Support-free high-strength polyether sulfone flat microporous membrane and preparation method thereof
Through the combination of the hourglass-shaped asymmetric gradient sponge-like structure of the unsupported high-strength polyethersulfone flat microporous membrane and the steam and liquid-induced phase conversion method, the existing technology solves the difficulty of regulating the mesoporous structure, the complexity of the process, and the lack of durability. solve the problem and achieve the preparation of microporous membranes with high strength, low damage and high flux, which are suitable for industrial applications.
Patent Information
- Application Number
- CN202410971968.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2018-09-17
- Publication Date
- 2024-10-11
AI Technical Summary
Existing polyethersulfone microporous membranes have problems such as difficulty in controlling the pore structure, complex production processes, and insufficient durability during the preparation process. In particular, the symmetrical structure membrane is easy to be damaged, and the existing asymmetric flat membrane formula system has poor stability and repeatability. Not good enough to be suitable for industrialization.
Using the preparation method of unsupported high-strength polyethersulfone flat microporous membrane, through the hourglass-shaped asymmetric gradient sponge-like micropore distribution, the micropores of the separation layer and the upper and lower surface cortex increase in a gradient, and the pore diameter gradually increases from the separation layer. It is prepared by combining steam and liquid-induced phase conversion methods to improve the mechanical strength and flux of the membrane.
A microporous membrane with high strength, low damage and high flux has been realized, with high separation efficiency and strong interception capacity, which simplifies the process and improves the feasibility of adjusting the membrane structure and performance.
Smart Images

Figure CN118751091A_ABST
Abstract
Description
This application is a divisional application of the invention patent application with the application date of September 17, 2018, application number 201811084562.3, and invention name “A kind of unsupported high-strength polyethersulfone flat microporous membrane and preparation method”. Technical Field
[0001] The invention belongs to the field of microporous separation membrane preparation, and particularly relates to an unsupported high-strength polyethersulfone flat microporous membrane and a preparation method thereof. Background Art
[0002] In the past 20 years, the industrialization of microporous membranes and related filter membrane products in my country has reached a certain scale. At present, the commercialized microporous membranes and widely used varieties in China are mainly the following categories: 1. Mixed cellulose (CN-CA); 2. Polyamides, such as nylon 6 (PA-6) and nylon 66 (PA-66) microporous membranes. These membranes have good hydrophilicity and are more resistant to alkalis but not acids. They are not easily corroded in ketones, phenols, ethers and high molecular weight alcohols. 3. Polyfluorines, such as polyvinylidene fluoride membranes (PVDF) and polytetrafluoroethylene membranes (PTFE). These two types of microporous membranes have excellent chemical stability and are suitable for use at high temperatures. In particular, PTFE membranes have an operating temperature of -40℃ to 260℃, and are resistant to strong acids, strong alkalis and various organic solvents. Due to their strong hydrophobicity, they are very suitable for filtering steam and various corrosive liquids. 4. Polyolefins, such as polypropylene (PP) stretched microporous membranes and polypropylene (PP) fiber deep filtration membranes. The current commercial membranes have various configurations such as flat plate and hollow fiber. They have various pore sizes ranging from ultrafiltration-grade micropores to 70μm. 5. Polyethersulfone (PES) microporous membranes, which have good chemical and thermal stability, radiation resistance, fast filtration rate, and a wide range of applications.
[0003] Patent CN1579603A discloses a method for preparing a polyethersulfone hollow fiber membrane, and prepares a polyethersulfone hollow fiber membrane hemodialysis membrane by a non-solvent induced phase separation method (NIPS method). U.S. Patent US4774039 discloses a method for preparing an asymmetric flat membrane without a finger-like pore structure. The formulation system used has poor stability and poor repeatability and is not suitable for industrialization. Patent CN101790413B provides a polyethersulfone-containing membrane-making stock solution, a separation membrane, and a method for manufacturing the separation membrane with high strength, high water permeability, high blocking performance and good anti-fouling properties. The thermally induced phase separation method (TIPS method) has technical problems such as complex production process and difficult pore structure control. The prepared separation membrane is a symmetrical structure with a filter cortex on the outside, which is easily damaged during use. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and provide an unsupported high-strength polyethersulfone flat microporous membrane and a preparation method thereof.
[0005] To solve the technical problem, the solution of the present invention is:
[0006] Provided is an unsupported high-strength polyethersulfone flat microporous membrane, comprising an upper surface cortex and a lower surface cortex, wherein the upper surface cortex and the lower surface cortex are provided with micropores on their surfaces, the micropores between the upper and lower surface cortexes are distributed in an hourglass-shaped asymmetric gradient sponge-like manner, the middle of the micropores is a separation layer of the membrane; and the pore diameter of the micropores from the separation layer to the upper and lower surface cortexes increases continuously.
[0007] As an improvement, the pore size of the separation layer is 0.05 to 2 μm.
[0008] As an improvement, the micropore diameter of the inner and outer skin layers of the separation layer is 0.1 to 50 μm.
[0009] As an improvement, the membrane has a porosity of at least 85%.
[0010] As an improvement, the separation layer is spaced at least 10 μm from one of the upper surface skin layer and the lower surface skin layer, preferably 20 μm.
[0011] The present invention also provides a method for preparing an unsupported high-strength polyethersulfone flat microporous membrane, comprising the following steps:
[0012] (a) preparing a film casting solution by mixing polyethersulfone, a porogen, a hydrophilic additive and a solvent;
[0013] (b) The casting liquid is extruded from the spinneret and cast onto a steel plate to obtain support to obtain a flat original membrane;
[0014] (c) Film formation through dry water mist spraying process;
[0015] (d) Finally, after rinsing and drying, an unsupported high-strength polyethersulfone flat microporous membrane is prepared.
[0016] As an improvement, the mass concentration of polyethersulfone is 12-18%, the mass concentration of the porogen is 10-30%, the mass concentration of the hydrophilic additive is 1-20%, and the mass concentration of the solvent is 32-77%.
[0017] As an improvement, the porogen inducing agent is one or two of tributyl phosphate, ethanol, diethylene glycol, triethylene glycol, ethylene glycol, polyethylene glycol or glycerol.
[0018] As an improvement, the hydrophilic additive is one or two of sulfonated polyethersulfone, polymethyl methacrylate, polyoxyethylene-polyoxypropylene block copolymer or polyvinyl pyrrolidone.
[0019] As an improvement, the solvent is one or two of triethyl phosphate, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide and trimethyl phosphate.
[0020] As an improvement, the dry steam spray process is that an external water vapor atomization device delivers water mist which contacts the original membrane and then separates into a membrane.
[0021] As an improvement, the humidity of the water mist is greater than 95%.
[0022] Description of the Invention Principle
[0023] PES microporous membrane is mainly prepared by non-solvent phase inversion method (NIPS). The main principle of this method is to physically exchange solvent and non-solvent to separate the homogeneous polymer solution into polymer-rich phase and polymer-poor phase. The polymer-rich phase forms a network gel structure after solidification, and the polymer-poor phase becomes membrane pores after desolventization. The non-solvent phase inversion method is called liquid-induced phase inversion method (LIPS) when the non-solvent is liquid, and the vapor-induced phase inversion method (VIPS) when the non-solvent is vapor.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) This cross-sectional micropore distribution is an hourglass-shaped asymmetric gradient sponge-like structure with excellent performance. The separation layer is far away from the feed end and the discharge end, which can fully protect the separation layer from mechanical damage and fouling by viruses and particulate matter. This structure has high separation efficiency and strong interception capacity; the separation layer is a little distance away from the outer skin layer, which protects the separation layer while also increasing the flux of the membrane.
[0026] (2) This method is relatively simple and easy to implement, and the combined method of steam and liquid phase transformation gives this membrane preparation method more process feasibility and can better adjust the membrane structure and performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is an electron microscope image of the upper surface of an unsupported high-strength polyethersulfone flat microporous membrane;
[0028] Figure 2 This is a cross-sectional electron microscope image of an unsupported high-strength polyethersulfone flat microporous membrane;
[0029] Figure 3 is a schematic diagram of the cross-sectional structure of the micropore in Example 1;
[0030] Figure 4 This is a magnified electron microscope image of the cross-section separation layer of an unsupported high-strength polyethersulfone flat microporous membrane;
[0031] Figure 5 This is an electron microscope image of the lower surface cortex of an unsupported high-strength polyethersulfone flat microporous membrane.
[0032] Figure 3 Middle: 1- separation layer; 2- upper surface cortex; 3- lower surface cortex. DETAILED DESCRIPTION
[0033] Example 1: Add 16% by weight of polyethersulfone resin (BASF 6020P), 15% of diethylene glycol, 15% of polyvinylpyrrolidone K-17, 0.5% of polyoxyethylene-polyoxypropylene block copolymer F127, and 53.5% of dimethylformamide into a stirring tank, stir at 60°C for 12 hours, filter, and vacuum degas for 24 hours to obtain a casting solution. The casting solution at a temperature of 35 degrees is extruded through a spinneret and cast onto a steel plate to obtain support to obtain a flat original membrane. After a water vapor section with a humidity of 95% and a residence time of 100s, it is immersed in a rinsing water tank after steam and liquid phase transformation, and finally dried to obtain an unsupported high-strength polyethersulfone flat microporous membrane. The membrane surface is a smooth single open-pore microporous structure (attached Figure 1 , 4 ), the pores at 20 μm below the surface cortex 2 on the cross section are the smallest, which is the separation layer 1. The pores from the separation layer 1 to the two surface cortexes are getting larger and larger, and the micropores are hourglass-shaped asymmetric microporous sponge structures (see Appendix Figure 2 , 3 ), the average pore size of the microporous membrane of the present invention is 0.22 μm, the thickness is 135 μm, and the pure water flux under 0.1 MPa and 25°C is 25 ml / cm 2. min.
[0034] Example 2: 14% by weight of polyethersulfone resin (BASF 6020P), 11% of triethylene glycol, 14% of polyvinylpyrrolidone K-30, 1.5% of sulfonated polyethersulfone (sulfonation degree 25%), and 59.5% of dimethylacetamide were added to a stirring tank, stirred at 60°C for 12 hours, filtered, and vacuum degassed for 24 hours to obtain a casting solution. The casting solution at a temperature of 30°C was extruded through a spinneret and cast on a steel plate to obtain a support to obtain a flat original membrane. After a water vapor section with a humidity of 97%, the residence time was 180s, and after steam and liquid phase transformation, it was immersed in a rinsing water tank, and finally dried to obtain an unsupported high-strength polyethersulfone flat microporous membrane. The membrane surface is a smooth single-hole microporous structure. The pores at 25 μm below the surface cortex 2 on the cross section are the smallest. This is the separation layer 1. The pores from the separation layer 1 to the two surface cortexes are getting larger and larger. The micropores are hourglass-shaped asymmetric microporous sponge structures. The average pore size of the microporous membrane of the present invention is distributed at 0.45 μm, the membrane thickness is 120 μm, and the pure water flux under 0.1 MPa and 25 ° C is 85 ml / cm 2. min.
[0035] Example 3: 18% by weight of polyethersulfone resin (BASF 6020P), 18% ethylene glycol, 12% polyvinylpyrrolidone K-30 and 42% N-methylpyrrolidone, 10% dimethyl sulfoxide were added to a stirring tank, stirred at 60°C for 12 hours, filtered, and vacuum degassed for 24 hours to obtain a casting solution. The casting solution at a temperature of 45°C was extruded and cast on a steel plate through a spinneret to obtain a support to obtain a flat original membrane. After a water vapor section with a humidity of 97% and a residence time of 30s, it was immersed in a rinsing water tank after steam and liquid phase conversion, and finally dried to obtain an unsupported high-strength polyethersulfone flat microporous membrane. The membrane surface is a smooth single open microporous structure. The pores at 10μm below the surface cortex 2 on the cross section are the smallest, which is the separation layer 1. The pores from the separation layer 1 to the two surface cortexes are getting larger and larger, and the micropores are hourglass-shaped asymmetric microporous sponge structures. The average pore size of the microporous membrane of the present invention is 0.05 μm, the membrane thickness is 150 μm, and the pure water flux is 3.4 ml / cm at 0.1 MPa and 25°C. 2. min.
[0036] Example 4: 12% by weight of polyethersulfone resin (BASF 6020P), 10% of triethylene glycol, 20% of diethylene glycol, 17% of polyvinylpyrrolidone K-17 and 1% of sulfonated polyethersulfone (sulfonation degree 20%), and 40% of dimethylacetamide were added to a stirring tank, stirred at 60°C for 12 hours, filtered, and vacuum degassed for 24 hours to obtain a casting solution. The casting solution at a temperature of 30°C was extruded and cast on a steel plate through a spinneret to obtain a support to obtain a flat original membrane. After a steam section with a humidity of 95%, the residence time was 200s, and after steam and liquid phase conversion, it was immersed in a rinsing water tank, and finally dried to obtain an unsupported high-strength polyethersulfone flat microporous membrane. The membrane surface is a smooth single open microporous structure, and the pores at 30μm below the surface cortex 2 on the cross section are the smallest, which is the separation layer 1. The pores from the separation layer 1 to the two surface cortexes are getting larger and larger, and the micropores are hourglass-shaped asymmetric microporous sponge structures. The average pore size of the microporous membrane of the present invention is 0.8 μm, the membrane thickness is 150 μm, and the pure water flux is 200 ml / cm at 0.1 MPa and 25°C. 2. min.
[0037] Example 5: 12% by weight of polyethersulfone resin (BASF 6020P), 30% polyethylene glycol, 18% polyvinylpyrrolidone K-30 and 2% sulfonated polyethersulfone (sulfonation degree 15%), and 38% dimethylacetamide were added to a stirring tank, stirred at 60°C for 12 hours, filtered, and vacuum degassed for 24 hours to obtain a casting solution. The casting solution at a temperature of 30°C was extruded and cast on a steel plate through a spinneret to obtain a support to obtain a flat original membrane. After a steam section with a humidity of 98%, the residence time was 300s, and after steam and liquid phase conversion, it was immersed in a rinsing water tank, and finally dried to obtain an unsupported high-strength polyethersulfone flat microporous membrane. The membrane surface is a smooth single open microporous structure. The pores at 40μm below the surface cortex 2 on the cross section are the smallest, which is the separation layer 1. The pores from the separation layer 1 to the two surface cortexes are getting larger and larger, and the micropores are hourglass-shaped asymmetric microporous sponge structures. The average pore size of the microporous membrane of the present invention is 2 μm, the membrane thickness is 160 μm, and the pure water flux is 1350 ml / cm at 0.1 MPa and 25°C. 2. min.
[0038] Example 6: 17% by weight of polyethersulfone resin (BASF 6020P), 15% ethylene glycol, 12% polyvinylpyrrolidone K-30, 22% triethyl phosphate and 34% N-methylpyrrolidone were added to a stirring tank, stirred at 60°C for 12 hours, filtered and vacuum degassed for 24 hours to obtain a casting solution. The casting solution at a temperature of 40°C was extruded and cast on a steel plate through a spinneret to obtain a support to obtain a flat original membrane. After a water vapor section with a humidity of 97% and a residence time of 60s, it was immersed in a rinsing water tank after steam and liquid phase conversion, and finally dried to obtain an unsupported high-strength polyethersulfone flat microporous membrane. The membrane surface is a smooth single open microporous structure. The pores 15μm below the upper surface of the cross section are the smallest, which is the separation layer 1. The pores from the separation layer 1 to the two surface cortical layers are getting larger and larger, and the micropores are hourglass-shaped asymmetric microporous sponge structures. The average pore size of the microporous membrane of the present invention is distributed in 0.1 μm, the membrane thickness is 140 μm, and the pure water flux under the conditions of 0.1 MPa and 25°C is 14 ml / cm 2 ·min.
[0039] Example 7: 17% by weight of polyethersulfone resin (BASF 6020P), 15% ethylene glycol, 10% diethylene glycol, 1% sulfonated polyethersulfone (sulfonation degree 20%), 22% trimethyl phosphate and 35% N-methylpyrrolidone were added to a stirring tank, stirred at 60°C for 12 hours, filtered and vacuum degassed for 24 hours to obtain a casting solution. The casting solution at a temperature of 40°C was extruded and cast on a steel plate through a spinneret to obtain a support to obtain a flat original membrane. After a water vapor section with a humidity of 96% and a residence time of 60s, it was immersed in a rinsing water tank after steam and liquid phase conversion, and finally dried to obtain an unsupported high-strength polyethersulfone flat microporous membrane. The membrane surface is a smooth single open microporous structure. The pores 15μm below the upper surface of the cross section are the smallest, which is the separation layer 1. The pores from the separation layer 1 to the two surface cortical layers are getting larger and larger, and the micropores are hourglass-shaped asymmetric microporous sponge structures. The average pore size of the microporous membrane of the present invention is distributed in 0.1 μm, the membrane thickness is 120 μm, and the pure water flux under the conditions of 0.1 MPa and 25°C is 11 ml / cm 2. min.
[0040] Any simple modifications, equivalent changes and modifications made to the above implementation cases based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall still fall within the scope of the technical solution of the present invention.
Claims
1. A method for preparing an unsupported high-strength polyethersulfone flat microporous membrane, characterized in that: The steps include: (a) preparing a film casting solution by mixing polyethersulfone, a porogen, a hydrophilic additive and a solvent; (b) The casting liquid is extruded from the spinneret and cast onto a steel plate to obtain support to obtain a flat original membrane; (c) Film formation through dry water mist spraying process; (d), finally, rinsing and drying to obtain an unsupported high-strength polyethersulfone flat microporous membrane; and The dry steam spraying process is that the water mist delivered by the external water vapor atomization device contacts with the original membrane and separates into a membrane, and the humidity of the water mist is greater than 95%. Characterized in that the mass concentration of the polyethersulfone is 12-18%, the mass concentration of the porogen is 10-30%, the mass concentration of the hydrophilic additive is 18-20%, and the mass concentration of the solvent is 32-77%, characterized in that the hydrophilic additive is sulfonated polyethersulfone and polyvinylpyrrolidone.
2. The preparation method according to claim 1, characterized in that: The porogen inducing agent is one or two of tributyl phosphate, ethanol, diethylene glycol, triethylene glycol, ethylene glycol, polyethylene glycol or glycerol.
3. The preparation method according to claim 1, characterized in that: The solvent is one or two of triethyl phosphate, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide and trimethyl phosphate.
4. An unsupported high-strength polyethersulfone flat microporous membrane prepared by the preparation method according to any one of claims 1 to 3, characterized in that: It comprises an upper surface cortex and a lower surface cortex, the upper surface cortex and the lower surface cortex are covered with micropores, the micropores between the upper and lower surface cortexes are distributed in an hourglass-shaped asymmetric gradient sponge-like manner, and the middle of the micropores is the separation layer of the membrane; the pore size of the micropores from the separation layer to the upper and lower surface cortexes continuously increases; the pore size of the separation layer is 0.05 to 2 μm; the pore size of the micropores on both sides of the separation layer is 0.1 to 50 μm; and the distance between the separation layer and one of the upper surface cortex and the lower surface cortex is at least 10 μm.
5. The unsupported high-strength polyethersulfone flat microporous membrane according to claim 4, characterized in that: The membrane has a porosity of at least 85%.