10 measurements was defined as shear strength, and the substrate adhesion was evaluated based on the following criteria: A and B were considered acceptable, and C was considered unacceptable.
[0205] A: Shear strength is 300mN or more
[0206] B: Shear strength is 250mN or more and less than 300mN
[0207] C: Shear strength is less than 250 mN.
[0208] (7) Evaluation of substrate adhesion of negative resin composition containing (D-1) photoacid generator
[0209] The negative resin composition containing the photoacid generator (D-1) was applied to a copper substrate using a spin coater (1H-360S manufactured by Mikasa Co., Ltd.), and heated and dried at 120° C. for 3 minutes using a hot plate (SCW-636 manufactured by Dainippon Screen Co., Ltd.) to form a 15 μm coating film. An alignment exposure machine (PLA-501F manufactured by Canon Co., Ltd.) was used through a photomask having a square pattern of 100 μm×100 μm, with an ultra-high pressure mercury lamp as the light source, at a rate of 500 mJ / cm 2The copper substrate formed with the coating film was exposed. The exposure amount was calculated by measuring the illumination at 365 nm. Then, it was heated at 100°C for 1 minute, and an automatic developer (AD-1200 manufactured by Takizawa Industry Co., Ltd.) was used, and a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution was used as a developer, and the development was performed in a liquid-covering manner twice for 30 seconds, and then rinsed with pure water for 30 seconds. Then, an inert oven (CLH-21CD-S manufactured by KOYO THERMO SYSTEM Co., Ltd.) was used, and the temperature was raised to 200°C at a heating rate of 3.5°C / min at an oxygen concentration of less than 20 ppm, and then a heating treatment was performed for 1 hour. The shear strength of the obtained cured film pattern was measured using a bare die shear tester (Dage-Series 4000 manufactured by Nordson Co., Ltd.) under the conditions of a 150 μm wide tool, a height of 1 μm from the copper substrate, and a speed of 15 μm / second. The average value of 10 measurements was taken as the shear strength, and the substrate adhesion was evaluated based on the following criteria. A and B were considered qualified, and C was considered unqualified.
[0210] A: Shear strength is 200mN or more
[0211] B: Shear strength is 150mN or more and less than 200mN
[0212] C: Shear strength is less than 150 mN.
[0213] (8) Evaluation of storage stability
[0214] After the resin composition was prepared, the viscosity at 25° C. was measured using an E-type viscometer (TVE-25 manufactured by Toki Sangyo Co., Ltd.) 12 to 24 hours later, and the value was defined as V. 1 Then, the resin composition was sealed and stored at room temperature (23°C) for 4 weeks, and then the viscosity was measured and the value was defined as V. 2 The viscosity increase rate (%) is defined as (V 2 -V 1 ) / V 1 ×100, and the storage stability was evaluated based on the following criteria: A, B, and C were considered acceptable, and D was considered unacceptable.
[0215] A: Viscosity increase rate is less than 3%
[0216] B: Viscosity increase rate is 3% or more and less than 5%
[0217] C: Viscosity increase rate is 5% or more and less than 20%
[0218] D: The viscosity increase rate is 20% or more.
[0219] [Synthesis Example 1 Synthesis of polyhydroxystyrene (P1)]
[0220] In a mixed solution to which 500 mL of tetrahydrofuran and 0.01 mol of sec-butyl lithium as an initiator were added, a total of 20 g of p-tert-butoxystyrene and styrene were added in a molar ratio of 3:1, and the mixture was polymerized while stirring at 120°C for 3 hours. 0.1 mol of methanol was added to the reaction solution to terminate the polymerization reaction. Next, in order to purify the polymer, the reaction mixture was injected into methanol, and the precipitated polymer was dried to obtain a white polymer. Furthermore, the polymer was dissolved in 400 mL of acetone, and a small amount of concentrated hydrochloric acid was added at 60°C. After stirring for 7 hours, the polymer was injected into water to precipitate the polymer, and p-tert-butoxystyrene was deprotected and converted into hydroxystyrene. After washing and drying, a refined copolymer (P1) of p-hydroxystyrene and styrene was obtained.
[0221] [Synthesis Example 2: Synthesis of polyimide precursor (P2)]
[0222] Under a dry nitrogen stream, 4,4'-oxydiphthalic anhydride (hereinafter referred to as ODPA) (21.72 g, 0.070 mole) and γ-butyrolactone (hereinafter referred to as GBL) were dissolved in GBL in a flask. Subsequently, 3-aminophenol (hereinafter referred to as MAP) (1.53 g, 0.014 mole), 1,3-bis(3-aminopropyl)tetramethyldisiloxane (hereinafter referred to as SiDA) (0.87 g, 0.0035 mole), and 2,2-bis(3-aminophenyl)hexafluoropropane (19.72 g, 0.059 mole) were added, and stirred at 60°C for 4 hours. After the reaction solution was cooled, it was put into 2.5 L of water, and the generated white precipitate was filtered, washed with water three times, and then vacuum dried at 80°C for 24 hours to obtain a polyimide precursor (P2).
[0223] [Synthesis Example 3: Synthesis of polyimide precursor (P3)]
[0224] A polyimide precursor (P3) was obtained in the same manner as in Synthesis Example 2 except that 2,2-bis(3-aminophenyl)hexafluoropropane (19.72 g, 0.059 mol) was changed to 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (hereinafter referred to as BAHF) (21.55 g, 0.059 mol).
[0225] [Synthesis Example 4: Synthesis of polyimide (P4)]
[0226] The reaction solution obtained in Synthesis Example 3 was further heated to 200°C and stirred for 4 hours. The reaction solution was cooled and then poured into 2.5 L of water. The generated white precipitate was filtered, washed with water three times, and then vacuum dried at 80°C for 24 hours to obtain a polyimide (P4).
[0227] [Synthesis Example 5: Synthesis of polyimide (P5)]
[0228] Under a dry nitrogen stream, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic dianhydride (hereinafter referred to as TDA-100) (30.03 g, 0.1 mol) was added to 100 g of GBL and dissolved by stirring at 60°C. Subsequently, MAP (0.55 g, 0.005 mol) and 2,2-bis(3-aminophenyl)hexafluoropropane (30.1 g, 0.09 mol) were added, and stirred at 60°C for 1 hour. Subsequently, the temperature was raised to 200°C and stirred for 4 hours. Subsequently, the mixture was poured into 3 L of cooled reaction solution water to precipitate, and the precipitate was collected by filtration, washed with water three times, and then dried in a vacuum dryer at 80°C for 5 hours to obtain a polyimide (P5).
[0229] [Synthesis Example 6: Synthesis of polyimide (P6)]
[0230] A polyimide (P6) was obtained in the same manner as in Synthesis Example 5 except that 2,2-bis(3-aminophenyl)hexafluoropropane (30.08 g, 0.09 mol) was changed to BAHF (32.96 g, 0.09 mol).
[0231] [Synthesis Example 7: Synthesis of polyimide precursor (P7)]
[0232] Under a dry nitrogen stream, ODPA (31.02 g, 0.10 mol) was dissolved in 200 g of GBL. BAHF (32.96 g, 0.09 mol: 90 mol% relative to all amines and their derivatives) was added thereto, and the mixture was stirred at 20°C for 1 hour, and then stirred at 50°C for 2 hours. MAP (1.09 g, 0.01 mol: 10 mol% relative to all amines and their derivatives) was then added, and the mixture was stirred at 50°C for 2 hours. Then, a solution diluted with 20 g of GBL of N,N-dimethylformamide dimethyl acetal (21.5 g, 0.18 mol) was added in small amounts each time, and the mixture was further stirred at 50°C for 3 hours. Then, the mixture was put into 3 L of the cooled reaction solution water to precipitate, and the precipitate was collected by filtration, washed with water 3 times, and then dried in a vacuum dryer at 80°C for 5 hours to obtain a polyimide precursor (P7).
[0233] [Synthesis Example 8 Synthesis of polybenzoxazole precursor (P8)]
[0234] Under a dry nitrogen flow, at 60°C, 1,1'-(4,4'-oxybenzoyl)diimidazole (hereinafter referred to as PBOM) (22.93g, 0.100 mole) was dissolved in 234.67g of NMP. MAP (1.09g, 0.010 mole) and 5g of NMP were added thereto, and the mixture was reacted at 85°C for 15 minutes. Then, 6FAP (32.55g, 0.105 mole) and 20g of NMP were added, and the mixture was reacted at 85°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, and the solution was added to 3L of water to obtain a white precipitate. The precipitate was collected by filtration, washed with water 3 times, and dried in a ventilated dryer at 50°C for 3 days to obtain a powder of a polybenzoxazole precursor (P8).
[0235] [Synthesis Example 9: Synthesis of polybenzoxazole (P9)]
[0236] The reaction solution obtained in Synthesis Example 8 was further heated to 200°C and stirred for 4 hours. After cooling, the reaction solution was poured into 2.5 L of water, and the generated white precipitate was filtered, washed with water three times, and then vacuum dried at 80°C for 24 hours to obtain polybenzoxazole (P9).
[0237] [Synthesis Example 10 Synthesis of Organic Salt (M1)]
[0238] Under a dry nitrogen stream, ODPA (6.20 g, 0.020 mol) and 200 g of ion exchange water were added to the flask, and stirred at 80° C. to hydrolyze ODPA. Subsequently, 2,2-bis(3-aminophenyl)hexafluoropropane (6.68 g, 0.020 mol) was added, and stirred at 80° C. for 1 hour. The generated yellow-white precipitate was filtered, washed with water three times, and then vacuum dried at 80° C. for 24 hours to obtain an organic salt (M1).
[0239] [Synthesis Example 11 Synthesis of Organic Salt (M2)]
[0240] An organic salt (M2) was obtained in the same manner as in Synthesis Example 10 except that 2,2-bis(3-aminophenyl)hexafluoropropane (6.68 g, 0.020 mol) was changed to BAHF (7.33 g, 0.020 mol).
[0241] The names of the compounds used in Examples and Comparative Examples are shown below.
[0242] [Synthesis Example 12 Synthesis of Organic Salt (M3)]
[0243] An organic salt (M3) was obtained in the same manner as in Synthesis Example 10 except that 2,2-bis(3-aminophenyl)hexafluoropropane (6.68 g, 0.020 mol) was changed to 2,2-bis(3-amino-4-hydroxyphenyl)propane (5.17 g, 0.020 mol).
[0244] [Synthesis Example 13 Synthesis of Organic Salt (M4)]
[0245] An organic salt (M4) was obtained in the same manner as in Synthesis Example 10 except that ODPA (6.20 g, 0.02 mol) was changed to TDA-100 (6.01 g, 0.02 mol).
[0246] [Synthesis Example 14 Synthesis of Organic Salt (M5)]
[0247] An organic salt (M5) was obtained in the same manner as in Synthesis Example 11 except that ODPA (6.20 g, 0.02 mol) was changed to TDA-100 (6.01 g, 0.02 mol).
[0248] [Synthesis Example 15 Synthesis of Organic Salt (M6)]
[0249] An organic salt (M6) was obtained in the same manner as in Synthesis Example 12 except that ODPA (6.20 g, 0.02 mol) was changed to TDA-100 (6.01 g, 0.02 mol).
[0250] [Synthesis Example 16 Synthesis of Organic Salt (M7)]
[0251] An organic salt (M7) was obtained in the same manner as in Synthesis Example 10 except that ODPA (6.20 g, 0.02 mol) was changed to 4,4′-dicarboxydiphenyl ether (5.16 g, 0.02 mol).
[0252] [Synthesis Example 17 Synthesis of Organic Salt (M8)]
[0253] An organic salt (M8) was obtained in the same manner as in Synthesis Example 11 except that ODPA (6.20 g, 0.02 mol) was changed to 4,4′-dicarboxydiphenyl ether (5.16 g, 0.02 mol).
[0254] [Synthesis Example 18 Synthesis of Organic Salt (M9)]
[0255] An organic salt (M97) was obtained in the same manner as in Synthesis Example 12 except that ODPA (6.20 g, 0.02 mol) was changed to 4,4′-dicarboxydiphenyl ether (5.16 g, 0.02 mol).
[0256] [Synthesis Example 19 Synthesis of Organic Salt (M10)]
[0257] An organic salt (M10) was obtained in the same manner as in Synthesis Example 10, except that ODPA (6.20 g, 0.020 mol) was replaced with phthalic anhydride (2.96 g, 0.020 mol) and 2,2-bis(3-aminophenyl)hexafluoropropane (6.68 g, 0.020 mol) was replaced with aniline (1.86, 0.020 mol).
[0258] The names of the compounds used in Examples and Comparative Examples are shown below.
[0259] <(C) = Solvent>
[0260] GBL: gamma-butyrolactone
[0261] EL: Ethyl lactate
[0262] <(D-1) Photoacid generator>
[0263] HA5-170: HA5-170 (manufactured by Toyo Gosei Co., Ltd.)
[0264] CPI-310FG: CPI-310FG (manufactured by San-Apro)
[0265] <(D-2) Photopolymerization initiator>
[0266] OXE02: "Irgacure" (registered trademark) OXE02 (manufactured by BASF Japan)
[0267] <Radical polymerizable compounds>
[0268] DCP-A: Light Acrylate DCP-A (manufactured by Kyoeisha Chemical Co., Ltd.)
[0269] BP-6EM: Light ester BP-6EM (manufactured by Kyoeisha Chemical Co., Ltd.)
[0270] MOI-BP: Karenz MOI-BP (manufactured by Showa Denko Co., Ltd.)
[0271] <Cross-linking agent>
[0272] MW-100LM: "NIKALAC" (registered trademark) MW-100LM (manufactured by Sanwa Chemical Co., Ltd.)
[0273] MX-270 "NIKALAC" (registered trademark) MX-270 (manufactured by Sanwa Chemical Co., Ltd.)
[0274] TEPIC-VL: TEPIC-VL (manufactured by Nissan Chemical Industries, Ltd.)
[0275] <Adhesion improving agent>
[0276] KBM403 (manufactured by Shin-Etsu Chemical Co., Ltd.)
[0277] <Surfactant>
[0278] PF77: Polyflow No.77 (manufactured by Kyoeisha Chemical Co., Ltd.)
[0279] [Example 1]
[0280] 3.5 g of polyhydroxystyrene (P1), 0.0175 g of organic salt (M1), 2.1 g of GBL, and 3.1 g of EL were mixed and filtered under pressure using a filter with a retention particle size of 1 μm to prepare a non-photosensitive resin composition. The substrate adhesion and storage stability of the non-photosensitive resin composition were evaluated according to the evaluation methods (4) and (8).
[0281] [Example 2 to Example 19]
[0282] A non-photosensitive resin composition was prepared in the same manner as in Example 1, with (A) soluble resin, (B) organic salt and (C) solvent as shown in Table 1. The substrate adhesion and storage stability of the non-photosensitive resin composition were evaluated according to the evaluation methods (4) and (8).
[0283] [Comparative Example 1 to Comparative Example 5]
[0284] A non-photosensitive resin composition was prepared in the same manner as in Example 1, with (A) soluble resin, (B) organic salt and (C) solvent as shown in Table 1. The substrate adhesion and storage stability of the non-photosensitive resin composition were evaluated according to the evaluation methods (4) and (8).
[0285] [Table 1]
[0286]
Table 1
[0287]
[0288] 注) In the table, the values in brackets represent the added amount [unit: g].
[0289] Table 2 shows the evaluation results of Examples 1 to 19 and Comparative Examples 1 to 5.
[0290] [Table 2]
[0291]
Table 2
[0292]
[0293] [Example 20]
[0294] Under a yellow light, 3.5 g of polyhydroxystyrene (P1), 0.0175 g of organic salt (M1), 0.5 g of OXE02, 0.5 g of DCP-A, 1.5 g of BP-6EM, 0.5 g of MOI-BP, 1.0 g of MW-100LM, 0.5 g of MX-270, 0.25 g of KBM403, 0.003 g of PF77, 2.1 g of GBL, and 3.1 g of EL were mixed and pressure filtered using a filter with a retention particle size of 1 μm to prepare a negative resin composition. The fine pattern processability, substrate adhesion, and storage stability of the negative resin composition containing the photopolymerization initiator (D-2) were evaluated according to the evaluation methods of (1), (5), and (8).
[0295] [Example 21] to [Example 40]
[0296] A negative resin composition containing a photopolymerization initiator (D-2) was prepared in the same manner as in Example 20, with (A) a soluble resin, (B) an organic salt, (C) a solvent, (D) a photosensitive agent, and other components being as described in Tables 3-1 and 3-2. The fine pattern processability, substrate adhesion, and storage stability of the negative resin composition containing the photopolymerization initiator (D-2) were evaluated according to the evaluation methods (1), (5), and (8).
[0297] [Comparative Example 6] to [Comparative Example 10]
[0298] A negative resin composition containing a photopolymerization initiator (D-2) was prepared in the same manner as in Example 20, with (A) a soluble resin, (B) an organic salt, (C) a solvent, (D) a photosensitizer, and other components being as described in Table 3-2. The fine pattern processability, substrate adhesion, and storage stability of the negative resin composition containing the photopolymerization initiator (D-2) were evaluated according to the evaluation methods (1), (5), and (8).
[0299] [Table 3-1]
[0300]
[0301]
[0302] Table 4 shows the evaluation results of Examples 20 to 40 and Comparative Examples 6 to 10.
[0303] [Table 4]
[0304]
Table 4
[0305]
[0306] [Example 41]
[0307] Under a yellow light, 3.5 g of polyhydroxystyrene (P1), 0.0175 g of organic salt (M1), 0.4 g of HA5-170, 0.17 g of TrisP-PA, 0.34 g of MX-270, 0.33 g of KBM1403, 4.3 g of GBL, and 2.4 g of EL were mixed and pressure filtered using a filter with a retention particle size of 1 μm to prepare a positive resin composition containing a photoacid generator (D-1). The fine pattern processability, substrate adhesion, and storage stability of the positive resin composition containing a photoacid generator (D-1) were evaluated according to the evaluation methods (2), (6), and (8).
[0308] [Example 42 to Example 61]
[0309] A positive resin composition containing a photoacid generator (D-1) was prepared in the same manner as in Example 41, with (A) a soluble resin, (B) an organic salt, (C) a solvent, (D) a photosensitive agent, and other components being as described in Tables 5-1 and 5-2. The fine pattern processability, substrate adhesion, and storage stability of the positive resin composition containing the photoacid generator (D-1) were evaluated according to the evaluation methods of (2), (6), and (8).
[0310] [Comparative Example 11 to Comparative Example 15]
[0311] A positive resin composition containing a photoacid generator (D-1) was prepared in the same manner as in Example 41, with (A) a soluble resin, (B) an organic salt, (C) a solvent, (D) a photosensitizer, and other components being as described in Table 5-2. The fine pattern processability, substrate adhesion, and storage stability of the positive resin composition containing the photoacid generator (D-1) were evaluated according to the evaluation methods of (2), (6), and (8).
[0312] [Table 5-1]
[0313]
[0314]
[0315] Table 6 shows the evaluation results of Examples 41 to 61 and Comparative Examples 11 to 15.
[0316] [Table 6]
[0317]
Table 6
[0318]
[0319] [Example 62]
[0320] Under a yellow light, 2.35 g of polyhydroxystyrene (P1), 0.0118 g of an organic salt (M1), 0.17 g of CPI-310FG, 3.0 g of TEPIC-VL, 0.20 g of KBM403, and 10 g of GBL were mixed and pressure filtered using a filter with a retention particle size of 1 μm to prepare a negative resin composition containing a photoacid generator (D-1). The fine pattern processability, substrate adhesion, and storage stability of the negative resin composition containing a photoacid generator (D-1) were evaluated according to the evaluation methods of (3), (7), and (8).
[0321] [Example 63 to Example 68]
[0322] (A) soluble resin, (B) organic salt, (C) solvent, (D) photosensitizer, and other components are as described in Table 7, and a negative resin composition containing (D-1) photoacid generator is prepared in the same manner as in Example 62. The fine pattern processability, substrate adhesion, and storage stability of the positive resin composition containing (D-1) photoacid generator are evaluated according to the evaluation methods (3), (7), and (8).
[0323] [Comparative Example 16 to Comparative Example 18]
[0324] (A) soluble resin, (B) organic salt, (C) solvent, (D) photosensitizer, and other components are as described in Table 7, and a negative resin composition containing (D-1) photoacid generator is prepared in the same manner as in Example 62. The fine pattern processability, substrate adhesion, and storage stability of the positive resin composition containing (D-1) photoacid generator are evaluated according to the evaluation methods (3), (7), and (8).
[0325] [Table 7]
[0326]
[0327] Table 8 shows the evaluation results of Examples 62 to 68 and Comparative Examples 16 to 18.
[0328] [Table 8]
[0329]
Table 8
[0330]
[0331] Industrial Applicability
[0332] The cured product formed by curing the resin composition of the present invention can be used as an insulating film, a protective film constituting an electronic component, or a planarization layer and a pixel segmentation layer constituting a display device. As electronic components, active components such as transistors, diodes, integrated circuits (ICs), and memories having semiconductors, passive components such as resistors, capacitors, and inductors can be cited. More specifically, it is preferably used for the passivation film of a semiconductor, a surface protective film of a semiconductor element, a TFT (Thin Film Transistor), an interlayer insulating film such as an interlayer insulating film between redistribution wiring in a multilayer wiring for high-density installation of 2 to 10 layers, an insulating film of a touch screen display, a protective film, an insulating layer of an organic electric field light-emitting element, etc., and various structures can also be used. As a display device, an organic EL display device having a planarization layer, a first electrode, a pixel segmentation layer, an organic EL layer, and a second electrode on a substrate, and a planarization layer and / or a pixel segmentation layer containing the cured product of the present invention. Taking an active matrix display device as an example, a TFT (thin film transistor) and wiring located on the side of the TFT and connected to the TFT are provided on a substrate such as a glass or resin film, a planarization layer is provided thereon in a manner covering the concave and convex portions, and a display element is further provided on the planarization layer. The display element and the wiring are connected via contact holes formed in the planarization layer.
Claims
1. A resin composition comprising (A) a soluble resin, (B) an organic salt and (C) a solvent, wherein the organic salt (B) is an organic salt formed from an organic compound having a carboxyl group and an organic compound having an amino group, and the amount of the organic salt (B) is 0.01 to 10 parts by mass relative to 100 parts by mass of the soluble resin (A).
2. The resin composition according to claim 1, wherein the (B) organic salt contains an organic salt having a structure represented by formula (6) or formula (7), [Chemistry 1] (In formula (6), R 14 represents a tetravalent organic group having 4 to 40 carbon atoms; R 15 represents a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms; R 16 represents a divalent organic group having 1 to 40 carbon atoms) (In formula (7), R 17 It represents a divalent organic group having 1 to 40 carbon atoms; in, R 17 Does not contain carboxyl or carboxylate groups; R 18 represents a divalent organic group having 1 to 40 carbon atoms). 3 . The resin composition according to claim 1 , wherein the (A) soluble resin contains at least one soluble resin selected from the group consisting of polyimide, polybenzoxazole, precursors thereof, and copolymers thereof. 4 . The resin composition according to claim 1 , further comprising (D) a photosensitizer.
5. The resin composition according to any one of claims 1 to 4, wherein the (A) soluble resin contains a A polyimide having a structure represented by formula (1), A polybenzoxazole having a structure represented by formula (3), A polyimide precursor having a structure represented by formula (4) wherein g in formula (4) is 2, A polybenzoxazole precursor having a structure represented by formula (4) wherein g in formula (4) is 0, and at least one soluble resin selected from the group consisting of copolymers thereof, [Chemistry 2] (In formula (1), R 1 represents a tetravalent organic group having 4 to 40 carbon atoms; R 2 The structure represented by expression (2) (In formula (2), R 3 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates that R 4 and R 5 represents a monovalent organic group having 1 to 20 carbon atoms; a and b each independently represent an integer of 1 to 4, c and d each independently represent an integer of 0 to 1; * represents a chemical bond) [Chemistry 3] (In formula (3), R 6 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates; R 7 represents a divalent organic group having 4 to 40 carbon atoms) [Chemistry 4] (In formula (4), R 8 represents a divalent to tetravalent organic group having 4 to 40 carbon atoms; R 9 The structure represented by formula (5); R 10 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms; g represents 0 or 2) (In formula (5), R 11 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates that R 12 and R 13 represents a monovalent organic group having 1 to 20 carbon atoms; k and l each independently represent an integer of 1 to 4, m and n each independently represent an integer of 0 to 1; * represents a chemical bond).
6. The resin composition according to any one of claims 1 to 5, wherein R in the formula (6) 16 And R in the formula (7) 18 is the structure represented by formula (8), [Chemistry 5] (In formula (8), R 19 By single bond, -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 - indicates that R 20 and R 21 represents a monovalent organic group having 1 to 20 carbon atoms; o and p each independently represent an integer of 1 to 4, q and r each independently represent an integer of 0 to 1; and * represents a chemical bond).
7. The resin composition according to claim 6, wherein R in the formula (8) 19 -C(CF 3 ) 2 -.
8. A cured product obtained by curing the resin composition according to any one of claims 1 to 7.
9. An electronic component comprising the hardened material according to claim 8.
10. A display device comprising the hardened object according to claim 8.