Preparation method and application of modified biomass for adsorbing vanadium-containing solution
Through simplified roasting and ultrasonic impregnation processes, an efficient modified biomass adsorbent is prepared, which solves the problems of complex processes and low adsorption efficiency in the existing technology, achieves efficient adsorption of vanadium and reuse of modified liquid, significantly Reduced potion consumption.
Patent Information
- Application Number
- CN202410952162.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-11
AI Technical Summary
The existing modified biomass adsorption process is complicated, the modified liquid cannot be reused, the chemical consumption is large, and the adsorption efficiency is low, making it difficult to effectively improve the adsorption performance of vanadium.
Modified biomass is prepared by roasting the crushed biomass in an inert atmosphere and mixing it with polyethylenimine and alcohol compounds, performing ultrasonic impregnation, adsorbing and desorbing through magnetic stirring, and reusing the modified liquid to simplify process and improve adsorption efficiency.
It achieves simplification of the process, reuse of modified liquid and reduction of chemical consumption, and improves the adsorption efficiency and capacity of vanadium, with the adsorption rate reaching 93-98% and the desorption rate reaching 95-98%.
Smart Images

Figure CN118751218A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of modified biomass, and specifically relates to a preparation method and application of modified biomass for adsorbing vanadium-containing solution. Background Art
[0002] Biomass adsorbent materials are low-cost, abundant in resources, non-toxic, and have good biocompatibility. They contain many active functional groups that adsorb metal ions and have a high affinity for metal ions. However, many commonly used chemical modification methods have not greatly improved the adsorption capacity and selectivity of metal ions. They have a small specific surface area, low adsorption capacity, and unsatisfactory adsorption performance. At the same time, they are difficult to recycle due to their small particle size, and solid residues are easily left in the solution, showing weak mechanical strength. In order to improve the adsorption performance of biomass, the mechanical strength and adsorption performance of the adsorbent material are enhanced by biomass modification.
[0003] Vanadium is a rare high melting point metal with good physical and chemical properties and catalytic performance. Vanadium and its compounds are widely used in industrial fields such as steel, non-ferrous alloys, chemicals, oil refining, glass and ceramics. At present, most processes use acid leaching to extract vanadium from stone coal mines, but the vanadium concentration in the acid leaching solution is low. Therefore, the adsorption of vanadium has become an important research topic for technicians at home and abroad.
[0004] The patented technology of "a preparation method and application of PEI modified biochar" (CN112547015A) is as follows: placing orange peel powder in a muffle furnace for oxygen-limited pyrolysis, cooling it to room temperature, taking it out, treating it with HCl, washing it to neutrality, and drying it to obtain raw biochar; adding the raw biochar to a NaOH solution, stirring it at 100°C for 5 hours; after stirring, washing it to neutrality; then drying it at 80°C for 12 hours to obtain alkali-treated biochar; adding the above-mentioned alkali-treated biochar to a PEI / methanol mixture with a mass concentration of 20%, stirring it at 30°C for 24 hours, and then transferring the mixture to a 1% (w / v) glutaraldehyde solution, continuing to stir for 30 minutes, and drying it to obtain PEI-modified biochar, and the modified biochar adsorbs Cu 2+ 、Cd 2+ , Pd 2+ This technology first carbonizes the biomass, then acid-washes it, alkali-modifies it, treats it with PEI, and then cross-links it to obtain modified biochar. The preparation process is complicated. The biochar is cross-linked with glutaraldehyde, which makes the modified liquid unable to be reused and consumes a lot of reagents.
[0005] "Preparation and application of a high-efficiency adsorption-reduction material of metallic vanadium using waste green tea residue as raw material"
[0006] (CN113893824A) patented technology, which provides a preparation and application of a high-efficiency adsorption-reduction material of metal vanadium using waste green tea residue as raw material. The surface and pores of green tea residue biochar are modified with zero-valent iron, and the vanadium adsorption capacity is further increased to 71.6 mg / g. This technology uses zero-valent iron modified biochar to adsorb vanadium. Although the adsorption capacity is improved, the adsorption efficiency is low.
[0007] The patented technology of "A modified mangosteen shell biochar and a method for reducing vanadium in water using the same" (CN107583609A) involves washing the mangosteen peel, heating it in a high-temperature vacuum, washing it, and drying it to obtain a powdered material, which is then mixed with a sodium hydroxide solution, shaken and filtered to obtain a filter cake, which is then washed and dried to obtain modified mangosteen shell biochar. The modified mangosteen shell biochar is mixed with vanadium-containing wastewater, shaken and filtered to obtain a purified solution. This technology uses sodium hydroxide solution to modify the mangosteen shell biochar to adsorb vanadium-containing waste. Although the solution is purified, the adsorption efficiency is low.
[0008] In summary, the existing modified biomass adsorption has technical defects such as complex preparation process, non-reusable modified liquid, high reagent consumption, and low adsorption efficiency. Summary of the invention
[0009] The present invention aims to overcome the defects of the prior art and aims to provide a method for preparing modified biomass for adsorbing vanadium-containing solution with simple process, reusable modified liquid and low reagent consumption; the modified biomass for adsorbing vanadium-containing solution prepared by the method has high adsorption efficiency for vanadium-containing solution and can be reused.
[0010] To achieve the above purpose, the specific steps of the technical solution adopted by the present invention are:
[0011] Step 1.1, the crushed biomass is placed in a tubular furnace, roasted at 500-800° C. for 1-2 h in an inert atmosphere, and cooled to room temperature to obtain carbonized biomass.
[0012] Step 1.2: Mix polyethyleneimine and an alcohol compound at a mass concentration of 5 to 20% to obtain a modified solution.
[0013] Step 1.3, according to the liquid-solid ratio of 10-20L / Kg, the modified liquid and the carbonized biomass are mixed, and then ultrasonically immersed for 1-4h at room temperature, solid-liquid separation is carried out to obtain modified biomass and modified liquid for adsorbing vanadium-containing solution.
[0014] Add polyethyleneimine to the modified liquid to prepare the modified liquid described in step 1.2, and reuse it.
[0015] The application method of the prepared modified biomass for adsorbing vanadium-containing solution is:
[0016] Step 2.1, adsorption
[0017] The modified biomass for adsorbing the vanadium-containing solution is added to the vanadium-containing solution at a liquid-solid ratio of 20 to 50 L / Kg, stirred with a magnetic stirrer for 8 to 24 hours at room temperature, and the solid and liquid are separated to obtain adsorbed biomass and adsorbed liquid.
[0018] Step 2.2, desorption
[0019] According to the liquid-solid ratio of 10-20 L / Kg, the desorbent of 25 wt% H2SO4 is mixed with the adsorbed biomass, stirred with a magnetic stirrer for 2-6 hours at room temperature, and the solid-liquid is separated to obtain the desorbed biomass and vanadium-containing desorption liquid.
[0020] The desorbed biomass can be repeatedly used to adsorb the vanadium-containing solution.
[0021] The particle size of the crushed biomass is 0.1-1 mm; the biomass is wood chips or straw.
[0022] The inert atmosphere is one of nitrogen, helium and argon.
[0023] The alcohol compound is methanol or ethanol.
[0024] The power of the ultrasound is 80-100W.
[0025] The vanadium-containing solution has: a vanadium valence of +5; a vanadium concentration of 0.5-3 g / L; and a pH of 2-4.
[0026] The rotation speed of the magnetic stirrer in step 2.1 and step 2.2 is 500-800 r / min.
[0027] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art:
[0028] 1. The present invention carbonizes biomass to obtain carbonized biomass, and then directly mixes the carbonized biomass with a modified liquid and immerses them in ultrasound, so that the modified biomass can be obtained in one step. Compared with the existing technology of preparing modified biochar by acid washing-alkali treatment-PEI treatment-crosslinking agent crosslinking, the process is simple.
[0029] 2. The modified liquid obtained by ultrasonic impregnation and solid-liquid separation in the present invention can be directly added with polyethyleneimine to prepare the modified liquid, so that the modified liquid can be reused. Compared with the modified liquid of the prior art that cannot be reused, the consumption of reagents is significantly reduced.
[0030] 3. The modified biomass prepared by the present invention for adsorbing vanadium-containing solutions has a porous structure, a larger specific surface area and a developed porosity. The polyethyleneimine used in the present invention is a soluble polymeric amine, the surface of which contains rich amine functional group molecular chains, which are composed of a large number of primary amines, secondary amines and tertiary amines, and has a good affinity for vanadium. The biomass is modified with polyethyleneimine to improve the adsorption efficiency of the biomass. The amine groups on the modified biomass are protonated, and some pentavalent vanadium ions are adsorbed to the active sites through electrostatic action; the amine groups undergo redox reactions with V(V), and V(V) is reduced to V(IV). The biomass modified by polyethyleneimine has an adsorption capacity of 143.3 mg / g for vanadium, and has a high adsorption efficiency for vanadium.
[0031] 4. The desorbed biomass obtained after desorption of the biomass in the present invention still has amine groups, and has the ability to adsorb the vanadium-containing solution. Therefore, the modified biomass still has the adsorption capacity after adsorption-desorption and can be reused.
[0032] The modified biomass prepared by the invention and used for absorbing vanadium-containing solution is tested to have an adsorption rate of 93-98% and a desorption rate of 95-98%.
[0033] The modified biomass prepared by the present invention for adsorbing vanadium-containing solution is tested before and after adsorption of vanadium-containing solution: the adsorption rate is 93-98%; the desorption liquid after desorption with 25wt% H2SO4 as desorbent is tested: the desorption rate is 95-98%.
[0034] Therefore, the invention has the characteristics of simple preparation, repeated use of modified liquid and low consumption of reagents. The prepared modified biomass has high adsorption efficiency for vanadium-containing solution and can be repeatedly used. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a SEM image of a modified biomass prepared by the present invention for adsorbing vanadium-containing solution;
[0036] Figure 2 for Figure 1 The SEM image of the modified biomass after adsorption of the vanadium-containing solution is shown;
[0037] Figure 3 for Figure 2 EDS pattern of biomass after adsorption is shown. Specific implementation methods
[0039] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, but is not intended to limit the scope of protection thereof.
[0040] A preparation method and application of modified biomass for adsorbing vanadium-containing solution. The steps of the preparation method described in this specific embodiment are:
[0041] Step 1.1, the crushed biomass is placed in a tubular furnace, roasted at 500-800° C. for 1-2 h in an inert atmosphere, and cooled to room temperature to obtain carbonized biomass.
[0042] Step 1.2: Mix polyethyleneimine and an alcohol compound at a mass concentration of 5 to 20% to obtain a modified solution.
[0043] Step 1.3, according to the liquid-solid ratio of 10-20L / Kg, the modified liquid and the carbonized biomass are mixed, and then ultrasonically immersed for 1-4h at room temperature, solid-liquid separation is carried out to obtain modified biomass and modified liquid for adsorbing vanadium-containing solution.
[0044] Add polyethyleneimine to the modified liquid to prepare the modified liquid described in step 1.2, and reuse it.
[0045] The application method of the prepared modified biomass for adsorbing vanadium-containing solution is:
[0046] Step 2.1, adsorption
[0047] The modified biomass for adsorbing the vanadium-containing solution is added to the vanadium-containing solution at a liquid-solid ratio of 20 to 50 L / Kg, stirred with a magnetic stirrer for 8 to 24 hours at room temperature, and the solid and liquid are separated to obtain adsorbed biomass and adsorbed liquid.
[0048] Step 2.2, desorption
[0049] According to the liquid-solid ratio of 10-20 L / Kg, the desorbent of 25 wt% H2SO4 is mixed with the adsorbed biomass, stirred with a magnetic stirrer for 2-6 hours at room temperature, and the solid-liquid is separated to obtain the desorbed biomass and vanadium-containing desorption liquid.
[0050] The desorbed biomass can be repeatedly used to adsorb the vanadium-containing solution.
[0051] The biomass is wood chips or straw.
[0052] The inert atmosphere is one of nitrogen, helium and argon.
[0053] The alcohol compound is methanol or ethanol.
[0054] The power of the ultrasound is 80-100W.
[0055] The vanadium-containing solution has: a vanadium valence of +5; a vanadium concentration of 0.5-3 g / L; and a pH of 2-4.
[0056] The rotation speed of the magnetic stirrer in step 2.1 and step 2.2 is 500-800 r / min.
[0057] In this specific implementation mode:
[0058] The particle size of the pulverized biomass is 0.1 to 1 mm.
[0059] This will not be described in detail in the embodiments.
[0060] Example 1
[0061] A preparation method and application of modified biomass for adsorbing vanadium-containing solution. The steps of the preparation method described in this embodiment are:
[0062] Step 1.1, the crushed biomass is placed in a tubular furnace, roasted at 600° C. for 2 h in an inert atmosphere, and cooled to room temperature to obtain carbonized biomass.
[0063] Step 1.2, polyethyleneimine and an alcohol compound are mixed at a mass concentration of 10% to obtain a modified solution.
[0064] Step 1.3, according to the liquid-solid ratio of 18L / Kg, the modified liquid and the carbonized biomass are mixed, and then ultrasonically immersed for 2h at room temperature, solid-liquid separation is performed to obtain modified biomass and modified liquid for adsorbing vanadium-containing solution.
[0065] Add polyethyleneimine to the modified liquid to prepare the modified liquid described in step 1.2, and reuse it.
[0066] The application method of the prepared modified biomass for adsorbing vanadium-containing solution is:
[0067] Step 2.1, adsorption
[0068] According to the liquid-solid ratio of 30L / Kg, the modified biomass for adsorbing the vanadium-containing solution is added to the vanadium-containing solution, stirred with a magnetic stirrer for 24 hours at room temperature, and the solid and liquid are separated to obtain the adsorbed biomass and the adsorbed liquid.
[0069] Step 2.2, desorption
[0070] According to the liquid-solid ratio of 20L / Kg, the desorbent of 25wt% H2SO4 was mixed with the adsorbed biomass, stirred for 6h with a magnetic stirrer at room temperature, and the solid-liquid was separated to obtain the desorbed biomass and vanadium-containing desorption liquid.
[0071] The desorbed biomass can be repeatedly used to adsorb the vanadium-containing solution.
[0072] The biomass is wood chips.
[0073] The inert atmosphere is nitrogen.
[0074] The alcohol compound is methanol.
[0075] The power of the ultrasound is 100W.
[0076] The vanadium-containing solution has: a vanadium valence of +5; a vanadium concentration of 0.5 g / L; and a pH of 2.5.
[0077] The rotation speed of the magnetic stirrer in step 2.1 and step 2.2 is 500r / min.
[0078] The modified biomass prepared in this embodiment for adsorbing vanadium-containing solution was tested before and after adsorption of the vanadium-containing solution: the adsorption rate was 98%; the desorption liquid after desorption with a desorbent of 25wt% H2SO4 was tested: the desorption rate was 98%.
[0079] Example 2
[0080] A preparation method and application of modified biomass for adsorbing vanadium-containing solution. The steps of the preparation method described in this embodiment are:
[0081] Step 1.1, the crushed biomass is placed in a tubular furnace, roasted at 800° C. for 1.8 h in an inert atmosphere, and cooled to room temperature to obtain carbonized biomass.
[0082] Step 1.2, polyethyleneimine and an alcohol compound are mixed at a mass concentration of 5% to obtain a modified solution.
[0083] Step 1.3, according to the liquid-solid ratio of 15L / Kg, the modified liquid and the carbonized biomass are mixed, and then ultrasonically immersed for 3 hours at room temperature, and the solid and liquid are separated to obtain the modified biomass and the modified liquid for adsorbing the vanadium-containing solution.
[0084] Add polyethyleneimine to the modified liquid to prepare the modified liquid described in step 1.2, and reuse it.
[0085] The application method of the prepared modified biomass for adsorbing vanadium-containing solution is:
[0086] Step 2.1, adsorption
[0087] According to the liquid-solid ratio of 20L / Kg, the modified biomass for adsorbing the vanadium-containing solution was added to the vanadium-containing solution, stirred with a magnetic stirrer for 12 hours at room temperature, and the solid and liquid were separated to obtain the adsorbed biomass and the adsorbed liquid.
[0088] Step 2.2, desorption
[0089] According to the liquid-solid ratio of 10L / Kg, the desorbent of 25wt% H2SO4 and the adsorbed biomass are mixed, stirred with a magnetic stirrer for 4 hours at room temperature, and the solid-liquid is separated to obtain the desorbed biomass and vanadium-containing desorption liquid.
[0090] The desorbed biomass can be repeatedly used to adsorb the vanadium-containing solution.
[0091] The biomass is straw.
[0092] The inert atmosphere is argon.
[0093] The alcohol compound is methanol.
[0094] The power of the ultrasound is 80W.
[0095] The vanadium-containing solution has: a vanadium valence of +5; a vanadium concentration of 3 g / L; and a pH of 2.
[0096] The rotation speed of the magnetic stirrer in step 2.1 and step 2.2 is 800r / min.
[0097] The modified biomass prepared in this embodiment for adsorbing vanadium-containing solution was tested before and after adsorption of the vanadium-containing solution: the adsorption rate was 97%; the desorption liquid after desorption with a desorbent of 25wt% H2SO4 was tested: the desorption rate was 95%.
[0098] Example 3
[0099] A preparation method and application of modified biomass for adsorbing vanadium-containing solution. The steps of the preparation method described in this embodiment are:
[0100] Step 1.1, the crushed biomass is placed in a tubular furnace, roasted at 700° C. for 1.5 h in an inert atmosphere, and cooled to room temperature to obtain carbonized biomass.
[0101] Step 1.2, polyethyleneimine and an alcohol compound are mixed at a mass concentration of 15% to obtain a modified solution.
[0102] Step 1.3, according to the liquid-solid ratio of 10L / Kg, the modified liquid and the carbonized biomass are mixed, and then ultrasonically immersed for 4 hours at room temperature, solid-liquid separation is performed to obtain modified biomass and modified liquid for adsorbing vanadium-containing solution.
[0103] Add polyethyleneimine to the modified liquid to prepare the modified liquid described in step 1.2, and reuse it.
[0104] The application method of the prepared modified biomass for adsorbing vanadium-containing solution is:
[0105] Step 2.1, adsorption
[0106] According to the liquid-solid ratio of 50L / Kg, the modified biomass for adsorbing the vanadium-containing solution was added to the vanadium-containing solution, stirred with a magnetic stirrer for 8 hours at room temperature, and the solid and liquid were separated to obtain the adsorbed biomass and the adsorbed liquid.
[0107] Step 2.2, desorption
[0108] According to the liquid-solid ratio of 12L / Kg, the desorbent of 25wt% H2SO4 and the adsorbed biomass are mixed, stirred for 2h with a magnetic stirrer at room temperature, and the solid-liquid is separated to obtain the desorbed biomass and vanadium-containing desorption liquid.
[0109] The desorbed biomass can be repeatedly used to adsorb the vanadium-containing solution.
[0110] The biomass is straw.
[0111] The inert atmosphere is helium.
[0112] The alcohol compound is ethanol.
[0113] The power of the ultrasound is 90W.
[0114] The vanadium-containing solution has: a vanadium valence of +5; a vanadium concentration of 1 g / L; and a pH of 3.
[0115] The rotation speed of the magnetic stirrer in step 2.1 and step 2.2 is 600r / min.
[0116] The modified biomass prepared in this embodiment for adsorbing vanadium-containing solution was tested before and after adsorption of the vanadium-containing solution: the adsorption rate was 96%; the desorption liquid after desorption with a desorbent of 25wt% H2SO4 was tested: the desorption rate was 95%.
[0117] Example 4
[0118] A preparation method and application of modified biomass for adsorbing vanadium-containing solution. The steps of the preparation method described in this embodiment are:
[0119] Step 1.1, the crushed biomass is placed in a tubular furnace, roasted at 500° C. for 1 h in an inert atmosphere, and cooled to room temperature to obtain carbonized biomass.
[0120] Step 1.2, polyethyleneimine and an alcohol compound are mixed at a mass concentration of 20% to obtain a modified solution.
[0121] Step 1.3, according to the liquid-solid ratio of 20L / Kg, the modified liquid and the carbonized biomass are mixed, and then ultrasonically immersed for 1h at room temperature, solid-liquid separation is performed to obtain modified biomass and modified liquid for adsorbing vanadium-containing solution.
[0122] Add polyethyleneimine to the modified liquid to prepare the modified liquid described in step 1.2, and reuse it.
[0123] The application method of the prepared modified biomass for adsorbing vanadium-containing solution is:
[0124] Step 2.1, adsorption
[0125] According to the liquid-solid ratio of 40L / Kg, the modified biomass for adsorbing the vanadium-containing solution was added to the vanadium-containing solution, stirred with a magnetic stirrer for 16 hours at room temperature, and the solid and liquid were separated to obtain the adsorbed biomass and the adsorbed liquid.
[0126] Step 2.2, desorption
[0127] According to the liquid-solid ratio of 15L / Kg, the desorbent of 25wt% H2SO4 and the adsorbed biomass are mixed, stirred with a magnetic stirrer for 5 hours at room temperature, and the solid-liquid is separated to obtain the desorbed biomass and vanadium-containing desorption liquid.
[0128] The desorbed biomass can be repeatedly used to adsorb the vanadium-containing solution.
[0129] The biomass is wood chips.
[0130] The inert atmosphere is nitrogen.
[0131] The alcohol compound is ethanol.
[0132] The power of the ultrasound is 100W.
[0133] The vanadium-containing solution has: a vanadium valence of +5; a vanadium concentration of 2 g / L; and a pH of 4.
[0134] The rotation speed of the magnetic stirrer in step 2.1 and step 2.2 is 700r / min.
[0135] The modified biomass prepared in this embodiment for adsorbing vanadium-containing solution was tested before and after adsorption of the vanadium-containing solution: the adsorption rate was 93%; the desorption liquid after desorption with a desorbent of 25wt% H2SO4 was tested: the desorption rate was 96%.
[0136] Compared with the prior art, this specific implementation has the following positive effects:
[0137] 1. In this specific implementation, the biomass is carbonized to obtain carbonized biomass, and then the carbonized biomass is directly mixed with the modified liquid and immersed in ultrasound, so that the modified biomass can be obtained in one step. Compared with the existing technology of preparing modified biochar by acid washing-alkali treatment-PEI treatment-crosslinking agent crosslinking, the process is simple.
[0138] 2. In this specific embodiment, the modified liquid obtained by ultrasonic impregnation and solid-liquid separation can be directly added with polyethyleneimine to prepare the modified liquid, so that the modified liquid can be reused. Compared with the modified liquid of the prior art that cannot be reused, the consumption of reagents is significantly reduced.
[0139] 3. The modified biomass prepared in this specific embodiment for adsorbing vanadium-containing solution is shown in the accompanying drawings: Figure 1 This is a SEM image of the modified biomass prepared in Example 1 for adsorbing vanadium-containing solution; Figure 2 for Figure 1 The SEM image of the modified biomass after adsorption of the vanadium-containing solution is shown; Figure 3 for Figure 2 The EDS graph of the biomass after adsorption is shown. Figure 1 It can be seen that the modified biomass used to adsorb vanadium-containing solutions has a porous structure, a larger specific surface area and a developed porosity, which improves the adsorption rate of vanadium-containing solutions. Figure 2 , Figure 3 It can be seen that the biomass contains vanadium after adsorption, indicating that the modified biomass prepared for adsorbing vanadium-containing solution successfully adsorbs vanadium.
[0140] The polyethyleneimine used in this specific embodiment is a soluble polymeric amine, the surface of which contains rich amine functional group molecular chains, composed of a large number of primary amines, secondary amines and tertiary amine groups, and has a good affinity for vanadium. Biomass is modified with polyethyleneimine to improve the adsorption efficiency of biomass. The amine groups on the modified biomass are protonated, and some pentavalent vanadium ions are adsorbed to the active sites through electrostatic effects; the amine groups undergo redox reactions with V(V), and V(V) is reduced to V(IV). The biomass modified with polyethyleneimine has an adsorption capacity of up to 143.3 mg / g for vanadium, and has a high adsorption efficiency for vanadium.
[0141] 4. In this specific implementation method, the desorbed biomass obtained after desorption of the biomass still has amine groups, which has the ability to adsorb the vanadium-containing solution. Therefore, the modified biomass still has the adsorption capacity after adsorption-desorption and can be reused.
[0142] The modified biomass prepared in this specific embodiment for adsorbing vanadium-containing solution is tested to have an adsorption rate of 93-98% and a desorption rate of 95-98%.
[0143] The vanadium-containing solution before and after adsorption of the modified biomass prepared by this specific implementation method for adsorbing vanadium-containing solution was tested: the adsorption rate was 93-98%; the desorption liquid after desorption with a desorbent of 25wt% H2SO4 was tested: the desorption rate was 95-98%.
[0144] Therefore, the specific implementation method has the characteristics of simple preparation, repeated use of the modified solution and low consumption of reagents. The prepared modified biomass has high adsorption efficiency for the vanadium-containing solution and can be repeatedly used.
Claims
1. A method for preparing modified biomass for adsorbing vanadium-containing solution, characterized in that The specific steps of the preparation method are: Step 1.1, placing the crushed biomass into a tubular furnace, roasting it at 500-800° C. for 1-2 hours under an inert atmosphere, and cooling it to room temperature to obtain carbonized biomass; Step 1.2, mixing polyethyleneimine and an alcohol compound at a mass concentration of 5 to 20% to obtain a modified solution; Step 1.3, mixing the modified liquid and the carbonized biomass at a liquid-solid ratio of 10 to 20 L / Kg, and then ultrasonically immersing for 1 to 4 hours at room temperature to separate the solid and the liquid, thereby obtaining a modified biomass and a modified liquid for adsorbing a vanadium-containing solution; Add polyethyleneimine to the modified liquid to prepare the modified liquid described in step 1.2, and reuse it.
2. A method for applying the modified biomass for adsorbing vanadium-containing solution obtained by the preparation method according to claim 1, characterized in that The specific steps of the application method are: Step 2.1, adsorption Adding the modified biomass for adsorbing the vanadium-containing solution to the vanadium-containing solution at a liquid-solid ratio of 20 to 50 L / Kg, stirring with a magnetic stirrer for 8 to 24 hours at room temperature, separating the solid and the liquid, and obtaining the adsorbed biomass and the adsorbed liquid; Step 2.2, desorption According to the liquid-solid ratio of 10 to 20 L / Kg, a desorbent of 25 wt% H2SO4 and the adsorbed biomass are mixed, stirred for 2 to 6 hours with a magnetic stirrer at room temperature, and solid-liquid separation is performed to obtain the desorbed biomass and vanadium-containing desorption liquid; The desorbed biomass can be repeatedly used to adsorb the vanadium-containing solution.
3. The method for preparing modified biomass for adsorbing vanadium-containing solution according to claim 1, characterized in that The particle size of the crushed biomass is 0.1-1 mm; the biomass is wood chips or straw.
4. The method for preparing modified biomass for adsorbing vanadium-containing solution according to claim 1, characterized in that The inert atmosphere is one of nitrogen, helium and argon.
5. The method for preparing modified biomass for adsorbing vanadium-containing solution according to claim 1, characterized in that The alcohol compound is methanol or ethanol.
6. The method for preparing modified biomass for adsorbing vanadium-containing solution according to claim 1, characterized in that The power of the ultrasound is 80-100W.
7. The application method of modified biomass for adsorbing vanadium-containing solution according to claim 2, characterized in that The vanadium-containing solution has: a vanadium valence of +5; a vanadium concentration of 0.5-3 g / L; and a pH of 2-4.
8. The application method of modified biomass for adsorbing vanadium-containing solution according to claim 2, characterized in that The rotation speed of the magnetic stirrer in step 2.1 and step 2.2 is 500-800 r / min.
Citation Information
Patent Citations
Method for removing hexavalent chromium in water by utilizing polyethyleneimine modified graphite oxide
CN103962108A
Polyethyleneimine modified biomass charcoal material and preparation method thereof, and application of polyethyleneimine modified biomass charcoal material to modification of lithium-sulfur battery diaphragm
CN107673350A
Preparation method and application of PEI modified biochar
CN112547015A
Impregnated biomass for treating vanadium (IV)-containing solution and preparation method thereof
CN114288992A
Preparation method of composite modified biochar and application of composite modified biochar in cadmium and lead polluted soil