Preparation method for improving stability of caprolactam Cu-Beta zeolite catalyst prepared from caprolactone and application of Cu-Beta zeolite catalyst

By improving the copper loading method of ammonia stripping on dealubilized Beta zeolite, a Cu-Beta zeolite catalyst was prepared, which solved the problem of easy catalyst deactivation and realized the efficient, low-energy and environmentally friendly production of caprolactam from caprolactone.

CN118751279AActive Publication Date: 2024-10-11DALIAN UNIV OF TECH +1

Patent Information

Application Number
CN202410835986.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-11
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Existing catalysts for the preparation of caprolactam from caprolactone are prone to deactivation under high temperature and high pressure, and also pose problems of equipment corrosion and environmental pollution, making it difficult to achieve efficient and low-energy industrial production.

Method used

Using dented-modified dealuated Beta zeolite as a support, copper was loaded via an improved ammonia stripping method to prepare Cu-Beta zeolite catalysts. This enhanced the dispersion and stability of copper particles, avoided the use of chromium and nickel additives, and improved the catalyst's resistance to sintering.

Benefits of technology

In gas-solid phase reactions, it improves the stability and selectivity of catalysts, reduces energy consumption, and minimizes equipment corrosion and environmental pollution, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751279A_ABST
    Figure CN118751279A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of petrochemical catalysis, and relates to a preparation method for improving the stability of a caprolactam Cu-Beta zeolite catalyst prepared from caprolactone and application of the catalyst. According to the invention, dealuminated Beta zeolite modified by chiseling is used as a carrier, and copper is loaded in a pore channel of the zeolite carrier by using an improved ammonia distillation method. The hole digging modification means that a weak organic alkali control desiliconization technology is applied to the dealuminated Beta zeolite carrier, so that hydroxyl holes generated by dealumination of the dealuminated Beta zeolite carrier are enlarged, and the purpose of better containing and stabilizing nano and sub-nano copper particles is achieved. The core of the improved ammonia distillation method is that a zeolite carrier is impregnated in a copper ammonia complex solution in an isovolumetric manner, so that the copper ammonia complex is mainly subjected to a reaction of depositing copper hydroxide in zeolite pore channels in the ammonia distillation process, and the anti-sintering capability is improved. When the Cu-Beta catalyst prepared by the method provided by the invention is applied to a reaction for preparing caprolactam by gas-solid phase hydroamination of caprolactone, the activity and selectivity are high, and the stability is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of petrochemical catalysis, and relates to a preparation method and application of a Cu-Beta zeolite catalyst for improving the stability of caprolactone to caprolactam. Background Art

[0002] ε-Caprolactam (CPL) is a white solid organic compound, most of which is used to produce polycaprolactam chips, and a small part is used to produce lysine and pharmaceutical intermediates. Among the downstream products of polycaprolactam chips, nylon-6 fiber and engineering plastics consume about 70% and 20% of polycaprolactam chips respectively. The remaining polycaprolactam chips are processed into packaging films and food cling films.

[0003] Nylon-6 is the first synthetic fiber product developed in the world. The most outstanding advantage of nylon-6 fiber is that it has higher wear resistance than all other fibers. It is 10 times more wear-resistant than cotton and 20 times more wear-resistant than wool. At the same time, the strength of nylon-6 fiber is 1-2 times higher than cotton, 4-5 times higher than wool, and 3 times higher than viscose fiber. Adding a small amount of polyamide fiber to blended fabrics can greatly improve its wear resistance, elastic recovery rate and flexural fracture resistance. In addition, nylon-6 fiber also has good moisture absorption and dyeability. Nylon-6 fiber can be used as civilian silk and industrial silk. Nylon civilian silk is used to make shirts, pullovers, pajamas, carpets, blankets, cords and bags, etc.; industrial silk is used to make tents, car tires, transmission belts, hoses, cables, fishing nets, ropes, insulation materials, etc.

[0004] At present, the benzene-based caprolactam process is the mainstream process for producing caprolactam. This process mainly includes three basic processes: benzene to cyclohexanone, cyclohexanone to cyclohexanone oxime, and cyclohexanone oxime rearrangement to caprolactam.

[0005] People familiar with the art know that the traditional benzene-based caprolactam process has many serious problems. However, in recent years, people have made some successful improvements to the traditional benzene-based caprolactam process in accordance with the requirements of green chemistry and atomic economy, including the use of benzene selective hydrogenation to produce cyclohexene and cyclohexene hydration and dehydrogenation to produce cyclohexanone processes in the benzene-to-cyclohexanone step to replace the non-selective hydrogenation of benzene to produce cyclohexane and the cyclohexane air oxidation process to produce cyclohexane; in the cyclohexanone-to-cyclohexanone oxime step, the cyclohexanone ammoximation process catalyzed by titanium silicon molecular sieves has eliminated the hydroxylamine sulfate process (HSO) that produces ammonium sulfate as a by-product and has equipment corrosion problems.

[0006] Despite this, the improved benzene-based caprolactam process still has many disadvantages. These include: (1) the efficiency of the process of selective hydrogenation of benzene to cyclohexene and the process of hydration of cyclohexanol is low; (2) the solvent consumption of the cyclohexanone ammoximation process is large, and the TS-1 catalyst deactivates quickly and consumes a lot during the reaction (titanium silicon molecular sieve is expensive. Cyclohexanone ammoximation to produce cyclohexanone oxime is a liquid phase reaction. The titanium silicon molecular sieve catalyst is in a strong alkaline environment for a long time, and the skeleton silicon dissolves and causes the catalyst to be ineffectively lost); (3) The liquid phase Beckmann rearrangement process (the current mainstream process) still uses fuming sulfuric acid as a catalyst, which not only corrodes the equipment, but also produces 1.5 to 1.8 tons of ammonium sulfate as a by-product for every ton of caprolactam produced. The vapor phase Beckmann rearrangement technology, which people have high hopes for, has serious problems such as rapid catalyst deactivation. People have encountered setbacks in their efforts to replace the liquid phase Beckmann rearrangement process with the vapor phase Beckmann rearrangement process.

[0007] In view of the technical status of the existing benzene-based caprolactam production process and the problems faced in the development of new processes, if we want to obtain a new process for the efficient preparation of caprolactam in the near future that has no low-value by-products (such as ammonium sulfate), no equipment corrosion and environmental pollution problems, high process atomic utilization, and low energy consumption (low carbon emissions), it is imperative to find a new way to carry out technical development and research.

[0008] As early as 1957, Shell Company first disclosed a method for preparing caprolactam from caprolactone in US Patent No. 2817646. Specifically, the method uses a hydrogenation catalyst (such as neutral Raney nickel) to prepare caprolactam from ammonia, hydrogen and caprolactone raw materials at 175-200°C and 7-40 standard atmospheres. However, the main products of the reaction are actually various amides, such as polyamides, amine amides and hydroxyamides. The yield of caprolactam is only about 4%. Obviously, the selectivity of this method is so poor that it has no application value.

[0009] In 1961, the Union Carbide Corporation (UCC) of the United States disclosed a method for preparing caprolactam in US Pat. No. 3,000,879. The method is to heat a 25% aqueous solution of 6-hydroxycaproamide to 300-475°C in a closed container, and prepare caprolactam through a non-catalytic reaction under high pressure (pressure up to 15 MPa), and a 30% single-pass caprolactam yield can be obtained. It is undoubtedly unimaginable for a bulk chemical to achieve industrial production under high temperature and high pressure using an intermittent reactor.

[0010] In the same year, Union Carbide Corporation of the United States once again disclosed a process for preparing caprolactam from caprolactone in US Patent US3000800. Specifically, the process is a process of preparing caprolactam by mixing caprolactone with ammonia water or primary amine aqueous solution under high pressure (P>22.1MPa) and above the critical temperature of ammonia and water (373℃<T>473℃) through non-catalytic reaction. This method has been successfully industrialized, but the process can only be carried out under high temperature and high pressure, and the energy consumption is huge. Moreover, the non-catalytic reaction carried out under high temperature and high pressure is easy to generate polymers, so the actual yield of caprolactam is low, not exceeding 50%. This may be the main reason why Union Carbide Corporation of the United States later stopped the production line of the process for preparing caprolactam from caprolactone. On the other hand, the raw material of caprolactone at that time came from the oxidation reaction of cyclohexanone and peracetic acid. Peracetic acid is a strong oxidant and is extremely unstable. Peracetic acid will explode when it encounters high heat, reducing agents or metal ions. In fact, peracetic acid is explosive when the concentration is greater than 45%, and it will explode even at -20℃. Therefore, the production process of caprolactone was extremely dangerous at that time. This may also be an important reason why Union Carbide later stopped the production line of caprolactam from caprolactone.

[0011] In 1964, Teijin Co., Ltd. of Japan disclosed a catalytic method for preparing caprolactam from amide derivatives of caprolactone, 6-hydroxycaproamide or 6-hydroxycaproic acid in U.S. Patents US3317516 and US3317517. Specifically, the catalytic method disclosed in the above patents is to heat caprolactone, 6-hydroxycaproamide or amide derivatives of 6-hydroxycaproic acid and ammonia water to 200-400° C. in a high-pressure reactor under the catalysis of at least one or a combination of hydrogenation catalysts containing precious metals, cobalt, and nickel to obtain caprolactam with less coloration. The method can be used under a hydrogen atmosphere. Obviously, the reaction conditions of the catalytic method are relatively mild. However, the single-pass yield of caprolactam obtained by the method is also not high, with a maximum of only 45.1%, so the economic efficiency of the method is not high.

[0012] In 1964, a French company disclosed an improved method for preparing caprolactam from caprolactone under non-catalytic conditions of high temperature and high pressure in British patent GB1121109. In previous patents, researchers found that in the absence of solvent, caprolactone and ammonia reacted at a temperature of 300°C to produce only polymers. Therefore, water had to be added as a solvent for the reaction to prevent the formation of polymers. However, the caprolactam product has a strong affinity for water and needs to be extracted with a solvent. Chloroform is effective as an extractant, but even if chloroform is used for extraction under the most favorable conditions, a large amount of chloroform must be used to extract caprolactam from a relatively dilute reaction solution. This means that solvent extraction is quite difficult and expensive. In response to this problem, the patent proposed an improved method: non-catalytic amination of caprolactone to produce caprolactam in the presence of a water-soluble neutral salt (soluble alkali metal or alkaline earth metal salt of an inorganic or organic acid). It was surprisingly found from the results that even at a high salt concentration, the amination reaction result would not be adversely affected. However, after adding salt, the extraction efficiency of caprolactam from the reaction product solution increased from 72.5% (caprolactam extraction rate of chloroform without adding salt) to 94.3% (caprolactam extraction rate of chloroform after adding ammonium sulfate). This can reduce the amount of chloroform used as the extractant.

[0013] In 1965, Union Carbide Corporation of the United States disclosed a continuous two-stage process for preparing caprolactam in U.S. Patent No. 3320241. The technical background of the process is that people already knew that the non-catalytic reaction of caprolactone and ammonia under high temperature and high pressure could produce caprolactam. However, the reaction under high temperature and high pressure is not suitable for industrial application. First, due to the limitation of reaction equilibrium, the single-pass yield of the reaction is relatively low. Secondly, the reaction process will produce a large number of irreversible by-products. Since the yield of each process is very low, the reaction intermediates and unconverted caprolactone must be recycled, which will increase energy consumption and carbon emissions. In addition, since the reaction generates a large number of irreversible by-products, the separation process is also very complicated. All of these make the operating cost too high. Accordingly, the new process proposed in the patent is that in the first stage of conversion, a mixture of caprolactone, ammonia and water is reacted at a relatively low temperature, and the reaction time is controlled so that a large amount of caprolactone is converted into a reaction intermediate. Then, in the second stage conversion, the product of the first stage conversion reaction is converted under the high temperature (300-400°C) and ultra-high pressure (136-680 standard atmospheres) required to form caprolactam. The downstream of the two-stage conversion reaction is the separation stage. The task of the separation stage is to separate caprolactam from the mixture containing caprolactam and reaction intermediates, and to recycle the unreacted products and intermediates back to the first stage for reconversion. Since the intermediates can be converted through the entire two-stage process after returning to the first stage, the reaction time is long, which is conducive to the maximum conversion into the target product caprolactam. The caprolactam separated from the second stage reaction mixture must undergo multiple steps of purification to become a pure product. All the residues produced during the product purification process can be recycled back to the first stage for reconversion to become the target product as much as possible. The use of this process can achieve a caprolactam yield of 90.2%. The process of this process is complicated and the second step is still a high-pressure reaction, which has extremely high requirements for production equipment and management, and the difficulty of industrialization is also relatively large.

[0014] In 1966, Kanegafuchi, BOSEKI KABUSHIKI KAISHA of Japan first disclosed a catalytic method for preparing caprolactam from caprolactone in the gas phase in British patent GB1109540. The method is to first vaporize caprolactone and a certain amount of water, then mix with ammonia and hydrogen, and the mixed gas is catalytically reacted by a copper chromite catalyst at 120-350°C and normal pressure. The conversion rate of caprolactone in this method can reach 100%, and the selectivity of caprolactam can reach 97%. However, the resin generated by the polymerization side reaction is deposited on the catalyst, resulting in rapid deactivation of the catalyst. This has become a major obstacle to the industrial application of the method. In addition, the copper chromite catalyst used in the method is toxic and will produce a large amount of chromium-containing wastewater during the preparation process, which is unfavorable to environmental protection.

[0015] In 1967, DuPont Canada disclosed a non-catalytic method for preparing caprolactam from caprolactone in Canadian Patent CA770148. The method involves reacting caprolactone or polycaprolactone with aqueous ammonia at 305-365°C in a stainless steel reactor at 18-45 MPa, and a maximum single-pass yield of caprolactam of 85% can be obtained. The method provided in the patent shows that polycaprolactone is a byproduct that can be reversed to the target product.

[0016] In 1968, Stamicarbon of the Netherlands disclosed in U.S. Patent No. 3401161 a non-catalytic process for preparing caprolactam by reacting caprolactone with ammonia in an inert organic solvent. The reaction is carried out at very high temperature and pressure (T>330°C, 125atm>P>90atm), and the maximum yield of caprolactam can be 60%. Organic solvents that can be used include pyridine, dibutyl ether, diacyl ether, dioxane, toluene, xylene, decalin, heptane and octane.

[0017] In 1970, Union Carbide Corporation of the United States also disclosed in U.S. Patent No. 3,497,500 a non-catalytic method for preparing caprolactam from caprolactone at high temperature and high pressure. The method emphasizes the importance of removing a portion of the carbon dioxide produced by the reaction from the reaction system. In short, according to the patent, in the reaction of caprolactone to caprolactam at high temperature and high pressure, the presence of an excess of carbon dioxide atmosphere in the reaction system is not conducive to obtaining a satisfactory caprolactam yield.

[0018] In 1972, Kanegafuchi, BOSEKI KABUSHIKI KAISHA of Japan disclosed a method for preparing caprolactam using copper chromite as a catalyst in U.S. Patent 3652549. The copper chromite catalyst is obtained by coprecipitation using copper nitrate and ammonium dichromate as raw materials and ammonia water as a precipitant. The technical features of the catalyst preparation process include that the precipitate generated by the coprecipitation reaction is filtered, dehydrated, low-temperature dried (75-80°C, 20h) and high-temperature decomposed, and then soaked in a dilute acetic acid solution. The catalyst precursor after soaking is filtered, washed with water, and dried (125°C, 12h) to become a catalyst. Before the catalyst is used in a fixed bed reactor, it needs to be pressed into tablets. Before the reaction, the catalyst needs to be reduced with hydrogen at 200°C. The atomic ratio of chromium to copper in the copper chromite catalyst is 0.1-5, preferably 0.1-3. The catalyst may also contain a third metal component (Ba, Ca, Mg, Sr, Al, Ga, Ti, V, Mn, Fe, Co, Ni, Zn, Mo, Ru, Rh, Pd, Ag, Cd, Sn, Pd, As, Bi, Sb). The atomic ratio of the third metal component to copper is 0.001-1, preferably 0.01-0.2. The raw material for preparing caprolactam conforms to the general formula X-(CH2)4-COY. Wherein, X=CHO, -CH(OR)(OR1), -COOH, -COONH4, -CONH2, or COR2; Y=OH, ONH4, NH2, or OR3. The reaction is carried out in a fixed bed reactor in a gas-solid phase, the reaction temperature ranges from 170-300°C, and the hydrogen partial pressure is 0.1-1.5atm. The feed also contains ammonia and water vapor, and the preferred usage ranges (molar ratio to the raw material) are 2-50 and 10-100 respectively. When dimethyl adipate is used as the raw material, the reaction results of the copper chromite catalyst containing a small amount of zinc are: the raw material conversion rate is 99%, and the caprolactam selectivity is 95%; the reaction results of the copper chromite catalyst containing a small amount of Mo are: the raw material conversion rate is 100%, and the caprolactam selectivity is 96%.

[0019] In 1975, Teijin Ltd. of Japan disclosed in US Pat. No. 3,888,845 a catalytic process for preparing caprolactam from C1-C4 alkyl esters of caprolactone or 6-hydroxycaproic acid. Specifically, the patent disclosed a process for producing caprolactam by gas-solid phase catalytic reaction using C1-C4 alkyl esters of caprolactone or 6-hydroxycaproic acid, hydrogen and ammonia as raw materials. The characteristics of the process are low reaction temperature and reaction pressure, high conversion rate of C1-C4 alkyl esters of caprolactone or 6-hydroxycaproic acid, and high selectivity of caprolactam. The solid catalyst used in the process consists of three parts: A, B and C: A is an oxide carrier selected from titanium oxide, aluminum oxide, silicon oxide and a composite of aluminum oxide and silicon oxide; B is the main metal component of the catalyst - copper; C is the trace metal component of the catalyst - nickel or chromium. The catalyst can be prepared by a deposition precipitation method. Among them, the carrier is preferably anatase titanium oxide, the optional range of the weight ratio of copper to the carrier is 0.5-200, preferably 5-100, and more preferably 10-70; the optional range of the atomic ratio of Ni(Cr) to Cu is 0.001-1, preferably 0.005-0.25. The gas-solid phase catalytic reaction of preparing caprolactam using C1-C4 alkyl esters of caprolactone or 6-hydroxycaproic acid can be carried out under the conditions of 200-320°C and 0.01-2atm, preferably under the conditions of 220-310°C and 0.1-1.2atm. The optional ranges of the amount of hydrogen and ammonia are 5-70 (H2 / ester molar ratio) and 1-50 (NH3 / ester molar ratio), respectively, and the preferred ranges are 10-50 (H2 / ester molar ratio) and 2-25 (NH3 / ester molar ratio), respectively. In addition, the process also emphasizes the importance of the hydrogen to ammonia molar ratio and the addition of water in the reactor feed. In general, the use of a suitable hydrogen to ammonia molar ratio is conducive to improving the selectivity of the reaction. Adding water to the feed of the reactor can not only reduce side reactions and improve the selectivity of caprolactam, but also slow down the deactivation rate of the catalyst. The optional range of the hydrogen to ammonia molar ratio is 0.2-30, and the preferred range is 0.5-15; the optional range of the water / ester molar ratio is 0-50, and the preferred range is 5-30. Under preferred conditions, when caprolactam is prepared from caprolactone, the conversion rate of caprolactone can reach up to 99%, and the caprolactam selectivity can reach up to 90%. The problem is that the catalyst is deactivated quickly by carbon deposition. However, the patent provides two methods for catalyst regeneration. One method is redox treatment, and the other method is steam treatment. The redox treatment is actually to regenerate the catalyst by burning carbon with molecular oxygen first, and then reduce the catalyst with hydrogen. The molecular oxygen burning carbon can be carried out in the temperature range of 100-800°C, preferably in the temperature range of 150-500°C. The charcoal burning time is 20 minutes to 20 hours; the hydrogen reduction after charcoal burning can be carried out in the temperature range of 170-350°C, preferably in the temperature range of 170-270°C.The steam treatment can be carried out at 100-500°C, preferably at 200-400°C. The steam treatment time is 20 minutes to 20 hours. The steam treatment can also be carried out in the presence of hydrogen, and it is best to reduce the catalyst with hydrogen after the steam treatment. The hydrogen reduction can be carried out in the temperature range of 170-350°C, preferably in the temperature range of 170-270°C.

[0020] In 2012, German patent DE102012006946A1 disclosed a new catalytic process for preparing caprolactam from D-glucose raw material via adipic acid and caprolactone. In the reaction of caprolactone to caprolactam, the patent used a Cu-Mo-Ti catalyst, and the raw materials for the reaction included ammonia and hydrogen in addition to caprolactone. The method can achieve a caprolactam yield of 80%.

[0021] In 2018, Chinese patent CN108774172A disclosed a catalytic method for preparing caprolactam and N-substituted caprolactam using caprolactone and ammonia (amine) as raw materials. Its technical feature is that the reactor is a fixed bed. The catalyst loaded in the fixed bed reactor is granular SO4 with a diameter of Φ = 4.0 to 6.0 mm. 2- / M X O Y Solid superacid. The patent emphasizes that the superacid catalyst used should always be under nitrogen protection. The reaction is carried out under normal pressure and nitrogen protection. The optional range of reaction temperature is 180-320°C, and the preferred range is 220-280°C; the molar ratio of caprolactone to ammonia (amine) is 1-1.5, and the preferred range is 1.1-1.3. The method also requires the use of a solvent. The solvent refers to water, benzene, toluene, xylene and cyclohexane. The amount of solvent added is 1-2 times the total weight of caprolactone and ammonia (amine).

[0022] In addition to the above patents, there are several journal articles on the research of caprolactone to caprolactam. For example:

[0023] In 1977, the open document Journal of the Chemical Society of Japan, 1977, (7), p. 1013-1017 reported the catalytic effect of a Cu-TiO2 catalyst on the gas phase ammonolysis of caprolactone to caprolactam. The ammonolysis reaction was carried out at normal pressure, and the products, in addition to caprolactam, included 6-hydroxycapronitrile, 6-hydroxycapronamide, adiponitrile and polymers. The article proved through a blank experiment that a simple solid acid catalyst resulted in the production of 6-hydroxycapronitrile, while a simple copper catalyst had almost no catalytic activity for the conversion of caprolactone. The Cu-TiO2 catalyst needs to be reduced with hydrogen before use, and hydrogen is required during the reaction. The activity of the catalyst decreases rapidly over time, presumably because the catalyst surface is covered with a polymer.

[0024] In 2001, the Japanese document Kobunshi Ronbunshu, 58 (12), 679-684 (2001) reported a study on the preparation of caprolactam by non-catalytic reaction of caprolactone and ammonia in supercritical water (T>374°C, P>22.1MPa). In this study, the reaction mechanism of preparing caprolactam from caprolactone was proposed, and 6-hydroxycaproamide was considered to be an intermediate in the reaction. 6-Hydroxycaproamide is dehydrated and ring-closed to form caprolactam. The article also studied the effects of reaction temperature, water density and ammonia concentration. The results showed that at 380°C and 38MPa (water density 0.5g / cm 3 ), the conversion rate of caprolactone and ammonia and the yield of caprolactam increase with the increase of reaction time. The yield of caprolactam can reach 79.2% when the reaction time is 60 minutes. However, the high temperature and high pressure conditions of supercritical water will increase equipment cost and operation difficulty, and also increase safety risks.

[0025] In 2022, the public document ChemSusChem, 2022, 15 (16) reported a reaction process for preparing caprolactam from 6-hydroxyhexanoic acid catalyzed by biological enzymes, which has little practical value.

[0026] From the above, it can be seen that the preparation of caprolactam from caprolactone can save the cyclohexanone oxime Beckmann rearrangement step in the existing benzene method caprolactam process, and can avoid the problems existing in the cyclohexanone ammoximation step, which is a new caprolactam production route with great application potential. However, at present, the technical route for preparing caprolactam from caprolactone raw materials has not received much attention. The existing process methods and catalysts for preparing caprolactam from caprolactone are mainly disclosed by patents and papers in the 1970s and before. In general, the reaction process methods proposed in the early stage are mainly divided into two types: non-catalytic method and catalytic method. Among them, the non-catalytic method requires high temperature and high pressure reaction conditions. Due to the problems of thermodynamic limitations and the generation of by-products, the caprolactam yield of the non-catalytic method is low. In contrast, the reaction conditions of the catalytic method are mild, which is not only favorable in terms of reaction thermodynamics, but also conducive to avoiding the occurrence of side reactions, and is also conducive to reducing equipment investment, reducing energy consumption and reducing production costs. Therefore, it is conducive to industrial application. However, the catalytic method requires a catalyst with high activity, high selectivity and strong anti-deactivation ability, and the existing catalysts cannot meet the needs of industrial application. Summary of the invention

[0027] The object of the present invention is to provide a preparation method capable of improving the stability of a Cu-Beta zeolite catalyst for preparing caprolactam by hydroamination of caprolactone.

[0028] The present invention provides a preparation method for improving the stability of a Cu-Beta zeolite catalyst for preparing caprolactam by hydroamination of caprolactone, specifically a preparation method for a catalyst using a dealuminated Beta zeolite modified with a chiseled cavity as a carrier and loading copper in the pores by an improved ammonia evaporation method. The chiseled cavity modification refers to a dealuminated Beta zeolite carrier modification technology that uses a weak organic base to control the desiliconization technology to enlarge the hydroxyl cavity generated by dealumination, thereby achieving the purpose of better accommodating and stabilizing nano and sub-nano copper particles.

[0029] After research, it was found that for the gas-solid phase catalytic reaction of caprolactone hydroamination to caprolactam, from the perspective of catalytic activity and selectivity, supported copper-based catalysts have the most promising prospects for industrial application. However, from the perspective of catalyst stability, the deactivation problem is the biggest challenge for the industrial application of supported copper-based catalysts. The deactivation of copper-based catalysts in the gas-solid phase catalytic reaction of caprolactone hydroamination to caprolactam is not only caused by carbon deposition. The sintering problem of highly dispersed copper particles is also an important cause of catalyst deactivation. People familiar with this field know that carbon deposition deactivation is a temporary deactivation of the catalyst, and its catalytic activity can generally be restored by various regeneration methods, thereby extending the service life of the catalyst. In contrast, sintering deactivation is generally a permanent deactivation of the catalyst, which has the greatest impact on the service life of the catalyst.

[0030] The main benefit of the method for preparing the Cu-Beta zeolite catalyst provided by the present invention is that it not only utilizes the dispersing and stabilizing effect of the hydroxyl nests of the dealuminated Beta zeolite on the loaded copper particles, but also controls the desiliconization technology through a weak organic base to enlarge the hydroxyl nests produced by dealumination, thereby increasing the contact area between the hydroxyl nests and the copper particles, further strengthening the stabilizing effect of the hydroxyl nests of the dealuminated Beta zeolite on the loaded copper particles, so that the copper-based catalyst can be used without adding anti-sintering additives such as chromium and nickel.

[0031] The catalyst preparation method provided by the present invention which can improve the stability of Cu-Beta zeolite catalyst has the following main technical features:

[0032] Firstly, the catalyst preparation method provided by the present invention can improve the stability of Cu-Beta zeolite catalyst, using the dealuminated Beta zeolite modified by chiseling as the carrier for loading copper.

[0033] The catalysts for preparing caprolactam from caprolactone by catalytic method, as recorded in the existing related patents and academic papers, are mainly non-loaded bulk copper chromite catalysts and copper catalysts (adding second metal components nickel or chromium) loaded with amorphous single oxide carriers (such as titanium oxide, aluminum oxide, silicon oxide) and binary composite oxide carriers (such as silicon oxide and aluminum oxide). People familiar with the art know that non-loaded copper chromite catalysts have a small specific surface area, and the exposed metal active sites are few, so the metal dosage is large and the catalytic efficiency is low; loading copper, copper-nickel and copper-chromium with amorphous oxide carriers (single oxide carriers and binary composite oxide carriers) can overcome the problems of non-loaded catalysts, but the loaded copper catalyst has the problem of easy sintering and deactivation, which is a huge challenge for industrial application. Adding chromium to the loaded copper catalyst to form a copper chromite phase can improve the anti-sintering ability of the loaded copper catalyst. However, chromium is a metal with limited use. Clinically, chromium and its compounds mainly infringe on human skin, respiratory and digestive systems, and even if the chromium content is very low, it will produce a strong toxic effect on the human body. Therefore, the catalysts added with chromium will encounter great troubles in the processes of preparation, use and harmless treatment of waste catalysts. Adding nickel to the supported copper catalyst can also improve the anti-sintering performance of copper. However, our research results show that for the reaction of preparing caprolactam from caprolactone, the introduction of a large amount of nickel into the supported copper catalyst will significantly reduce the ability of the catalyst to catalyze the gas-solid phase hydroamination of caprolactone into caprolactam. For example, under the same conditions, the copper-amorphous silicon oxide catalyst (10wt.%Cu) prepared with white carbon black silica (fumed silica) as a carrier, when a small amount of nickel (Ni:Cu=0.3) is added, its ability to catalyze the hydroamination of caprolactone into caprolactam has decreased by 15-20%. In the relevant patent (US3888845), although nickel is used as a preferred auxiliary agent for the supported copper catalyst, its addition amount is strictly limited to the range of Ni:Cu=0.001-1 (atomic ratio), preferably within the range of 0.005-0.25. Undoubtedly, the addition of a small amount of nickel can improve the sintering resistance of supported copper catalysts, but the effect of a small amount of nickel alone is not enough to properly solve the sintering deactivation problem of supported copper catalysts.

[0034] In fact, the sintering deactivation problem of supported copper catalysts is a common problem. Copper-based catalysts are widely used in alcohol dehydrogenation, carbonyl hydrogenation, ester hydrogenolysis, ammoniation, hydrocarbon hydrogenation, isomerization, and the hydrogenolysis of C-C and C-Si bonds, etc., because of their low price and environmental friendliness. The main reason for the easy sintering and growth of highly dispersed copper particles is that copper metal has a large ionic radius, a low melting point (1083 °C), and low Tammann and Hüttig temperatures. Supported copper catalysts can sinter at a temperature of 170 °C. Someone summarized the thermal stabilities of common metal catalysts and gave the following order: Ag < Cu < Pd < Fe < Ni < Co < Pt < Rh < Ru < Ir < Os < Re. It can be seen from this that the thermal stability of copper is lower than that of most common metal catalysts.

[0035] As mentioned above, the present invention prepares a supported copper-based catalyst using the chiseled and modified dealuminated Beta zeolite as a carrier. It not only utilizes the stabilizing effect of the hydroxyl nests of the dealuminated Beta zeolite on the supported copper particles, but also enlarges the hydroxyl nests generated by dealumination through the weak organic base-controlled desilication technology, increasing the contact surface between the hydroxyl nests and the copper particles, and further strengthening the stabilizing effect of the hydroxyl nests of the dealuminated Beta zeolite on the supported copper particles. Therefore, the copper-based catalyst Cu-Beta zeolite catalyst prepared by the method of the present invention has strong anti-sintering ability and can be used without adding anti-sintering aids such as chromium and nickel, and has high stability in the reaction of hydrogenation amination of ε-caprolactone to ε-caprolactam.

[0036] A large number of hydroxyl nest lattice defect sites in dealuminated Beta zeolite can be generated by removing framework aluminum from the Beta zeolite crystal using conventional acid treatment methods. When the Beta zeolite is subjected to acid dealumination treatment, for every framework aluminum removed, four Si-O-Al bonds need to be acid hydrolyzed ([Al-(OSi)4] - +4H2O = [Al(OH)4] - +4≡Si-OH, [Al(OH)4] - +4H + =Al 3+ +4H2O, and the total reaction equation is [Al-(OSi)4] - +4H + =Al 3+ +4≡Si-OH), generating a hydroxyl nest lattice defect site surrounded by four silanol groups (≡Si-OH).

[0037] The chiseling modification, i.e. the modification in which a weak organic alkali solution controls the desiliconization to enlarge the hydroxyl cavity of dealuminated Beta zeolite, is essentially a base-catalyzed hydrolytic desiliconization modification ([(OSi)3-O-SiOH]+3H2O=Si(OH)4+3≡Si-OH). Every time a silicon atom is released (in the form of orthosilicic acid (Si(OH)4)), that is, every time a silicon atom is "chiselled" from the wall of the hydroxyl cavity (in the form of Si(OH)4), three silicon hydroxyl groups (≡Si-OH) will be generated on the new wall of the hydroxyl cavity.

[0038] The main idea of ​​the present invention comes from the inventor's previous work. In the previous work, the inventor has conducted in-depth research on the physicochemical properties and catalytic functions of hydroxyl nest lattice defects in the MFI zeolite family (ZSM-5, B-ZSM-5, Silicalite-1 (S-1) and TS-1). The following public documents record some representative research work: Silicalite-1zeolite acidification by zinc modification and its catalytic properties for isobutane conversion, RSC Advances, 2018, 33(8), p.18663-1867; Pt supported on Znmodified silicalite-1zeolite as a catalyst for n-hexane aromatization, JOURNAL OF ENERGY CHEMISTRY,2018,(36),p.96-103; Operando Dual Beam FTIR Study of Hydroxyl Groups and Zn Species over Defective HZSM-5Zeolite Supported ZincCatalysts,Catalysts,2019,1(9),p.100; Effect of Zeolitic Hydroxyl Nests on theAcidity and Propane Aromatization Performance of Zinc Nitrate Impregnation-Modified HZSM-5 Zeolite, Industrial & Engineering Chemistry Research, 2020, 37(59), p.16146-16160. Liu Guodong. Study on the surface acidity and catalytic performance of ZnO modified nano-silicalite-1 zeolite [D]. Dalian University of Technology, 2020.; Lin Long. Characterization, modification and catalytic performance of defective ZSM-5 zeolite [D]. Dalian University of Technology, 2022.). In short, the above research results show that the silanol in the lattice defect of the zeolite hydroxyl nest is easy to form hydrogen bonds, and its chemical activity is much higher than that of the isolated silanol on the outer surface of the zeolite crystal.In addition, it is particularly worth mentioning that the inventors discovered the important phenomenon that zinc oxide preferentially locates in the hydroxyl nest lattice defect sites of zeolite in the study of zinc nitrate impregnation and preparation of zinc oxide modified catalysts for defective all-silicon zeolite S-1 and defective ZSM-5 zeolite. Moreover, the zinc oxide located in the hydroxyl nest lattice defect sites of zeolite is highly dispersed sub-nanometer zinc oxide species. These research experiences provide important scientific guidance for the present invention.

[0039] However, the present invention does not use defective MFI zeolite (e.g., defective all-silica zeolite S-1 and deborated B-ZSM-5 zeolite) as a carrier for preparing a loaded copper catalyst, but uses dealuminated Beta zeolite as a carrier for preparing a loaded copper catalyst. This is not because the hydroxyl nest lattice defect sites in the defective MFI molecular sieve (e.g., defective all-silica zeolite S-1 and deborated B-ZSM-5 zeolite) cannot disperse and stabilize copper particles, nor is it because the loaded copper catalyst prepared using the defective MFI molecular sieve (e.g., defective all-silica zeolite S-1 and deborated B-ZSM-5 zeolite) carrier is ineffective for catalyzing the gas-solid phase reaction of preparing caprolactam from caprolactone. This is because the cylindrical pores of the MFI family zeolites are ten-membered rings. When the loading amount of metallic copper is slightly larger, the effective size of the pores will be significantly reduced, which is not conducive to the intrapore diffusion of the reactant caprolactone (seven-membered ring), nor is it conducive to the formation and intrapore diffusion of the caprolactam product, which is also a seven-membered ring. Therefore, it is not conducive to the preparation of catalysts with high activity, high selectivity and strong resistance to deactivation.

[0040] People familiar with the art know that as a crystalline porous catalytic material, Beta zeolite and MFI zeolite have similar advantages such as: (1) Both are high-silicon zeolites, so they have high thermal stability and hydrothermal stability, good regeneration performance, and can be repeatedly regenerated and reused after being made into catalysts; (2) Both are cylindrical channels, and both have a three-dimensional cross-channel system, which can provide a networked channel for molecular diffusion, so the channel diffusivity is good and the anti-clogging ability is strong, which is conducive to the catalyst to maintain long-term activity and stability during continuous reaction. In addition, compared with MFI zeolite, Beta zeolite is unique. On the one hand, the three-dimensional cylindrical channels of Beta zeolite are all large pores with twelve-membered rings. In the three-dimensional pore system of Beta zeolite, there is a group of "Z"-shaped curved pores parallel to the

[001] direction and with an elliptical cross-section, with a pore size of 0.56nm×0.65nm; there are also two groups of straight pores parallel to the

[100] and

[010] directions, with elliptical cross-sections and pore sizes of 0.66nm×0.77nm. In contrast, the three-dimensional cylindrical pores of MFI zeolite are all mesopores with ten-membered rings. In the pore system of MFI zeolite, there is a group of straight pores parallel to the (100) crystal plane and with a nearly circular cross-section (pore size of 0.53nm×0.56nm) and two groups of "Z"-shaped curved pores parallel to the (010) crystal plane, with opposite folds and elliptical cross-sections (pore size of 0.51nm×0.55nm). It is conceivable that the pore system of Beta zeolite is more suitable for the diffusion of the reactant caprolactone (seven-membered ring) in the pores due to its relatively loose macropore characteristics, and is also more suitable for the formation and diffusion of the caprolactam product, which is also a seven-membered ring, and is therefore more conducive to the preparation of catalysts with high activity, high selectivity and strong resistance to deactivation. In fact, Beta zeolite is the only zeolite molecular sieve among industrial zeolite catalytic materials that has the advantages of a high silicon-aluminum oxide molar ratio, a three-dimensional cross-pore system, and all pores are twelve-membered ring macropores.

[0041] On the other hand, the framework aluminum of Beta zeolite can be easily removed by acid treatment, thus producing a high density of hydroxyl pit defect sites on the crystal framework. This feature is rare in industrial zeolite catalytic materials and is unmatched by MFI zeolite. When Beta zeolite is subjected to acid dealumination treatment, four Si-O-Al bonds ([Al-(OSi)4] - +4H2O=[Al(OH)4] - +4≡Si-OH, [Al(OH)4] - +4H + =Al 3+ +4H2O, the overall reaction equation is [Al-(OSi)4] - +4H + =Al 3++4≡Si-OH), producing a hydroxyl nest lattice defect site surrounded by four silanol groups (≡Si-OH). In MFI zeolite, the hydroxyl nest lattice defect sites of defective all-silicon zeolite S-1 are randomly formed during the hydrothermal synthesis of S-1 zeolite in an alkaline medium, and their number and distribution are poorly controllable; although the framework aluminum content of ZSM-5 zeolite can be adjusted in a wide range, the lower limit of its silicon-aluminum molar ratio (Si / Al) can reach about 10, and the upper limit can reach all-silicon zeolite, namely Silicalite-1 (S-1). However, it is difficult to completely remove the framework aluminum of ZSM-5 zeolite. Therefore, in the research on the preparation of titanium atom hybridized ZSM-5 zeolite by post-synthesis method, the general practice is to first try to synthesize boron-containing ZSM-5 zeolite (B-ZSM-5), and then remove boron from B-ZSM-5 zeolite to obtain a ZSM-5 zeolite carrier with a high density of hydroxyl nest defects on the framework.

[0042] In summary, the present invention does not use MFI zeolite with hydroxyl nest lattice defect sites (for example, defective all-silicon zeolite S-1 and deborated B-ZSM-5 zeolite) as a carrier for preparing copper-based catalysts, but selects Beta zeolite with hydroxyl nest lattice defect sites as a carrier for preparing copper-based catalysts. The main reason is that for the purpose of the present invention, Beta zeolite combines the three advantages of high silicon-aluminum oxide molar ratio framework, three-dimensional twelve-membered ring cross-channel system and easy and complete removal of framework aluminum, which is an unmatched material advantage. In addition, Beta zeolite is a catalytic material that has been industrially synthesized earlier, that is, it can be obtained in large quantities through commercial sales, and it can also be easily prepared by hydrothermal synthesis.

[0043] The reason why the dealuminated Beta zeolite carrier is subjected to the chiseling modification before use is to enlarge the hydroxyl pits generated by dealumination so as to better accommodate and stabilize nano and sub-nano copper particles. The chiseling modification refers to the supplementary modification of the dealuminated Beta zeolite carrier with an aqueous solution of a small molecule weak organic base, and the controlled removal of 1-2 silicon atoms from the pit wall of the hydroxyl pit, thereby expanding the original small hydroxyl pit with only one skeleton atom defect (acid dealumination) to a larger hydroxyl pit with 2-3 skeleton atom defects.

[0044] This is the revelation obtained after a lot of preliminary exploration and research. Much larger than the ionic radius of aluminum Therefore, the smaller hydroxyl cavity produced by dealumination of Beta zeolite can only accommodate one copper atom at most. Obviously, the active silanol in the hydroxyl cavity of Beta zeolite only interacts closely with one copper atom, which is bound to limit its ability to disperse and stabilize metallic copper particles.

[0045] If 1-2 silicon atoms can be controllably removed from the hydroxyl pit wall of dealuminated Beta zeolite, thereby expanding the small hydroxyl pit with only one skeleton atom defect (acid dealumination) to a larger hydroxyl pit with 2-3 skeleton atom defects, the dispersion and stabilization ability of the hydroxyl pit for metallic copper particles can be enhanced. According to this idea, the inventors have carried out a lot of exploratory research work using weaker alkaline organic base aqueous solutions. Compared with alkali metal hydroxide solutions (inorganic strong bases) and quaternary ammonium base solutions (organic strong bases), weaker alkalinity organic bases have weaker desiliconization ability and can only desiliconize in small amounts, so it is easy to achieve the purpose of controllable desiliconization. At the same time, weaker alkalinity organic bases have weaker desiliconization ability, so it is also easy to achieve selective desiliconization, that is, mainly desiliconize from the weakest part of the Beta zeolite skeleton - the hydroxyl pit defect site. Research has found that aqueous solutions of small molecule fatty amines (methylamine, ethylamine, propylamine, tert-butylamine, isopropylamine, n-butylamine, diethylamine, ethylenediamine, isobutylamine, triethylamine) and small molecule alcoholamines (ethanolamine, diethanolamine, triethanolamine, isopropanolamine, diisopropanolamine) have a controllable desiliconization effect when in contact with dealuminated Beta zeolite, and have a good "chisel-hole" modification effect on the hydroxyl holes of Beta zeolite. Compared with general organic bases, small molecule fatty amines and alcoholamines have the advantages of good water solubility and small dosage. In order not to make the specification of the present invention look too complicated, the present invention only takes ethanolamine as an example to chisel-hole modify the dealuminated Beta zeolite when performing chisel-hole modification on the dealuminated Beta zeolite. The chiseling modification is essentially a base-catalyzed hydrolytic desiliconization modification ([(OSi)3-O-SiOH]+3H2O=Si(OH)4+3≡Si-OH). Every time a silicon atom is released (in the form of orthosilicic acid (Si(OH)4)), that is, every time a silicon atom is "chiselled" from the pit wall of the hydroxyl pit (in the form of Si(OH)4)), three silicon hydroxyl groups (≡Si-OH) will be generated on the new pit wall of the hydroxyl pit.

[0046] Secondly, the catalyst preparation method provided by the present invention which can improve the stability of Cu-Beta zeolite catalyst is realized by loading copper with improved ammonia distillation method.

[0047] The core of the improved ammonia evaporation copper loading technology is to impregnate the zeolite carrier with an equal volume of copper-ammine complex solution. In this process, the capillary condensation of the pores of the zeolite carrier is used to absorb most of the copper-ammine complex solution into the pores of the zeolite, so that the copper hydroxide generated during the ammonia evaporation process is directly deposited in the pores of the Beta zeolite. Therefore, in the subsequent drying, roasting and hydrogen reduction treatment processes, the copper hydroxide can be first converted into copper oxide in the pores of the zeolite, and then further converted into sub-nano and nano particles of metallic copper. The sub-nano and nano particles of metallic copper can be directly captured by the hydroxyl nest lattice defect sites that are mainly present in the pores of the zeolite and have been treated with a hollow hole during the formation process, so as to be dispersed and stabilized in a timely and more effective manner.

[0048] People familiar with the art know that ammonia evaporation is one of the most commonly used methods for preparing copper-based catalysts. Ube Industries Ltd. (US4 440 873 (1984), EP0 064 241B1 (1985)) first proposed the use of ammonia evaporation to prepare Cu / SiO2 catalysts for the purpose of gas-solid phase hydrogenation of dimethyl oxalate to produce ethylene glycol and glycolate. The earliest proposed ammonia evaporation method is as follows: the first step is to prepare a copper-ammine complex solution. First, a soluble copper-containing compound is dissolved in water to obtain an aqueous solution containing copper ions, and then an appropriate amount of concentrated ammonia water is added to the aqueous solution containing copper ions to make the pH value greater than 10, for example, to make the pH value reach 10-12. Thus, a dark blue transparent solution containing a copper-ammine complex can be obtained; the second step is to use silica sol as a precursor of the SiO2 carrier and mix it with the copper-ammine complex. That is, silica sol is added to the dark blue transparent solution containing the copper-ammine complex and stirred thoroughly to mix them evenly. This stirring mixing process can be carried out under normal pressure and pressurized conditions, from room temperature to 150°C; the third step is ammonia evaporation treatment. That is, the mixture containing the copper ammonia complex is subjected to ammonia evaporation treatment to obtain a solid catalyst precursor. The ammonia evaporation treatment can be carried out under pressurized and reduced pressure, and the preferred temperature range is 60-90°C; the fourth step is the pretreatment of the solid catalyst precursor. This step refers to the pretreatment of the solid catalyst precursor before hydrogen reduction, including drying and water washing. In addition, pre-calcination treatment can also be selected. The temperature range of the pre-calcination treatment is 400-800°C, preferably 500-750°C; the fifth step is hydrogen reduction treatment. The pretreated solid catalyst precursor is subjected to hydrogen reduction treatment. The hydrogen reduction time is 1-15h, and the reduction temperature range is 150-500°C, preferably 200-400°C.

[0049] In US Pat. No. 4,440,873, examples of soluble copper-containing compounds that can be used to prepare copper-ammine complex solutions are given, including copper nitrate, copper sulfate, copper oxalate, copper chloride and copper acetate, and copper nitrate is pointed out as a preferred option. In Example 1, the preparation of Cu / SiO2 catalyst by ammonia evaporation is described as follows: (1) 19.0 g of copper nitrate (Cu(NO3)2.3H2O) is dissolved in 200 ml of water to obtain an aqueous solution containing copper ions, and then 60 ml of concentrated ammonia solution is added thereto, and the pH value is adjusted to 11-12, thereby obtaining a dark blue solution containing copper-ammine complex; (2) 66.6 g of silica sol (30 wt.% SiO2) is added to the copper-ammine complex solution and stirred at room temperature for several hours; (3) The reaction mixture of step (2) is subjected to ammonia evaporation treatment by heating. Ammonia is evaporated until most of the water is also evaporated to obtain a solid product; (4) The solid product is dried at 120°C for 12 hours. The dried product was fully washed with water and then dried. The drying condition was 140°C for 14 hours; (5) The dried product was subjected to hydrogen reduction treatment. The reduction condition was 350°C for 2-3 hours. The prepared Cu / SiO2 catalyst contained about 20 wt.% copper.

[0050] From the above, it can be seen that the earliest proposed process for preparing Cu / SiO2 catalyst by ammonia evaporation has the following characteristics: On the one hand, the amorphous silica carrier is not prefabricated, but is generated in situ during the ammonia evaporation process using silica sol as a precursor. Specifically, during the ammonia evaporation process, the silica sol is converted into silica gel. At the same time, the copper ammonia complex loses ammonia to generate copper hydroxide precipitate, which is deposited on the surface of the silica gel. This process has dynamic characteristics. That is, the silica gel particles continue to grow after being generated, and at the same time, the copper hydroxide precipitate is also continuously generated. While the silica gel particles grow, the copper hydroxide precipitate is deposited and reacted on its surface, resulting in a loading state in which silica gel and copper hydroxide are mixed layer by layer. Later, researchers in this field pointed out (J.Catal.257(2008)172–180) that this ammonia evaporation method is essentially a homogeneous deposition-precipitation method, and the prepared Cu / SiO2 catalyst is a layered copper silicate. On the other hand, a diluted copper ammonia complex solution is prepared and used. The volume of this copper-ammine complex solution is greatly in excess relative to the liquid holding capacity (pore volume) of the silica gel finally generated. The water solvent therein needs to be removed by post-treatment operations such as filtration or evaporation, and the mechanism of copper loading and dispersion on the silica carrier is deposition and precipitation, that is, the silica gel particles grow while copper hydroxide precipitates and reacts on its surface, and a uniform loading state is achieved by the layer-by-layer mixing of silica gel and copper hydroxide. It is conceivable that if the silica carrier is not generated during the ammonia evaporation process but is prefabricated, then the use of this diluted and excessive volume (the solution volume is greatly excessive relative to the total pore volume of the silica carrier) copper-ammine complex solution for ammonia evaporation will inevitably lead to a large amount of copper hydroxide being deposited on the outer surface of the carrier particles, resulting in the uneven result that less copper is loaded in the carrier pores and more copper is loaded outside the carrier pores.

[0051] After that, some scholars prepared amorphous oxide carrier-supported copper-based catalysts for the purpose of gas-solid phase hydrogenation of dimethyl oxalate to ethylene glycol according to the earliest proposed ammonia evaporation method. For example, in the public literature J. Catal. 257 (2008) 172-180 and Appl. Catal. A: Gen. 458 (2013) 82-89, there are reports of related research, and the amorphous oxide carriers involved are silicon dioxide and a binary composite of silicon dioxide and titanium dioxide. When silicon dioxide is used as a carrier, silica sol (Ludox AS-40) is used as a precursor of the carrier. When a binary composite of silicon dioxide and titanium dioxide is used as a carrier, silica sol (JN30, Qingdao Haiyang Chem. Co., Ltd.) and titanium dioxide sol are used as precursors of the carrier. After the ammonia evaporation is completed (the pH value of the slurry drops to 6-7), the amorphous oxide-supported copper hydroxide solid product is obtained by filtration.

[0052] Some scholars have improved the ammonia evaporation method proposed earlier when preparing Cu / SiO2 catalysts for gas-solid phase hydrogenation of dimethyl oxalate. Among them, in the open literature J.Am.Chem.Soc.2012,134,13922-13925 and J.Catal.297(2013)142-150, researchers reported the ammonia evaporation hydrothermal (AEH) method. This method is actually to transfer the ammonia evaporation product (slurry containing copper hydroxide / silica gel precipitate, pH=6-7) of the traditional ammonia evaporation method (the earliest proposed ammonia evaporation method) to a high-pressure synthesis reactor for hydrothermal treatment at 190-210℃ for 12h, and then perform conventional filtration, washing, drying, roasting and hydrogen reduction treatment on the solid product. In other words, this method is not to improve the ammonia evaporation method itself, but to insert a hydrothermal post-treatment step for the product of the ammonia evaporation method before the conventional post-treatment. It should be emphasized that the operation of the ammonia evaporation hydrothermal method before the hydrothermal post-treatment is the same as that of the traditional ammonia evaporation method. The silica carrier is generated in situ using silica sol as a precursor, and the water solvent of the diluted and excess copper ammonia complex solution is finally removed by filtration; in the public document J.Phys.Chem.C 2015,119,13758-13766, scholars added urea as a precipitation aid to the solution when preparing the copper ammonia complex solution. The other methods are the same as those of the traditional ammonia evaporation method. The silica carrier is generated in situ using silica sol (Ludox AS-40, 40wt.% SiO2) as a precursor, and the water solvent of the diluted and excess copper ammonia complex solution is finally removed by filtration. In the open literature Natural Gas Chemical Industry (C1 Chemistry and Chemical Industry), 2013, 38(3):43-47, Natural Gas Chemical Industry (C1 Chemistry and Chemical Industry), 2014, 39(5):31-34 and Journal of Shenyang University of Chemical Technology, 2016, 30(3):212-216., the researchers used prefabricated JN-25 alkaline silica gel (primary particle size 10nm, Qingdao Ocean Chemical Co., Ltd.) as the carrier of the Cu / SiO2 catalyst prepared by the ammonia evaporation method. In order to achieve a uniform deposition and precipitation effect, a certain amount of silica sol is also added as a precursor for the in situ generation of the silica gel carrier. In order to overcome the problem caused by the reduced amount of silica sol when using prefabricated JN-25 alkaline silica gel as a carrier for Cu / SiO2 catalyst, the researchers also tried to add hexadecyltrimethylammonium bromide (CTAB) surfactant to the prepared copper ammine complex aqueous solution to disperse the silica sol and produce mesopores in the in-situ generated silica gel.The other methods are the same as the traditional ammonia evaporation method; in the open literature RSC Adv., 2015, 5, 29040-29047 and Applied Catalysis A: General 509 (2016) 66-74, the researchers used prefabricated titanium dioxide (P25, Degussa Co., Ltd) as the carrier of the Cu / TiO2 catalyst prepared by the ammonia evaporation method, and the other methods are the same as the traditional ammonia evaporation method. It should be noted that the P25 type TiO2 carrier is a low specific surface carrier with underdeveloped capillaries. Therefore, in the prepared Cu / TiO2 catalyst, there is no uniform deposition and precipitation effect, that is, the loaded copper hydroxide mainly exists on the outer surface of the titanium dioxide carrier. The calcined sample is analyzed by X-ray diffraction, and there are obvious diffraction characteristic peaks of the CuO phase at 2θ = 35.5°, 38.7° and 48.7°, indicating that the dispersion of its hydrogen reduction product - metallic copper is poor.

[0053] In addition, it is worth mentioning that in the open document Applied Catalysis A, General 539 (2017) 59–69, the researchers used prefabricated ordered mesoporous silica (OMS) as the carrier of the Cu / OMS catalyst prepared by the ammonia evaporation method. In order to reduce the destructive effect of the alkalinity of the copper-ammine complex solution on the ordered mesopores of the prefabricated silica carrier, the researchers also appropriately reduced the concentration of ammonia water in the prepared copper-ammine complex solution (the researchers regarded it as an improvement on the ammonia evaporation method). In addition to the above two points, there is no other difference between the improved ammonia evaporation method described in this study and the traditional ammonia evaporation method. After the ammonia evaporation is completed (the pH value of the slurry drops to 6-7), the water solvent of the diluted and excess volume of the copper-ammine complex solution is finally removed by filtration to obtain a solid product loaded with copper hydroxide. The research results show that the ordered mesoporous structure of the prefabricated silica carrier used in this study has been largely destroyed after being loaded with metallic copper by the ammonia evaporation method, and a large amount of layered copper silicate exists in the catalyst, indicating that the prefabricated silica carrier used was dissolved in large quantities during the contact with the copper-ammine complex solution and turned into silica sol, which produced a uniform deposition and precipitation effect with copper hydroxide during the ammonia evaporation process; in the open document Journal of Catalysis 280 (2011) 77–88, the researchers also used prefabricated mesoporous silica (HMS) as the carrier of the Cu / HMS catalyst prepared by the ammonia evaporation method. In addition, the researchers also added a water-soluble nickel salt (nickel nitrate) to the prepared copper-ammine complex aqueous solution, so that the prepared copper-based catalyst contained metallic nickel ( CuxNi / HMS). The ammonia evaporation method used in this study is no different from the traditional ammonia evaporation method except that a prefabricated mesoporous silica carrier is used and a water-soluble nickel salt (nickel nitrate) is added to the prepared copper-ammine complex aqueous solution so that the prepared copper-based catalyst contains a metallic nickel additive. The ammonia evaporation operation is carried out at 90°C. After the ammonia evaporation is completed (the pH value of the slurry drops to 7-8), the diluted and excess volume of the copper-ammine complex solution The water solvent is finally removed by filtration to obtain a solid product loaded with copper hydroxide and nickel hydroxide. Similarly, in this study, after the ordered mesopores of HMS silica were loaded with metallic copper and nickel by the ammonia evaporation method, the ordered mesoporous structure in them had been mostly destroyed (the specific surface area decreased by more than 50%). Moreover, the XRD characterization results show that the prepared supported catalyst sample has characteristic diffraction peaks of the metal oxide phase before hydrogen reduction (calcined at 450°C for 4h), and characteristic diffraction peaks of the metal phase after hydrogen reduction, indicating that the metallic copper and nickel are unevenly loaded on the HMS carrier and have poor dispersion.

[0054] According to the results of literature survey, except for a recent open article in Science (Science10.1126 / science.adj1962(2023).) reporting the use of ammonia evaporation to prepare a supported copper catalyst on a dealuminated Beta zeolite carrier for the purpose of gas-solid phase hydrogenation of dimethyl oxalate, no other research work on the use of ammonia evaporation to prepare supported metal catalysts on zeolite carriers has been found at home and abroad so far. It should be noted that the relevant research work recently published in Science used the traditional ammonia evaporation method to prepare a supported copper catalyst on a dealuminated Beta zeolite carrier. The specific method is as follows: the first step is to dissolve 0.23g Cu(NO3)2·3H2O in 100ml ammonia solution (containing 0.75g NH3·H2O) and stir at room temperature for 10min to prepare a copper-ammine complex aqueous solution; the second step is to add 1.94g dealuminated Beta zeolite carrier (Beta-deAl) to the copper-ammine complex solution and evaporate ammonia under vigorous stirring. The temperature of ammonia evaporation is 80℃, and the time of ammonia evaporation is 6h; in the third step, after the ammonia evaporation is completed, the water solvent of the diluted and excessive volume of the copper-ammine complex solution is finally removed by filtration; in the fourth step, the solid product is dried at 100℃ overnight and calcined at 400℃ for 3h to obtain the catalyst; in the fifth step, in order to catalyze the hydrogenation reaction of dimethyl oxalate with the catalyst, it is reduced with hydrogen at 400℃ for 3h. It is not difficult to see that in this study, except that the catalyst carrier is prefabricated dealuminated Beta zeolite (obtained by acid dealumination treatment of Al-Beta zeolite matrix with Si / Al=13 with 13MHNO3 solution at 80℃ for 12h), the other methods are the same as the traditional ammonia evaporation method. In the prepared copper-ammine complex solution, the copper ion concentration is very dilute (only about 9.5mmol / L); when the catalyst is prepared by the ammonia evaporation method, the initial liquid-solid ratio is as high as about 51.5 (ml / g), that is, the volume of the copper-ammine complex solution is greatly excessive to the zeolite carrier. The results show that although the prepared dealuminated Beta zeolite-loaded copper catalyst Cu / Beta-deAl has a very low copper content (about 3wt.% Cu), the specific surface area loss is as high as 15% (due to the excessive copper-ammine complex solution (NH3 / Cu molar ratio 22.5) causing a large amount of dissolution and desiliconization of the dealuminated Beta zeolite, which destroys the skeleton structure), and its XRD pattern still has obvious characteristic diffraction peaks of metallic copper (2θ=43.3°). Transmission electron microscopy studies have shown that the copper in the fresh catalyst is mainly loaded on the outer surface of the dealuminated Beta zeolite, and the particle size is relatively large (the use of a diluted and excessive copper-ammine complex solution causes excessive deposition of copper hydroxide outside the zeolite pores during the ammonia evaporation process), and requires methanol vapor post-treatment to be redispersed through the reverse Ostwald ripening process in order to transfer it into the zeolite pores.This research work fully demonstrates that when using dealuminated Beta zeolite as a carrier to prepare molecular sieve-loaded copper catalysts through copper-ammine complexes, the traditional ammonia evaporation method reported in the literature for silica carriers cannot be used. Otherwise, the following problems will occur: (1) Excess copper-ammine complex solution will deposit a large amount of copper outside the zeolite pores during the ammonia evaporation process; (2) Dealuminated Beta zeolite will undergo a desiliconization reaction (ammonia evaporation temperature 80°C) in an excess of copper-ammine complex solution (pH = 10-12), destroying the crystal structure.

[0055] The present invention therefore proposes to use an improved ammonia distillation process different from the known practices to meet the need for supporting metallic copper in the pores of a zeolite support, especially a high-silica zeolite support that is easily desiliconized, such as dealuminated Beta zeolite.

[0056] In addition, the main feature of the present invention is that the provided Cu-Beta zeolite catalyst is used for the purpose of preparing caprolactam from caprolactone in a gas-solid phase reaction state. So far, neither the disclosed invention patents nor other published documents have involved this application purpose of the Cu-Beta zeolite catalyst. The reaction system is unique. This is mainly because the reaction of preparing caprolactam from caprolactone in a gas-solid phase reaction state involves the use of water vapor, hydrogen and ammonia. For copper-based catalysts, this is a harsh application scenario.

[0057] As mentioned above, in the catalytic methods for preparing caprolactam from caprolactone recorded in the existing relevant patents and academic papers, the catalysts used are mainly two types, one is a non-supported bulk copper chromite catalyst, and the other is a copper catalyst (with a second metal component of nickel or chromium added) supported by a single oxide carrier (such as titanium oxide, aluminum oxide, silicon oxide) or a binary composite oxide carrier (such as silicon oxide and aluminum oxide). The single oxide and the binary composite oxide used as the carrier in the supported copper catalyst (with a second metal component of nickel or chromium added) are both amorphous.

[0058] The gas-solid phase reaction state is a suitable way to convert caprolactone into caprolactam by the approach of catalytic method. As mentioned above, the catalytic methods for preparing caprolactam from caprolactone disclosed by Kanegafuchi, Bosekikabushiki Kaisha in British Patent GB1109540 (1966) and U.S. Patent 3652549 (1972), and Teijin Co., Ltd. in U.S. Patent 3888845 (1975) all adopt the gas-solid phase reaction state.

[0059] As is known to all, the gas-solid phase reaction state is a common form of heterogeneous catalysis, specifically referring to the catalytic reaction in which the reactants contact the solid catalyst in the form of gas. In the field of heterogeneous catalysis, the gas-solid phase reaction is sometimes referred to as the gas-phase reaction. The gas-solid phase reaction state is a reaction form with mild reaction conditions, high mass transfer and heat transfer efficiency, and very simple operation. For the gas-solid phase reaction, the process of the reactants being converted into products on the catalyst consists of seven elementary steps: (1) external diffusion of reactants. In this step, the reactants pass through the adsorption film on the surface of the solid catalyst and contact the outer surface of the catalyst; (2) internal diffusion of reactants. In this step, the reactants diffuse into the pores through the pores on the surface of the solid catalyst to approach the catalytic active centers in the pores; (3) chemical adsorption of reactants on the catalytic active centers. In this step, the reactant molecules are activated and become activated molecules; (4) surface reaction. In this step, the reactants are converted into adsorbed product forms on the catalyst active centers; (5) product desorption. In this step, the adsorbed product detaches from the catalytic active centers; (6) internal diffusion of products. This step is the process of the product molecules moving from the pores to the outer surface of the catalyst after they have separated from the catalytic active centers; (7) External diffusion of the product. In this step, the product molecules leave the pores on the outer surface of the solid catalyst, pass through the adsorption film on the surface of the solid catalyst, separate from the solid catalyst particles, and become reaction products.

[0060] The Cu-Beta catalyst provided by the present invention is suitable for the gas-solid phase hydrogenation catalytic reaction conditions of preparing caprolactam from caprolactone recorded in existing relevant patents and academic papers. As mentioned above, in 1966, Kanegafuchi, BOSEKI KABUSHIKI KAISHA first disclosed a gas-solid phase catalytic method for preparing caprolactam in British patent GB1109540, specifically, firstly vaporizing caprolactone and a certain amount of water, then mixing with ammonia and hydrogen, and the mixed gas is catalytically reacted by copper chromite catalyst at 120-350°C and normal pressure; in 1972, Kanegafuchi, BOSEKI KABUSHIKI KAISHA disclosed a method for preparing caprolactam again in U.S. Patent 3652549, which is also a gas-solid phase catalytic method. Specifically, the method uses a fixed bed reactor, the reaction temperature range is 170-300°C, and the hydrogen partial pressure is 0.1-1.5atm. There are also ammonia and water vapor in the feed, and the preferred range of their dosage (molar ratio to the raw material) is 2-50 and 10-100 respectively; in 1975, Teijin Co., Ltd. of Japan disclosed a method for preparing caprolactam in US Pat. No. 3,888,845, which is also a gas-solid phase catalytic method. Specifically, its gas-solid phase catalytic reaction can be carried out under the conditions of 200-320°C and 0.01-2atm, preferably under the conditions of 220-310°C and 0.1-1.2atm. The optional range of hydrogen and ammonia dosage is 5-70 (H2 / ester molar ratio) and 1-50 (NH3 / ester molar ratio), respectively, and the preferred range is 10-50 (H2 / ester molar ratio) and 2-25 (NH3 / ester molar ratio). In addition, the process also emphasizes the importance of the hydrogen to ammonia molar ratio and the addition of water in the reactor feed. In general, the use of an appropriate hydrogen to ammonia molar ratio is conducive to improving the selectivity of the reaction. Adding water to the reactor feed can not only reduce side reactions and improve caprolactam selectivity, but also slow down the deactivation rate of the catalyst. The optional range of the hydrogen to ammonia molar ratio is 0.2-30, preferably 0.5-15; the optional range of the water to ester molar ratio is 0-50, preferably 5-30.

[0061] In summary, according to the relevant patents and academic papers, the gas-solid phase hydroamination catalytic reaction of preparing caprolactam from caprolactone, in addition to the caprolactone raw material, the reactor feed also includes water, ammonia and hydrogen. 10 O2) and the molecular formula of the caprolactam product (C6H 11NO) It is not difficult to see that ammonia and hydrogen are also reaction raw materials, and water vapor becomes water vapor after vaporization and is a diluent gas. The optional range of reaction temperature is 120-350°C, the optional range of reaction pressure is 0.01-2atm, and the optional ranges of ammonia-ester, hydrogen-ester and water-ester molar ratios are 1-50, 5-70 and 0-100 respectively; the preferred range of reaction temperature is 220-300°C, the preferred range of reaction pressure is 0.1-1.2atm, and the preferred ranges of ammonia-ester, hydrogen-ester and water-ester molar ratios are 2-25, 10-50 and 5-30 respectively. In order to facilitate people in this field to better understand the implementation effect of the present invention, in the present invention, the catalytic performance of the provided Cu-Beta zeolite catalyst in the gas-solid phase hydrogenation reaction of caprolactone to caprolactam is evaluated, and the reaction conditions adopted are within the above range.

[0062] The technical solution of the present invention:

[0063] A preparation method for improving the stability of Cu-Beta zeolite catalyst for preparing caprolactam from caprolactone, comprising the following steps:

[0064] The first step is to prepare the dealuminated Beta zeolite carrier

[0065] Engineers familiar with the art can prepare a dealuminated Beta zeolite carrier from a Beta zeolite matrix according to the requirements of the present invention, combined with their own work experience and reference to conventional acid dealumination methods in relevant literature. The requirements of the present invention are as follows:

[0066] (1) Select Beta zeolite matrix

[0067] The Beta zeolite matrix refers to a silicon-aluminum zeolite. The present invention has no restrictions on the crystal size of the Beta zeolite matrix, nor on the production process of the Beta zeolite matrix. However, in order to facilitate the implementation of the present invention, the Beta zeolite matrix has the following restrictions: 1) There are no impurity crystals in the Beta zeolite matrix; 2) The crystallization of the Beta zeolite matrix is ​​good; 3) The molar ratio of silicon-aluminum oxide (the molar ratio of SiO2 to Al2O3) of the Beta zeolite matrix is ​​appropriate.

[0068] Wherein, whether there are impurity crystals in the Beta zeolite matrix can be checked and confirmed by X-ray polycrystalline powder diffraction (XRD) method. People familiar with the art know that the silicon aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) of the Beta zeolite produced by the hydrothermal synthesis method is usually between 10-200 (US3 308 069 (1967)). In the Beta zeolite product with a lower silicon aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3), there may generally be impurity crystals of mordenite (MOR), while in the Beta zeolite with a higher silicon aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3), there may generally be impurity crystals of ZSM-5 zeolite. By sampling and performing XRD analysis on the Beta zeolite matrix and comparing the XRD pattern of the sample with the standard diffraction cards of Beta zeolite, MOR zeolite and ZSM-5 zeolite, it can be determined whether there are characteristic peaks of MOR zeolite and ZSM-5 zeolite impurities in the XRD pattern of the sample, thereby knowing whether the Beta zeolite matrix is ​​a pure Beta zeolite phase.

[0069] Theoretically, the crystallization of the Beta zeolite matrix can also be analyzed by XRD and measured by the relative crystallinity index. However, in view of the fact that the XRD relative crystallinity index needs to be obtained by comparing the sum of the intensities of the medium-intensity characteristic diffraction peak of the Beta zeolite matrix located between 2θ=7.6-8° and the highest intensity characteristic diffraction peak located at 2θ=22-23° with the sum of the intensities of the corresponding diffraction peaks of the reference sample (standard Beta zeolite with a crystallinity of 100%), and the reference sample has no unified definition; and in view of the fact that the intensity of the medium-intensity characteristic diffraction peak of the Beta zeolite located between 2θ=7.6-8° and the highest intensity characteristic diffraction peak located at 2θ=22-23° is greatly affected by the process and conditions of post-processing such as calcination. Therefore, using the XRD relative crystallinity index to determine whether the crystallization of the purchased or synthesized Beta zeolite matrix is ​​good has poor universality. For this reason, the present invention recommends using the specific surface area index of the Beta zeolite matrix to measure whether the crystallization of the purchased or synthesized Beta zeolite matrix meets the requirements. According to our statistical results of the specific surface area data of Beta zeolite reported in the literature, the BET specific surface area of ​​well-crystallized Beta zeolite produced by hydrothermal synthesis is generally not less than 450 m 2 / g. Engineers familiar with the art can use conventional nitrogen physical adsorption method to first measure the nitrogen adsorption isotherm data of Beta zeolite matrix, and then calculate its BET specific surface area value according to the BET model. In short, the present invention requires that the BET specific surface area value of the Beta zeolite matrix used is ≥450m 2 / g, indicating that its crystallization is good.

[0070] The molar ratio of silicon to aluminum oxide (the molar ratio of SiO2 to Al2O3) is a key indicator of the Beta zeolite matrix. This is because, on the one hand, the lower the molar ratio of silicon to aluminum oxide (the molar ratio of SiO2 to Al2O3) of the Beta zeolite matrix, that is, the higher the content of framework aluminum, the more hydroxyl nest lattice defect sites that the dealuminated Beta zeolite carrier can use to disperse and stabilize nano and subnano copper particles; on the other hand, pure phase Beta zeolite with a very low molar ratio of silicon to aluminum oxide (the molar ratio of SiO2 to Al2O3) is difficult to synthesize using a hydrothermal method. Moreover, after the Beta zeolite matrix with a very low molar ratio of silicon to aluminum oxide (the molar ratio of SiO2 to Al2O3) is made into a dealuminated Beta zeolite carrier by the acid dealumination method, the framework has poor thermal stability, and the crystallinity will be lost in the subsequent calcination step of preparing the Cu-Beta zeolite catalyst, resulting in poor performance of the catalyst. Therefore, the molar ratio of silicon-aluminium oxide (molar ratio of SiO2 to Al2O3) of the Beta zeolite matrix required by the present invention is in the range of 10-200, preferably in the range of 20-100, and more preferably in the range of 25-60. The molar ratio of silicon-aluminium oxide (molar ratio of SiO2 to Al2O3) of the Beta zeolite matrix can be analyzed by conventional chemical analysis (titration), or by X-ray fluorescence spectroscopy (XRF) or inductively coupled plasma emission spectroscopy (ICP). The present invention recommends the use of the simple and fast XRF method.

[0071] The Beta zeolite matrix that meets the requirements of the present invention can be obtained from commercial sources or synthesized by itself. Engineers familiar with the art can also synthesize the Beta zeolite matrix that meets the requirements of the present invention based on their own experience and other literature reports.If the Beta zeolite matrix is ​​synthesized by itself, the methods reported in the following invention patents and public documents can be selected: US3308069 (1967), EP187522A2 (1986), US4847055 (1989), CN1086792A (application date 1993.9.20), CN1108213A (application date 1994.3.11), CN1108214A (application date 1994.3.11), CN1154341A (application date 1996.1.11), CN1154242A (application date 1996.1.9), CN1154342A (application date 1996.1.11), CN1268545A (application date 1999.3.30), CN1 133 497C (application date March 30, 1999), CN1108 275C (application date September 10, 1999), CN1 100 004C (application date May 19, 2000), CN1 335 258A (application date February 28, 2001), CN1 116 227C (application date March 12, 2001), CN101 205 072B (application date December 18, 2006), Chem. Comm., 1996, 625; J. Mater. Chem., 1998, 8 (9), 2137-2145; Microporous and Mesoporous Materials 21 (1998) 305-313; Applied Catalysis A-GENERAL,166(1998),97–103;Microporous and Mesoporous Materials 48(2001)23-29;Microporous and Mesoporous Materials 56(2002)1–10.;Journal of Molecular Catalysis A:Chemical252(2006)76–84;Microporous and Mesoporous Materials 94(2006)1–8; J.Mater.Sci.41(2006)1861-1864; Cryst.Res.Technol.44,No.4,379-385(2009)DOI10.1002 / crat.200800474; Microporous and Mesoporous Materials 143(2011)97-103;RSC Adv.2019,9,3653-3660.

[0072] (2) Preparation of dealuminated Beta zeolite carrier

[0073] As mentioned above, a dealuminated Beta zeolite carrier can be prepared on the basis of a Beta zeolite matrix by a conventional acid dealumination method. The present invention requires that the silicon-aluminum oxide molar ratio (the molar ratio of SiO2 to Al2O3) of the dealuminated Beta zeolite carrier be as high as possible, that is, the skeleton aluminum of the Beta zeolite matrix should be completely removed as much as possible. The dealuminated Beta zeolite carrier that meets the requirements of the present invention has a silicon-aluminum oxide molar ratio (the molar ratio of SiO2 to Al2O3) in a suitable range of ≧700, a preferred range of ≧800, and a more preferred range of ≧900. Because the silicon-aluminum oxide molar ratio (the molar ratio of SiO2 to Al2O3) of the dealuminated Beta zeolite is very high and the aluminum content is very low, the inductively coupled plasma emission spectroscopy (ICP) method or the atomic absorption (AA) method is required to accurately determine its silicon-aluminum oxide molar ratio (the molar ratio of SiO2 to Al2O3). The present invention recommends the use of the ICP method.

[0074] When the Beta zeolite matrix is ​​subjected to acid dealumination treatment, efforts should be made to remove all of its framework aluminum. The harm of too much framework aluminum remaining on the dealumination Beta zeolite carrier is that the strong acidity of the framework aluminum will accelerate the coking and deactivation of the Cu-Beta zeolite catalyst and reduce the selectivity of the catalyst for the main product of caprolactam.

[0075] Although the framework aluminum of Beta zeolite is easy to remove, so that a dealuminized Beta zeolite carrier that meets the requirements of the present invention can be prepared on the basis of Beta zeolite matrix by high-temperature steam dealumination, EDTA and other complexing agent dealumination, organic acid solution dealumination, inorganic acid (concentrated hydrochloric acid, concentrated nitric acid) solution dealumination, or a dealumination method formed by any combination of the above different methods, but considering the production cost of the dealuminized Beta zeolite carrier, the complexity of the process and the difficulty of treating the waste liquid generated by dealumination, the present invention recommends using a concentrated nitric acid aqueous solution dealumination method to prepare a dealuminized Beta zeolite carrier that meets the requirements of the present invention.

[0076] Engineers familiar with the art can, based on their own experience or referring to the specific practices disclosed in the following documents, carry out acid dealumination treatment on the Beta zeolite matrix with concentrated nitric acid aqueous solution to prepare the dealumination Beta zeolite carrier that meets the requirements of the present invention: Chemical Communications, 1998, 1: 87-88; Micropor. Mesopor. Mater., 1999, 31: 163-173; Micropor. Mesopor. Mater., 2001, 49: 103–109; Micropor. Mesopor. Mater., 2008, 110: 480–487; Micropor. Mesopor. Mater., 2012, 163: 122-130; ACS Catalysis, 2014, 4(8): 2801-2810.

[0077] When a Beta zeolite matrix is ​​subjected to acid dealumination with concentrated nitric acid aqueous solution to prepare a dealuminated Beta zeolite carrier, the concentration of the nitric acid aqueous solution, the ratio of the acid solution to the zeolite (liquid-to-solid ratio), and the temperature and time of the acid treatment are all important factors affecting the degree of acid dealumination of the Beta zeolite matrix. The influence of the above-mentioned factors on the dealumination of the Beta zeolite matrix is ​​ultimately reflected in the residual aluminum content of the dealuminated Beta zeolite carrier. In addition, the pretreatment of the Beta zeolite matrix will also affect the degree of acid dealumination and the residual aluminum content of the dealuminated Beta zeolite carrier. However, if a dealuminated Beta zeolite carrier with a silicon-aluminum oxide molar ratio (SiO2 to Al2O3 molar ratio) that meets the requirements cannot be obtained after one dealumination, the silicon-aluminum oxide molar ratio (SiO2 to Al2O3 molar ratio) of the dealuminated Beta zeolite can be made to meet the requirements of the present invention by secondary or even multiple additional dealuminations. The present invention recommends using 13M concentrated nitric acid as the dealuminated acid solution and using the acid solution according to a liquid-to-solid ratio (ml / g) of 20:1. Under this premise, the dealumination reaction is carried out at 95°C for 20 hours. After the dealumination reaction is completed, the solid product is first recovered by solid-liquid separation, and then the solid product is washed with water until the pH value is neutral, and then dried at 80-200°C for 3-24 hours, and calcined at 500°C-600°C for 3-8 hours to obtain the dealumination Beta zeolite. After the Beta zeolite matrix is ​​dealumination, a large number of hydroxyl nest lattice defect sites are generated, and its water and moisture absorption capacity is stronger, so it should be sealed and stored for future use.

[0078] In the second step, the hydroxyl holes of the dealuminated Beta zeolite carrier are modified by chiseling holes with an aqueous solution of ethanolamine.

[0079] The chiseling modification of the hydroxyl nest is carried out by a conventional aqueous solution immersion method. The chiseling modification is essentially a base-catalyzed hydrolysis reaction modification ([(OSi)3-O-SiOH]+3H2O=Si(OH)4+3≡Si-OH). Every time a silicon atom is released (in the form of orthosilicic acid (Si(OH)4)), that is, every time a silicon atom is "chiseled" off the pit wall of the hydroxyl nest (in the form of Si(OH)4), three silicon hydroxyl groups (≡SiOH) will be generated on the new pit wall of the hydroxyl nest.

[0080] When the dealuminated Beta zeolite carrier is impregnated with ethanolamine solution (weak organic base) for cavity modification, the concentration of the ethanolamine aqueous solution, the ratio of the ethanolamine solution to the dealuminated Beta zeolite, i.e., the liquid-solid ratio (ml / g), and the impregnation temperature and time are the main factors affecting the controllable desiliconization modification of the hydroxyl cavity of the dealuminated Beta zeolite by the ethanolamine solution. The present invention provides the following ranges of values ​​for these four parameters:

[0081] The suitable range of ethanolamine solution concentration is 0.01M-0.4M, preferably 0.02M-0.3M; more preferably 0.03M-0.16M;

[0082] The ratio of the ethanolamine solution to the dealuminated Beta zeolite carrier, i.e., the liquid-to-solid ratio (ml / g), is suitably in the range of 1:1-100:1, preferably in the range of 2:1-50:1; more preferably in the range of 3:1-20:1;

[0083] The suitable range of the immersion temperature is 20°C-100°C; the preferred range is 30°C-90°C; the more preferred range is 40°C-80°C;

[0084] The suitable range of the immersion time is 0.1h-24h; the preferred range is 0.5h-10h; the more preferred range is 1-5h.

[0085] Engineers familiar with the art can refer to the impregnation process commonly used in the preparation of multiphase catalysts, and use ethanolamine solution to impregnate the dealuminated Beta zeolite carrier, so as to achieve the purpose of chiseling the hydroxyl pits of the dealuminated Beta zeolite carrier. The details will not be repeated. Similarly, after the chiseling modification, the liquid-solid mixture should be post-processed according to common sense, mainly including conventional liquid-solid separation, water washing (to neutral pH), drying and calcination. Among them, the conditions for drying and calcination can refer to the drying and calcination conditions of the dealuminated Beta zeolite carrier in the first step (preparation of dealuminated Beta zeolite carrier) of the implementation scheme of the present invention. No more details.

[0086] However, it should be pointed out that for dealuminated Beta zeolite carriers with different numbers of hydroxyl pits prepared from Beta zeolite matrix with different molar ratios of silicon and aluminum oxides (molar ratio of SiO2 to Al2O3), the key to using an aqueous solution of ethanolamine to perform controllable chiseling modification of the hydroxyl pits is to correctly select the modification conditions composed of four parameters (ethanolamine solution concentration, liquid-to-solid ratio (ml / g), immersion temperature and time). It is not difficult to understand that the modification conditions composed of the lower limit values ​​of the above four parameters have the weakest desiliconization effect and are suitable for chiseling modification of dealuminated Beta zeolite carriers with a small number of hydroxyl pits; the modification conditions composed of the upper limit values ​​of the above four parameters have the strongest desiliconization effect and can be used for chiseling modification of dealuminated Beta zeolite carriers with a large number of hydroxyl pits; and the modification conditions composed of other different values ​​of the above four parameters within the specified range will produce different desiliconization effects between the weakest and the strongest. Likewise, the above explanation of the present invention is intended to provide principled guidance to engineers in the field. For different dealuminated Beta zeolite carriers, the ethanolamine solution impregnation treatment conditions that achieve a moderate degree of cavitation modification are best determined through experiments.

[0087] The third step is to prepare a Cu-Beta zeolite catalyst by loading copper in the pores of the dealuminated Beta zeolite carrier modified by the improved ammonia evaporation method.

[0088] As mentioned above, the core of the improved ammonia evaporation method of the present invention is to use a copper-ammonia complex solution to impregnate a zeolite carrier in equal volume. In this process, the capillary condensation of the zeolite pores is relied on to absorb most of the complex solution into the pores, so as to achieve the purpose of depositing copper hydroxide and loading metallic copper in the pores. The specific method is as follows:

[0089] (1) Preparation of dilute ammonia basic solution and saturated solution of copper ammonia complex: 4.4 g industrial ammonia (containing 25-28 wt. %) and 100 ml deionized water were used to prepare a dilute ammonia basic solution with a pH value of 11-12, which was sealed and stored for later use; 2+ ) and ammonia molecules in a molar ratio of 1:4, using copper nitrate trihydrate (Cu(NO3)2·3H2O) as a soluble copper-containing compound to react with industrial ammonia to synthesize a copper-ammine complex; finally, dissolving the copper-ammine complex with a dilute ammonia base solution at room temperature to prepare a saturated solution of the copper-ammine complex, which is sealed and stored for later use. The concentration of copper-ammine ions in the saturated solution of the copper-ammine complex is about 0.4 mol / L (0.4 M), and the color is dark blue, clear and transparent.

[0090] It should be noted that, although it is recorded in U.S. Pat. No. 4,440,873 (1984) that soluble copper-containing compounds that can be used to prepare copper ammonia complex solutions include copper nitrate, copper sulfate, copper oxalate, copper chloride and copper acetate, considering that sulfate and chloride ions will increase the burden of subsequent water washing, and oxalate and acetate have corrosive problems, the present invention recommends the use of copper nitrate (Cu(NO3)2·3H2O).

[0091] (2) Impregnation of the zeolite carrier with an equal volume of copper-ammine complex solution: First, the saturated water absorption rate of the zeolite carrier is measured, and the amount of copper-ammine complex solution used for impregnation of the zeolite carrier with an equal volume is calculated. Then, the concentration of the required copper-ammine complex solution is calculated according to the copper loading of the Cu-Beta zeolite catalyst to be prepared. When the calculated concentration is equal to 0.4M, the zeolite carrier is directly impregnated with an equal volume of the saturated solution of the copper-ammine complex; when the calculated concentration is lower than 0.4M, the saturated solution of the copper-ammine complex is appropriately diluted with a dilute ammonia basic solution, and then the zeolite carrier is impregnated with an equal volume; when the calculated value is higher than 0.4M, the concentration of the copper-ammine complex solution for a single equal volume impregnation should be recalculated according to multiple equal volume impregnations, and the dilute ammonia basic solution and the saturated solution of the copper-ammine complex are used to prepare a copper-ammine complex solution of the required concentration for each equal volume impregnation. After each impregnation, the zeolite carrier is subjected to ammonia evaporation.

[0092] The equal volume impregnation is carried out at room temperature in a closed container. In this process, the zeolite carrier absorbs the copper ammine complex solution into the zeolite pores by capillary condensation, so that the copper ammine complex ions contact and interact with the hydroxyl nest lattice defect sites in the pores. The suitable range of the equal volume impregnation time is 0.5-24h, the preferred range of the equal volume impregnation time is 1-12h, and the more preferred range of the equal volume impregnation time is 2-6h;

[0093] (3) Ammonia evaporation treatment: The ammonia evaporation process can be carried out under normal pressure or under reduced pressure. The suitable range of ammonia evaporation temperature and time is 50-100°C and 0.5-48h, the preferred range of ammonia evaporation temperature and time is 60-90°C and 1-24h, and the more preferred range of ammonia evaporation temperature and time is 65-85°C and 3-12h. During the ammonia evaporation process, the copper ammonia complex decomposes to generate ammonia gas and copper hydroxide, the former is absorbed by water, and the latter is deposited in the zeolite pores and hydroxyl nest lattice defect sites.

[0094] (4) Dehydration and drying treatment after ammonia evaporation: The suitable ranges of drying temperature and time are 100-200°C and 0.5-48h, respectively. The preferred ranges of drying temperature and time are 110-170°C and 1-24h, respectively. The more preferred ranges of drying temperature and time are 120-150°C and 3-12h, respectively.

[0095] (5) Calcination after ammonia evaporation: This step is used to convert the copper hydroxide precipitates deposited in the zeolite pores and hydroxyl nest lattice defect sites into nano and sub-nano copper oxide particles, thereby obtaining a catalyst precursor. The calcination is carried out in an air atmosphere, and the appropriate ranges of calcination temperature and time are 350-650°C and 0.5-24h, respectively, the preferred ranges of calcination temperature and time are 400-600°C and 1-12h, respectively, and the more preferred ranges of calcination temperature and time are 450-550°C and 2-6h, respectively;

[0096] (6) Hydrogen reduction treatment of catalyst precursor: to obtain Cu-Beta zeolite finished catalyst. The suitable ranges of reduction temperature, time and hydrogen flow rate (expressed as hydrogen volume space velocity, defined as the volume of hydrogen passing through a unit volume of catalyst per unit time, calculated as ideal gas) are 280-600°C, 0.5-20h and 1-2000h, respectively. -1 , the preferred ranges are 300-550℃, 1-15h and 10-1500h respectively -1 , the more preferred ranges are 350-500°C, 2-8h and 20-1000h respectively -1 .

[0097] The Cu-Beta zeolite catalyst obtained by the preparation method is used to catalyze the gas-solid phase hydroamination of caprolactone to produce caprolactam.

[0098] As mentioned above, one of the main features of the present invention is that the provided Cu-Beta zeolite catalyst is used for catalyzing the gas-solid phase hydroamination reaction of caprolactone to produce caprolactam.

[0099] However, the present invention does not limit the specific method of preparing caprolactam by gas-solid phase hydroamination of caprolactone. Engineers familiar with the art can refer to the methods disclosed in relevant patents and other literature materials to implement the gas-solid phase hydroamination of caprolactone. According to relevant patents and other literature materials, the present invention sorts out the following range of conditions for gas-solid phase hydroamination of caprolactone for reference: the suitable range of reaction temperature is 120-350°C, the suitable range of reaction pressure is 0.01-2atm, the suitable range of feed space velocity (WHSV) of caprolactone is 0.1-5h -1 The suitable ranges of the molar ratios of ammonia-ester, hydrogen-ester and water-ester are 1-50, 5-70 and 0-100 respectively; the preferred range of the reaction temperature is 220-300°C, the preferred range of the reaction pressure is 0.1-1.2 atm, and the preferred range of the feed space velocity (WHSV) of caprolactone is 0.2-2h -1 The preferred ranges of the molar ratios of amino-ester, hydrogen-ester and water-ester are 2-25, 10-50 and 5-30, respectively.

[0100] In order to facilitate the explanation of the implementation effect of the catalyst and the preparation method of the present invention and to avoid unnecessary complexity, a small fixed-bed reactor in the laboratory is taken as an example to introduce a typical method for preparing caprolactam by gas-solid hydrogenation reaction of caprolactone on a Cu-Beta zeolite catalyst as follows: The small fixed-bed reactor adopts an upper feeding and lower discharging operation mode, and the Cu-Beta zeolite catalyst is installed in the constant temperature zone of the reactor. The upper and lower spaces of the catalyst bed are filled with inert porcelain balls. Among them, the upper porcelain ball area of ​​the reactor serves as the vaporization and preheating zone of the raw materials. For convenience, caprolactone, water and ammonia can be prepared into a mixed feed, which is transported by a micro-metering pump, and the hydrogen feed is controlled by a mass flowmeter. The reaction is carried out under fixed conditions: reaction temperature 270°C, reaction pressure 1atm, caprolactone feed space velocity (WHSV) 0.6h -1 The molar ratios of amino-ester, hydrogen-ester and water-ester are 6, 50 and 30 respectively.

[0101] Beneficial effects of the present invention:

[0102] First, the present invention uses an improved ammonia evaporation method to prepare a Cu-Beta zeolite catalyst on a dealuminated Beta zeolite carrier modified by chiseling holes, so that the copper-ammonia complex can react to deposit copper hydroxide mainly in the zeolite pores during the ammonia evaporation process. After calcination and hydrogen reduction treatment, the copper hydroxide deposited in the zeolite pores can directly form highly dispersed nano and sub-nano copper particles at the hydroxyl pore lattice defect sites in the pores, and the latter obtains anti-sintering ability by interacting with the hydroxyl pores. Secondly, the present invention utilizes the dispersing and stabilizing effect of the dealuminated Beta zeolite hydroxyl pores on the loaded copper particles, and also uses a weak organic base to control the desiliconization technology to enlarge the hydroxyl pores produced by dealumination, increase the contact area between the hydroxyl pores and the copper particles, and further strengthen the stabilizing effect of the dealuminated Beta zeolite hydroxyl pores on the loaded copper particles. These measures enable the Cu-Beta zeolite catalyst to be used without adding anti-sintering aids such as chromium and nickel. The Cu-Beta zeolite catalyst prepared by the method of the present invention can be used without adding anti-sintering aids such as chromium and nickel. In addition, the core of the improved ammonia distillation method used in the present invention is to impregnate the dealuminated Beta zeolite carrier with an equal volume of copper ammonia complex solution. Since the amount of copper ammonia complex solution used is small, it is beneficial to inhibit the destruction of the dealuminated Beta zeolite skeleton by the silicon dissolving effect of the copper ammonia complex alkaline solution (pH=10-12), thereby facilitating the dispersion and stabilization effect of the dealuminated Beta zeolite hydroxyl nests on highly dispersed nano and sub-nano copper particles, and is beneficial to the preparation of a Cu-Beta zeolite catalyst with high activity, high selectivity and high stability. Finally, the present invention uses the Cu-Beta zeolite catalyst for the purpose of gas-solid phase hydroamination of caprolactone, which will greatly reduce the industrialization difficulty of the technical route of using caprolactone to prepare caprolactam. BRIEF DESCRIPTION OF THE DRAWINGS

[0103] Figure 1 It is the infrared spectrum of the hydroxyl region of the dealuminated Beta zeolite carrier (Beta24c) produced by acid dealumination of a Beta zeolite matrix having a silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) of 24, and the infrared spectrum of the hydroxyl region of the chiseled-hole modified dealuminated Beta zeolite carrier (Beta24C) obtained by controlled desiliconization of Beta24c with an aqueous solution of a weak organic base ethanolamine.

[0104] Figure 2 It is the XRD diagram of the dealuminated Beta zeolite carrier Beta24C modified by the chiseling, and the XRD diagram of the Cu-Beta zeolite catalyst (Cu3-Beta24C-1) with a copper content of 3wt.% prepared by using Beta24C as the carrier and the improved ammonia distillation method.

[0105] Figure 3 This is a high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) photograph of the Cu3-Beta24C-1 catalyst.

[0106] Figure 4 This is a high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) photograph of a Cu3-Beta24C-1 catalyst sample calcined at high temperature (550℃×3h).

[0107] Figure 5 It is the XRD diagram of the dealuminated Beta zeolite carrier Beta24C modified by the chiseling, and the XRD diagram of the Cu-Beta zeolite catalyst (Cu3-Beta24C-CE1) with a copper content of 3wt.% prepared by using Beta24C as the carrier and the traditional ammonia distillation method. DETAILED DESCRIPTION

[0108] The implementation effect of the present invention can be evaluated by characterizing the physicochemical properties of the prepared Cu-Beta zeolite catalyst and detecting its catalytic performance in the gas-solid phase hydroamination reaction of caprolactone to produce caprolactam.

[0109] In characterizing the physicochemical properties of Cu-Beta zeolite catalysts, the focus can be on characterizing the damage of the crystal structure, the occupation of hydroxyl nests, the high dispersion of the loaded metallic copper, and the resistance to sintering of copper particles.

[0110] Among them, the damage of the Beta zeolite crystal structure can be characterized by the X-ray polycrystalline powder diffraction (XRD) method. If the ammonia evaporation treatment leads to significant damage to the Beta zeolite crystal structure, the intensity of the characteristic diffraction peak at 2θ=22-23° in the XRD diagram of the catalyst will be significantly reduced. If the dealuminated Beta zeolite carrier modified by the chiseling is used as a reference sample, the relative degree of reduction of the zeolite carrier in the Cu-Beta zeolite catalyst can also be estimated.

[0111] The occupancy of the hydroxyl cavity in the Cu-Beta zeolite catalyst can be determined by using Fourier transform infrared spectroscopy (FT-IR) to obtain the hydroxyl vibration infrared spectrum of the catalyst and comparing it with the hydroxyl vibration infrared spectrum of the dealuminated Beta zeolite carrier modified by the cavity chiseling to make a qualitative judgment. The more nano and sub-nano copper particles are located in the hydroxyl cavity, the stronger the infrared characteristic band of the hydroxyl cavity of the catalyst (located at 3300-3600cm -1 The intensity of the broadened absorption band between them will be weaker, and vice versa.

[0112] In addition, the high dispersion of the metal copper loaded in the Cu-Beta zeolite catalyst can be observed by transmission electron microscopy (TEM), and the anti-sintering of the copper particles can be concluded by calcination treatment combined with TEM observation. It can also be judged by the attenuation of the catalytic activity (caprolactam yield) of the catalyst in the gas-solid phase hydroamination of caprolactone to produce caprolactam.

[0113] As for the catalytic performance of Cu-Beta zeolite catalyst in the gas-solid phase hydroamination of caprolactone to produce caprolactam, it can be evaluated using a small laboratory fixed bed reactor. Its operation method and reaction conditions are as described above. The reaction product composition is analyzed by gas chromatography (GC). The GC uses an FID detector and is equipped with an OV-1701 chromatographic column. The conversion rate of caprolactone and the selectivity of caprolactam are calculated by the internal standard method (the internal standard is 1,4-dioxane). The product of the caprolactone conversion rate and the caprolactam selectivity is used to obtain the caprolactam yield data as an evaluation index of the catalyst activity.

[0114] The present invention will be further described below by way of examples, but the present invention is not limited by these examples.

[0115] Embodiment 1: This embodiment is used to illustrate that the Cu-Beta zeolite catalyst prepared by loading copper in the pores with the improved ammonia distillation method using the dealuminated Beta zeolite modified by the chiseled cavity as the carrier according to the present invention can not only better maintain the crystal structure of the dealuminated Beta zeolite carrier, so that the loaded metallic copper is mainly located in the hydroxyl cavity lattice defect position in the zeolite pores in the form of highly dispersed nanometer and sub-nanometer copper particles, but also the active silanol groups in the hydroxyl cavity are more closely combined with the highly dispersed nanometer and sub-nanometer copper particles, which better improves the anti-sintering ability of the catalyst, thereby improving the stability of the catalyst. The prepared Cu-Beta zeolite catalyst is suitable as a catalyst for the gas-solid phase hydroamination of caprolactone to produce caprolactam.

[0116] First, a Cu-Beta zeolite catalyst is prepared according to the embodiment provided by the present invention:

[0117] The first step is to prepare the dealuminated Beta zeolite carrier

[0118] (1) According to the hydrothermal crystallization method provided in U.S. Pat. No. 3,308,069 (1967), a Beta zeolite matrix with a silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) of 25 was synthesized as a raw material for preparing a dealuminated Beta zeolite carrier. After conventional filtration, washing, drying (110°C, 12h) and calcination to remove the template agent (540°C, 6h), the synthesized Beta zeolite matrix was observed to have a grain size of less than 100 nanometers by TEM, belonging to nano Beta zeolite; no impurities were found in it by XRD inspection, and its BET specific surface area was calculated to be about 550 m by nitrogen physical adsorption data. 2 / g, and the molar ratio of silicon aluminum oxide (the molar ratio of SiO2 to Al2O3) measured by XRF method is about 24, which meets the technical requirements of the Beta zeolite matrix of the present invention, and is sealed and stored for future use.

[0119] (2) The Beta zeolite matrix was dealuminated with concentrated nitric acid to prepare a dealuminated Beta zeolite carrier.

[0120] First, a concentrated nitric acid solution with a molar concentration of 13M was prepared. Then, according to a liquid-solid ratio of 20:1 (ml / g), 30g of the Beta zeolite matrix that had been dried and calcined as described above was added to a three-necked flask containing 600ml of 13M concentrated nitric acid solution under stirring for dealumination. The dealumination temperature was 95°C and the dealumination time was 20h. During the dealumination reaction, the three-necked flask was kept in a reflux state. After the dealumination reaction was completed, the feed liquid was cooled to room temperature and the solid product was filtered and recovered. Then, conventional water washing, drying (overnight at 110°C) and calcination (550°C, 3h) were used to obtain a dealumination Beta zeolite carrier. The molar ratio of silicon aluminum oxide (molar ratio of SiO2 to Al2O3) of the dealumination Beta zeolite carrier was measured by ICP method to be 985 (>900). Suitable as a carrier of the catalyst of the present invention (codenamed Beta24c, where the lowercase "c" represents the hydroxyl pits produced by dealumination in Beta zeolite). Keep sealed for future use to avoid moisture absorption.

[0121] In the second step, the hydroxyl holes of the dealuminated Beta zeolite carrier are modified by chiseling holes with an aqueous solution of ethanolamine.

[0122] The chiseling hole modification adopts the atmospheric pressure impregnation method. First, prepare 44mmol / L (44mM) ethanolamine aqueous solution as the chiseling hole modification liquid. Then, add 20g of dealuminated Beta zeolite carrier into 120ml of ethanolamine modification liquid according to the liquid-solid ratio of 6:1 (ml / g). Heat the reaction mass to 40°C under stirring, and react the reaction mass under continuous stirring at this temperature for 1h. During this period, the dealuminated Beta zeolite carrier undergoes a weak base-catalyzed hydrolysis desiliconization reaction ([(OSi)3-O-SiOH]+3H2O=Si(OH)4+3≡Si-OH) in the weak alkaline solution of ethanolamine. For each silicon atom (in the form of orthosilicic acid (Si(OH)4)) released, three silicon hydroxyls (≡Si-OH) will be generated on the new side wall of the hydroxyl hole. After 1 hour of reaction, the reaction materials were filtered to recover the solid product, and then the solid product was repeatedly washed with deionized water until neutral, and then dried (overnight at 110°C) and calcined (550°C, 3h) to obtain the dealuminated Beta zeolite modified by the chiseling. It was sealed and stored for later use. According to the weight loss estimation, the average number of skeleton silicon atoms (in terms of SiO2) chiseled out at the hydroxyl nest lattice defect sites of the dealuminated Beta zeolite carrier is 1.2 silicon atoms, indicating that the chiseling modification is a moderate desiliconization carried out under controllable conditions, which meets the chiseling modification requirements for the dealuminated Beta zeolite carrier. The chiseled carrier is code-named Beta24C (the capital "C" indicates that the chiseling modification increases the volume of the hydroxyl nest in the dealuminated Beta zeolite). The Fourier transform infrared spectroscopy (FT-IR) method was used to obtain the hydroxyl vibration infrared spectrum of the dealuminated Beta zeolite carrier (Beta24c) and its chiseled modified sample (Beta24C), as shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the hydroxyl vibration infrared spectrum of the dealuminated Beta zeolite carrier has undergone significant changes after the dimple modification, indicating that the dimple modification does occur at the hydroxyl dimple lattice defect site of the dealuminated Beta zeolite.

[0123] The third step is to prepare Cu-Beta zeolite catalyst by loading copper in the pores of dealuminated Beta zeolite modified by chiseling holes using an improved ammonia distillation method.

[0124] (1) Prepare a dilute ammonia basic solution, and synthesize a copper ammonia complex with copper nitrate trihydrate (Cu(NO3)2'3H2O), and then prepare a saturated solution of the copper ammonia complex at room temperature. The pH value of the dilute ammonia basic solution is 11-12, and industrial ammonia (containing 25-28 wt. % NH3) is prepared in the ratio of 100 ml of deionized water to 4.4 g of industrial ammonia; the copper ammonia complex is obtained by reacting Cu(NO3)2·3H2O with industrial ammonia in the ratio of 1:4 of copper ions to ammonia molecules; the saturated solution of the copper ammonia complex is obtained by dissolving the copper ammonia complex with the dilute ammonia basic solution, and contains about 0.4 M of the copper ammonia complex.

[0125] (2) A zeolite carrier is impregnated with an equal volume of a copper-ammine complex solution to prepare a Cu-Beta zeolite catalyst with a copper loading of 3 wt.%. First, 5 g of a dealuminated Beta zeolite carrier (Beta24C) modified by a hole chiseling and sealed after calcination is taken, and titrated with deionized water until all samples are evenly soaked but no free liquid water appears. A total of 6.25 ml of deionized water is consumed, and the water absorption rate of the dealuminated Beta zeolite (Beta24C) modified by a hole chiseling is calculated to be 1.25 ml / g. According to the feed amount of 10 g of the carrier, a total of 12.5 ml of copper-ammine complex solution is required. According to the copper loading of 3 wt.%, the concentration of the required copper-ammine complex solution is about 0.38 M. That is, the calculated value of the required copper-ammine complex solution concentration is very close to the concentration of the saturated copper-ammine complex solution (0.4 M). Therefore, 10 g of the dealuminated Beta zeolite support (Beta24C) modified by the chiseling process was directly impregnated with 12.5 ml of the saturated solution of the copper-ammine complex in equal volume. The equal volume impregnation was carried out at room temperature for 4 hours.

[0126] (3) Equal volume of impregnated material is treated with ammonia evaporation at normal pressure. The ammonia evaporation temperature is 80°C and the ammonia evaporation time is 10 hours. In this process, the copper-ammonia complex that enters the zeolite pores due to capillary condensation gradually precipitates in the zeolite pores in the form of copper hydroxide due to the loss of ammonia.

[0127] (4) Dehydrate and dry the material after ammonia evaporation at a drying temperature of 110°C and a drying time of 12 hours.

[0128] (5) The dried material is calcined at a temperature of 500°C for 3 hours. After calcination, the copper hydroxide deposited in the zeolite pores is converted into nano and sub-nano copper oxide particles, thereby obtaining a catalyst precursor.

[0129] (6) The catalyst precursor is subjected to hydrogen reduction treatment. The reduction temperature is 400°C, the reduction time is 4 hours, and the hydrogen flow rate (expressed as the volume space velocity of hydrogen, defined as the volume of hydrogen passing through a unit volume of catalyst per unit time, calculated as an ideal gas) is 300 hours. -1 After hydrogen reduction treatment, the finished Cu-Beta zeolite catalyst was obtained, code-named Cu3-Beta24C-1.

[0130] Secondly, in order to understand the implementation effect of the catalyst preparation method provided by the present invention from the aspect of the physicochemical properties of the catalyst, the carrier crystal structure and surface hydroxyl groups of Cu3-Beta24C-1 and its dimple-modified dealuminated Beta zeolite carrier (Beta24C) were characterized by XRD and FT-IR, respectively. In addition, TEM photos of the Cu3-Beta24C-1 catalyst and its high-temperature calcined sample (550°C×3h) were taken by transmission electron microscopy.

[0131] From the XRD characterization results ( Figure 2 ) found that the Cu3-Beta24C-1 catalyst prepared by the improved ammonia evaporation method provided by the present invention well retains the crystal structure of the Beta zeolite carrier, and the relative crystallinity of the zeolite in the catalyst calculated based on the dealuminized Beta zeolite carrier (Beta24C) modified by the chiseled cavity is 84%. From the FT-IR characterization results, it was found that the intensity of the infrared characteristic band of the zeolite hydroxyl cavity of the Cu3-Beta24C-1 catalyst decreased significantly compared with the dealuminized Beta zeolite carrier modified by the chiseled cavity, indicating that the metal copper occupied a large number of hydroxyl cavity lattice defect sites. In addition, from the TEM photos ( Figure 3 and Figure 4 ) It can be seen that the metallic copper in the Cu3-Beta24C-1 catalyst exists in the form of highly dispersed nano and sub-nano particles, with an average particle size of about 5nm. After calcination at 550℃ for 3h, the metallic copper particles are well dispersed, with an average particle size of about 8nm. These data indicate that the hydroxyl nest lattice defect sites of the dealuminated Beta zeolite carrier modified by the chiseling have a good effect of dispersing and stabilizing nano and sub-nano copper particles.

[0132] On this basis, the catalytic performance of Cu3-Beta24C-1 catalyst and its 550℃ high-temperature calcined sample were evaluated by the gas-solid phase hydroamination of caprolactone to produce caprolactam. The reaction was carried out in a small fixed-bed reactor. The inner diameter of the stainless steel reaction tube was 9mm, and the upper feeding and lower discharging operation mode was adopted. 2g of tablet-formed catalyst (20-40 mesh samples were taken after sieving) was loaded in the constant temperature zone of the reactor. The upper and lower spaces of the catalyst bed were filled with inert ceramic balls. Among them, the upper ceramic ball area of ​​the reactor served as the vaporization and preheating zone of the raw materials. The temperature of the reaction constant temperature zone was 270℃, the reaction pressure was 1atm, and the feed space velocity (WHSV) of caprolactone was 0.6h -1 . For convenience, caprolactone, ammonia water raw materials (analytical grade, ammonia concentration of 25-28wt.%) and deionized water were prepared into raw material liquid according to the ammonia-ester molar ratio of 6 and the water-ester molar ratio of 30, and the reactor was fed with a micro-metering pump, and the hydrogen was fed with a mass flow meter according to the hydrogen-ester molar ratio of 50. The reaction product was continuously collected by a stainless steel collection tank connected to the reactor outlet and equipped with a cooling water jacket. The product liquid was collected at fixed time intervals and analyzed on Shimadzu gas chromatograph GC-2014 (FID detector, OV-1701 chromatographic column), and the caprolactone conversion rate and caprolactam selectivity were calculated by the internal standard method (internal standard substance was 1,4-dioxane). Under the above conditions, when the hydroamination reaction of caprolactone was carried out continuously for 6 hours, the caprolactam yield of Cu3-Beta24C-1 catalyst was about 82%; the caprolactam yield of its 550℃ high temperature roasted sample was close to 81%. The above reaction results show that the Cu-Beta zeolite catalyst provided by the present invention is a catalyst with excellent performance for the hydroamination of caprolactone to produce caprolactam.

[0133] Comparative Example 1: This example is used to illustrate that when a dealuminated Beta zeolite modified by chiseling is used as a carrier and copper is loaded by the traditional ammonia evaporation method to prepare a Cu-Beta zeolite catalyst, the crystal structure of the Beta zeolite carrier is greatly damaged, the loaded metallic copper is mainly located outside the zeolite pores, the dispersion is low, and the copper particles are large in size. Since the active silanol groups in the hydroxyl holes of the dealuminated Beta zeolite are not protected, the anti-sintering ability is poor, and the stability of the catalyst is poor, and the performance is poor in the gas-solid phase hydroamination reaction of caprolactone to produce caprolactam.

[0134] Example 1 was repeated, but after preparing the dealuminated Beta zeolite carrier (Beta24C) modified by the chiseling in the second step, copper hydroxide was deposited on the zeolite carrier by the conventional ammonia evaporation method as disclosed in the open document Science 10.1126 / science.adj1962 (2023), as follows:

[0135] (1) 1.18 g of Cu(NO3)2·3H2O was dissolved in 515 ml of aqueous ammonia solution (containing 3.86 g of NH3·H2O, equivalent to 8.1 ml of 26 wt.% industrial ammonia solution, with a molar ratio of copper ions to ammonia molecules of about 1:23) and stirred at room temperature for 10 min to prepare a copper-ammonia complex aqueous solution (complex ion concentration of about 9.5 mmol / L, i.e., 9.5 mM);

[0136] (2) 10 g of the dealuminated Beta zeolite carrier (Beta24C) modified by the chiseling process was added to 515 ml of the copper-ammine complex solution and subjected to ammonia evaporation treatment under vigorous stirring. The ammonia evaporation temperature was 80°C and the ammonia evaporation time was 6 h;

[0137] (3) After the ammonia evaporation is completed, the water solvent of the diluted and excess copper-ammine complex solution is finally removed by filtration. The filter cake obtained is dried, calcined and hydrogen-reduced in the same post-treatment method as in Example 1 to obtain a Cu-Beta zeolite catalyst, code-named Cu3-Beta24C-CE1 (CE=Comparative Example).

[0138] In order to understand the characteristics of Cu-Beta zeolite catalyst prepared by traditional ammonia distillation method from the perspective of physicochemical properties of the catalyst, the Beta zeolite crystal structure of Cu3-Beta24C-CE1 catalyst was characterized by XRD method and compared with its carrier (Beta24C). Figure 5 In addition, the Cu metal dispersion of Cu3-Beta24C-CE1 catalyst and its high temperature calcined sample (550℃×3h) was characterized by transmission electron microscopy, and the catalytic performance of Cu3-Beta24C-CE1 catalyst and its high temperature calcined sample at 550℃ was evaluated by gas-solid phase hydroamination of caprolactone to produce caprolactam.

[0139] XRD characterization results ( Figure 5) showed that the zeolite crystal structure of the Cu3-Beta24C-CE1 catalyst prepared by the traditional ammonia evaporation method was greatly damaged, and the relative crystallinity of the zeolite calculated based on its carrier (Beta24C) was 65%. According to the characterization results of transmission electron microscopy, the average particle size of Cu metal of the Cu3-Beta24C-CE1 catalyst and its high-temperature calcined sample was 10nm and 21nm, respectively, that is, the Cu metal dispersion on the catalyst was low and easy to sinter. The reaction evaluation results showed that under the same reaction conditions, the caprolactam yield of the Cu3-Beta24C-CE1 catalyst was about 76%; the caprolactam yield of its high-temperature calcined sample was about 72%. The reaction results show that the Cu-Beta zeolite catalyst prepared by the traditional ammonia evaporation method on the dealuminated Beta zeolite carrier modified by the chiseling hole has low catalytic activity for the gas-solid phase hydroamination of caprolactone to produce caprolactam and has poor resistance to sintering deactivation.

[0140] Comparative Example 2: This example is used to illustrate that using dealuminated Beta zeolite modified by chiseling instead of dealuminated Beta zeolite as a carrier of Cu-Beta catalyst and using an improved ammonia evaporation method to load copper in the pores to prepare Cu-Beta zeolite catalyst is beneficial to obtaining a Cu-Beta zeolite catalyst with stronger anti-sintering ability and better stability.

[0141] Example 1 was repeated, but the dealuminated Beta zeolite carrier (Beta24c) prepared in the first step was directly used in the third step, and copper was loaded in the pores by the improved ammonia evaporation method to prepare a Cu-Beta zeolite catalyst. Among them, when the dealuminated Beta zeolite carrier was impregnated with an equal volume of copper ammonia complex solution, the water absorption of the dealuminated Beta zeolite (Beta24c) was measured by deionized water titration method to be 1.2 ml / g. According to the feed amount of 10 g of the carrier, a total of 12 ml of copper ammonia complex solution is required. According to the copper loading of 3 wt.%, the concentration of the required copper ammonia complex solution is about 0.39 M. That is, the calculated value of the required copper ammonia complex solution concentration is very close to the concentration of the saturated solution of copper ammonia complex (0.4 M). Therefore, 10 g of the dealuminated Beta zeolite carrier was directly impregnated with an equal volume of 12 ml of a saturated solution of copper ammonia complex. Other methods remain unchanged. The obtained Cu-Beta zeolite catalyst is named Cu3-Beta24c-CE2.

[0142] To avoid tediousness, in this example, only the catalytic performance of Cu3-Beta24c-CE2 catalyst and its high temperature calcined sample (550℃×3h) was evaluated by the gas-solid phase hydroamination of caprolactone to caprolactam. The reaction evaluation results show that under the same reaction conditions, the caprolactam yield of Cu3-Beta24c-CE2 catalyst is about 78%; the caprolactam yield of its high temperature calcined sample is about 77%. The reaction results show that the Cu-Beta zeolite catalyst directly prepared by the improved ammonia evaporation method with dealuminated Beta zeolite as the carrier also has good catalytic activity and resistance to sintering deactivation in the gas-solid phase hydroamination of caprolactone to caprolactam, but its catalytic performance is obviously not as good as the catalyst prepared with the dealuminated Beta zeolite modified by the chiseling as the carrier.

[0143] Comparative Example 3: This example is used to illustrate that amorphous fumed silica (white carbon black, BET specific surface area 286m 2 / g) as a carrier and the copper-silicon dioxide catalyst prepared by the traditional ammonia evaporation method with copper loading has poor sintering resistance and stability.

[0144] The conventional ammonia distillation method described in this example is based on the method of Example 1 in U.S. Pat. No. 4,440,873 (1984), which is as follows:

[0145] (1) 1.14 g of copper nitrate (Cu(NO3)2.3H2O) was dissolved in 100 ml of water to obtain an aqueous solution containing copper ions, and then 3.6 ml of concentrated ammonia solution (industrial ammonia water with an NH3 content of 26 wt.%, density 0.89 g / ml) was added thereto at a molar ratio of copper ions to ammonia molecules of about 1:10, and 50 ml of water was added to obtain a dark blue copper-ammonia complex solution with a pH value of 11-12 (complex ion concentration of about 30.8 mM. The purpose of adding 50 ml of water was to keep the ratio of solution volume to silica dry basis consistent with the literature);

[0146] (2) adding 10 g of fumed silica (dry basis) to the copper ammonia complex solution and stirring at room temperature for 2 h;

[0147] (3) heating the reaction mixture of step (2) to evaporate ammonia (80° C., 6 h), and when the pH of the mixture drops to 6-7, filtering to obtain a solid, washing it three times with deionized water to obtain a solid product;

[0148] (4) drying the solid product at 120°C for 12 h and calcining at 450°C for 4 h;

[0149] (5) The calcined solid product was subjected to hydrogen reduction treatment at 350°C for 2 h to obtain a copper-silicon dioxide catalyst, codenamed Cu3-SiO2-CE3.

[0150] The evaluation results of the gas-solid phase hydroamination of caprolactone to caprolactam showed that under the same reaction conditions, the caprolactam yield of the Cu3-SiO2-CE3 catalyst was about 75%; the caprolactam yield of its high-temperature calcined sample (550℃×3h) was 65%. The reaction results show that the copper-based catalyst prepared with amorphous silica as a carrier has poor sintering resistance and its catalytic activity drops significantly after high-temperature treatment.

[0151] Comparative Example 4: This example is used to further illustrate that the copper-silicon dioxide catalyst prepared by the traditional ammonia evaporation method of copper loading has poor sintering resistance and poor stability.

[0152] Comparative Example 3 was repeated, but 33.3 g of silica sol (30 wt.% SiO2) was used as a precursor for the in-situ generation of 10 g of silica support. In order to keep the ratio of the volume of the copper ammonia complex solution to the dry basis of silica consistent with that of Comparative Example 3, the amount of water added in step (1) when preparing the copper ammonia complex solution was changed to 26.7 ml. The prepared copper-silica catalyst was coded as Cu3-SiO2-CE4

[0153] The evaluation results of the gas-solid phase hydroamination of caprolactone to caprolactam showed that under the same reaction conditions, the caprolactam yield of the Cu3-SiO2-CE4 catalyst was 79%; the caprolactam yield of its high-temperature calcined sample (550℃×3h) was 70%. The reaction results also show that the copper-based catalyst prepared with amorphous silica as a carrier has poor sintering resistance and its catalytic activity drops significantly after high-temperature treatment.

[0154] Comparative Example 5: This example is used to illustrate that the amorphous nature of the silica carrier determines that the copper-silica catalyst has poor sintering resistance and poor stability.

[0155] In this example, the copper-silicon dioxide catalyst was prepared on a fumed silicon dioxide carrier using the improved ammonia evaporation method provided by the present invention. The details are as follows:

[0156] Example 1 was repeated, but 10 g of the dealuminated Beta zeolite carrier modified by the chiseling was replaced by 10 g (dry basis) of fumed silica (white carbon black, BET specific surface area 286 m 2 / g, saturated water absorption rate is 2.5ml / g), 10g fumed silica requires 25ml of copper ammonia complex solution. According to the copper loading of 3wt.%, the concentration of the required copper ammonia complex solution is about 0.19M. 11.9ml of the saturated copper ammonia complex solution is diluted to 25ml with a dilute ammonia base solution to obtain 25ml of a copper ammonia complex solution with a concentration of 0.19M. The prepared copper-silicon dioxide catalyst is code-named Cu3-SiO2-CE5.

[0157] The evaluation results of the gas-solid phase hydroamination of caprolactone to caprolactam showed that under the same reaction conditions, the caprolactam yield of the Cu3-SiO2-CE5 catalyst was 76%; the caprolactam yield of its high-temperature calcined sample (550℃×3h) was 65%. The reaction results also show that the copper-based catalyst prepared with amorphous silica as a carrier has poor sintering resistance and its catalytic activity drops significantly after high-temperature treatment.

[0158] Example 2: This example is used to illustrate that according to the method for preparing a Cu-Beta zeolite catalyst provided by the present invention, which uses a dealuminated Beta zeolite modified by chiseling as a carrier and uses an improved ammonia evaporation method to load copper in the zeolite pores, Cu-Beta zeolite catalysts with different metallic copper loadings can be prepared.

[0159] Example 1 was repeated, but the copper loading in the prepared Cu-Beta zeolite catalyst was reduced to 1wt.% and 2wt.% respectively, and the concentration of the required copper ammonia complex solution was about 0.13M and 0.25M respectively. 3.9ml and 7.8ml of the saturated copper ammonia complex solution were diluted to 12.5ml with a dilute ammonia base solution to obtain equal volume impregnation solutions of Cu-Beta zeolite catalysts with copper loadings of 1wt.% and 2wt.%. When the Cu-Beta zeolite catalyst was prepared by the improved ammonia evaporation method, the time for the equal volume impregnation treatment of the dealuminated Beta carrier (Beta24C) modified by the chiseling at room temperature was changed to 6h, the temperature and time of the ammonia evaporation treatment were changed to 65℃ and 12h respectively, the temperature and time of the dehydration drying were changed to 150℃ and 3h respectively, the subsequent calcination temperature and time were changed to 450℃ and 6h respectively, the final hydrogen reduction temperature and time were changed to 350℃ and 8h respectively, and the hydrogen flow rate (volume space velocity) was changed to 1000h -1 The prepared Cu-Beta zeolite catalysts are coded Cu1-Beta24C-2 and Cu2-Beta24C-2, respectively.

[0160] The evaluation results of the gas-solid phase hydroamination of caprolactone to produce caprolactam showed that under the same reaction conditions, the caprolactam yield of Cu1-Beta24C-2 catalyst was 80%; the caprolactam yield of Cu2-Beta24C-2 was 81%.

[0161] Example 3: This example is used to further illustrate that according to the method for preparing a Cu-Beta zeolite catalyst provided by the present invention, which uses a dealuminated Beta zeolite modified by chiseling as a carrier and uses an improved ammonia distillation method to load copper in the zeolite pores, a Cu-Beta zeolite catalyst with different metallic copper loadings can be prepared. However, when preparing a Cu-Beta zeolite catalyst with a copper loading of more than 3 wt.%, it is preferable to use a multiple loading scheme to prepare the catalyst.

[0162] Example 1 was repeated, but the copper loading in the prepared Cu-Beta zeolite catalyst was increased to 4wt.% and 6wt.%, respectively, and the concentrations of the required copper ammonia complex solution were calculated to be approximately 0.50M and 0.76M, respectively. Obviously, the required copper ammonia complex concentrations all exceeded the concentration (0.4M) of the copper ammonia complex saturated solution prepared with a dilute ammonia base solution. We tried to use industrial ammonia instead of the dilute ammonia base solution to dissolve the copper ammonia complex, and the maximum concentration of the copper ammonia complex solution was approximately 0.5M. Although a high-concentration copper ammonia complex solution with a concentration of approximately 0.5M can be prepared by dissolving the copper ammonia complex with industrial ammonia, the ammonia / copper ion molar ratio of the solution exceeds 24:1, the alkalinity is strong, and the ammonia volatilization is serious, which is not conducive to protecting the crystal structure of the dealuminated Beta zeolite and is not conducive to operation. This shows that the improved ammonia evaporation method cannot obtain a Cu-Beta zeolite catalyst with a high copper loading by a single equal volume impregnation and ammonia evaporation operation on a given dealuminated Beta zeolite carrier modified by a given chiseling hole. In view of this, the present invention uses a dilute ammonia base solution to dilute a saturated solution of a copper-ammine complex, and prepares a Cu-Beta zeolite catalyst with a copper loading increased to 4wt.% and 6wt.% respectively through multiple equal volume impregnation and ammonia evaporation operations. For the preparation of a catalyst with a copper loading of 4wt.%, the equal volume impregnation and ammonia evaporation operations can be carried out twice, such as 1wt.%+3wt.%, 2wt.%+2wt.%; for the preparation of a catalyst with a copper loading of 6wt.%, it can be carried out twice (3wt.%+3wt.%), or it can be carried out three times (2wt.%+2wt.%+2wt.%). For simplicity, in this example, the preparation of a Cu-Beta zeolite catalyst with a copper loading increased to 4wt.% and 6wt.% respectively is carried out twice (2wt.%+2wt.%, 3wt.%+3wt.%). To load 2 wt.% of copper metal on a dealuminated Beta zeolite carrier modified by a chiseled hole by an improved ammonia evaporation method, 12.5 ml of an impregnation solution with a copper-ammine complex concentration of 0.25 M is required; to load 3 wt.% of copper metal on a dealuminated Beta zeolite carrier modified by a chiseled hole by a single time, 12.5 ml of an impregnation solution with a copper-ammine complex concentration of 0.38 M is required. The 0.25 M impregnation solution is obtained by diluting 7.8 ml of a saturated copper-ammine complex solution with a dilute ammonia base solution, and the 0.38 M impregnation solution is directly obtained by using a saturated copper-ammine complex solution. When the dealuminated Beta carrier modified by the chiseling was treated with equal volume impregnation at room temperature, the impregnation time was changed to 6 h, the temperature and time of the ammonia evaporation treatment were changed to 85 ° C and 3 h, respectively, the temperature and time of the dehydration drying were changed to 120 ° C and 5 h, respectively, the subsequent calcination temperature and time were changed to 550 ° C and 2 h, respectively, the final hydrogen reduction temperature and time were changed to 500 ° C and 2 h, respectively, and the hydrogen flow rate (volume space velocity) was changed to 20 h. -1(After preparing a mixed gas with an appropriate amount of nitrogen, the feed is controlled by a mass flow meter.) The prepared Cu-Beta zeolite catalysts are coded Cu4-Beta24C-3 and Cu6-Beta24C-3, respectively.

[0163] The evaluation results of the gas-solid phase hydroamination of caprolactone to produce caprolactam showed that under the same reaction conditions, the caprolactam yield of Cu4-Beta24C-3 catalyst was 85%; the caprolactam yield of Cu6-Beta24C-3 was 84%.

[0164] Example 4: This example is used to illustrate that when preparing Cu-Beta zeolite catalyst according to the improved ammonia distillation method provided by the present invention, it is allowed to use Beta zeolite matrix with different particle sizes to prepare dealuminated Beta zeolite carrier.

[0165] Example 1 was repeated, but in the first step of preparing the dealuminated Beta zeolite carrier, a Beta zeolite matrix with a silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) of 22 was synthesized by the hydrothermal crystallization method (with ammonium fluoride as an auxiliary agent) provided in the open document J. Mater. Sci. 41 (2006) 1861-1864 as the raw material for preparing the dealuminated Beta zeolite carrier. The synthesized Beta zeolite matrix was subjected to conventional filtration, washing, drying (80°C, 24h) and calcination to remove the template agent (600°C, 3h). The average grain size of the synthesized Beta zeolite matrix was 1 μm by TEM observation, belonging to large-grained Beta zeolite. No impurities were found in the matrix by XRD inspection. The BET specific surface area was calculated to be about 480 m by nitrogen physical adsorption data. 2 / g, and its molar ratio of silicon and aluminum oxide (molar ratio of SiO2 to Al2O3) measured by XRF method is about 23, which meets the technical requirements of the present invention for Beta zeolite matrix. The Beta zeolite matrix is ​​dealuminated with 13M concentrated nitric acid to become a large-grain dealuminated Beta zeolite carrier (codenamed Beta23c), and its molar ratio of silicon and aluminum oxide (molar ratio of SiO2 to Al2O3) is 748 (>700), which meets the technical requirements of the present invention for dealuminated Beta zeolite carrier. On this basis, according to the method of the second step of Example 1, the above-mentioned large-grain dealuminated Beta zeolite carrier (Beta23c) is subjected to a chiseling modification treatment with an aqueous solution of ethanolamine to obtain a chiseled modified large-grain dealuminated Beta zeolite carrier, named Beta23C; further according to the method of the third step of Example 1, copper is loaded in the zeolite pores by an improved ammonia evaporation method to obtain a Cu-Beta zeolite catalyst with a copper content of 3wt.%, codenamed Cu3-Beta23C-4.

[0166] The evaluation results of the gas-solid phase hydroamination of caprolactone to produce caprolactam showed that under the same reaction conditions, the caprolactam yield of the Cu3-Beta23C-4 catalyst was 83%.

[0167] Example 5: This example is used to illustrate that when a Cu-Beta zeolite catalyst is prepared by loading copper in the pores using an improved ammonia evaporation method using dealuminized Beta zeolite modified by chiseling as a carrier according to the present invention, the chiseling degree of the dealuminized Beta zeolite can be regulated by changing the impregnation modification conditions of the ethanolamine solution.

[0168] Example 1 was repeated, but in the second step, when the hydroxyl nests of the dealuminated Beta zeolite carrier were modified by chiseling with an aqueous solution of ethanolamine, the concentration of the aqueous solution of ethanolamine was changed to 0.16M, the ratio of the volume of the modified liquid to the amount of the dealuminated Beta zeolite carrier (Beta24c) (liquid-to-solid ratio) was changed to 10:1, the immersion temperature was changed to 50°C, and the immersion time was changed to 0.5h. After the chiseling modification was completed, the reaction material was filtered to recover the solid product, and then the solid product was repeatedly washed with deionized water until neutral, and then dried (overnight at 110°C) and calcined (550°C, 3h) to obtain the dealuminated Beta zeolite modified by chiseling. It was sealed and stored for later use. According to the weight loss estimation, the average number of skeleton silicon atoms (in terms of SiO2) chiseled out of the hydroxyl nest lattice defect of the dealuminated Beta zeolite carrier was 1.5 silicon atoms, and the desiliconization amount increased. The above treatment conditions strengthen the chiseling modification treatment and increase the geometric space of the hydroxyl pit lattice defect site of the dealuminated Beta zeolite. On this basis, the improved ammonia evaporation method is used to load copper in the pores of the modified carrier to prepare a Cu-Beta zeolite catalyst with a copper content of 3wt.%, named Cu3-Beta24C-5.

[0169] The evaluation results of the gas-solid phase hydroamination of caprolactone to produce caprolactam showed that under the same reaction conditions, the caprolactam yield of the Cu3-Beta24C-5 catalyst was 84%; the caprolactam yield of its high-temperature calcined sample (550℃×3h) was 83%.

[0170] Example 6: This example is used to further illustrate that when a Cu-Beta zeolite catalyst is prepared by loading copper in the pores using an improved ammonia evaporation method using dealuminized Beta zeolite modified by chiseling as a carrier according to the present invention, the chiseling degree of the dealuminized Beta zeolite can be regulated by changing the impregnation modification conditions of the ethanolamine solution.

[0171] Example 1 was repeated, but in the second step, when the hydroxyl nests of the dealuminated Beta zeolite carrier were subjected to a chiseling modification treatment with an aqueous solution of ethanolamine, the concentration of the aqueous solution of ethanolamine was changed to 0.30 M, the liquid-to-solid ratio was changed to 2:1, the immersion temperature was changed to 20°C, and the immersion time was changed to 1 h. After the chiseling modification was completed, the reaction material was filtered to recover the solid product, and then the solid product was repeatedly washed with deionized water until neutral, and then dried (overnight at 110°C) and calcined (550°C, 3h) to obtain a chiseled-modified dealuminated Beta zeolite. It was sealed and stored for later use. According to the weight loss estimation, the average number of skeleton silicon atoms (in terms of SiO2) chiseled out of the hydroxyl nest lattice defect sites of the dealuminated Beta zeolite carrier was 1.1 silicon atoms, and the amount of desiliconization was reduced, indicating that the above combination of chiseling modification conditions weakened the chiseling modification treatment. On this basis, an improved ammonia evaporation method was used to load copper in the pores to prepare a Cu-Beta zeolite catalyst with a copper content of 3wt.%, named Cu3-Beta24C-6.

[0172] The evaluation results of the gas-solid phase hydroamination of caprolactone to produce caprolactam showed that under the same reaction conditions, the caprolactam yield of the Cu3-Beta24C-6 catalyst was 83%; the caprolactam yield of its high-temperature calcined sample (550℃×3h) was 83%.

[0173] Example 7: This example is used to illustrate that when preparing Cu-Beta zeolite catalysts according to the improved ammonia distillation method provided by the present invention, it is allowed to use Beta zeolite matrix with different silicon-aluminum oxide molar ratios (molar ratios of SiO2 to Al2O3) to prepare the dealuminated Beta zeolite carrier modified by the chiseling. When Beta zeolite with a higher silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) is used as the matrix, a relatively mild combination of chiseling modification conditions is preferably used. The opposite is also true.

[0174] Example 1 was repeated, but in the first step of preparing the dealuminated Beta zeolite carrier, a Beta zeolite matrix with a silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) of 60 was synthesized by the hydrothermal crystallization method provided in U.S. Pat. No. 3,308,069 (1967) as the raw material for preparing the dealuminated Beta zeolite carrier. The synthesized Beta zeolite matrix was subjected to conventional filtration, washing, drying (170°C, 3h) and calcination to remove the template agent (500°C, 8h). The average grain size of the synthesized Beta zeolite matrix was close to 100 nanometers by TEM observation, belonging to nano Beta zeolite. No impurity crystals were found in the matrix by XRD inspection. The BET specific surface area was calculated to be about 530 m 2 / g, and the molar ratio of silicon aluminum oxide (the molar ratio of SiO2 to Al2O3) measured by XRF method is about 57, which meets the technical requirements of the present invention for Beta zeolite matrix.

[0175] The Beta zeolite matrix was used for dealumination with concentrated nitric acid to prepare a dealuminated Beta zeolite carrier, and a dealuminated Beta zeolite carrier (codenamed Beta57c) with a silicon aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) of 861 (>800) was obtained. The dealumination degree of the carrier meets the requirements of the present invention. In the second step, when the hydroxyl nests of the dealuminated Beta zeolite carrier were subjected to a chiseling modification treatment with an aqueous solution of ethanolamine, the concentration of the aqueous solution of ethanolamine was changed to 0.02M, the liquid-solid ratio was changed to 20:1, the immersion temperature was changed to 80°C, and the immersion time was changed to 5h. After the chiseling modification was completed, the reaction material was filtered to recover the solid product, and then the solid product was repeatedly washed with deionized water until neutral, and then dried (overnight at 110°C) and calcined (550°C, 3h) to obtain a chiseled-modified dealuminated Beta zeolite. It was sealed and stored for later use. According to the weight loss estimation, the average number of skeleton silicon atoms (in terms of SiO2) chiseled out of the hydroxyl nest lattice defect of the dealuminated Beta zeolite carrier is 1.6 silicon atoms, and the desiliconization amount has increased, indicating that the above combination of chiseling modification conditions has strengthened the chiseling modification treatment for the dealuminated Beta zeolite carrier with a small number of hydroxyl nests. The obtained chiseled-hole modified dealuminated Beta zeolite carrier is named Beta57C; further according to the third step of Example 1, copper is loaded in the zeolite pores by an improved ammonia evaporation method to obtain a Cu-Beta zeolite catalyst with a copper content of 3wt.%. Among them, when the carrier is impregnated with an equal volume of a saturated solution of a copper-ammonia complex at room temperature, the impregnation time is changed to 2h. When ammonia is evaporated, a slight negative pressure ammonia is used, the ammonia evaporation temperature is 50℃, and the ammonia evaporation time is 48h. When the material after ammonia evaporation is dehydrated and dried, the drying temperature and time are changed to 100℃ and 48h respectively. The subsequent calcination temperature and time are changed to 350℃ and 24h respectively. The final hydrogen reduction treatment temperature, time and hydrogen flow rate (volume space velocity) were changed to 300 °C, 20 h and 2000 h, respectively. -1 , the catalyst code is Cu3-Beta57C-7.

[0176] The evaluation results of the gas-solid phase hydroamination of caprolactone to produce caprolactam showed that under the same reaction conditions, the caprolactam yield of the Cu3-Beta57C-7 catalyst was 81%.

[0177] Example 8: This example is used to further illustrate that when preparing Cu-Beta zeolite catalyst according to the improved ammonia distillation method provided by the present invention, it is allowed to use Beta zeolite matrix with different silicon-aluminum oxide molar ratios (molar ratio of SiO2 to Al2O3) to prepare the dealuminated Beta zeolite carrier modified by the chiseling. When Beta zeolite with a higher silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) is used as the matrix, a relatively mild combination of chiseling modification conditions is preferably used. The opposite is also true.

[0178] Example 7 was repeated, but in the second step, when the hydroxyl nests of the dealuminated Beta zeolite carrier were subjected to a chiseling modification treatment with an aqueous solution of ethanolamine, the liquid-to-solid ratio was changed to 100:1, and the immersion time was changed to 24 hours. After the chiseling modification was completed, the reaction materials were filtered to recover the solid product, and then the solid product was repeatedly washed with deionized water until neutral, and then dried (overnight at 110°C) and calcined (550°C, 3h) to obtain the chiseled-modified dealuminated Beta zeolite. It was sealed and stored for later use. According to the weight loss estimation, the average number of skeleton silicon atoms (in terms of SiO2) chiseled out of the hydroxyl nest lattice defect sites of the dealuminated Beta zeolite carrier was 3.0 silicon atoms, and the desiliconization amount was significantly increased, indicating that the above combination of chiseling modification conditions strengthened the chiseling modification treatment for the dealuminated Beta zeolite carrier with a small number of hydroxyl nests. On this basis, the obtained dealuminated Beta zeolite modified by the chiseling was used as a carrier, and a Cu-beta zeolite catalyst was prepared according to the third step of Example 1, with the code name of Cu3-Beta57C-8.

[0179] The evaluation results of the gas-solid phase hydroamination of caprolactone to produce caprolactam showed that under the same reaction conditions, the caprolactam yield of the Cu3-Beta57C-8 catalyst was 75%.

[0180] Example 9: This example is used to further illustrate that when preparing Cu-Beta zeolite catalyst according to the improved ammonia distillation method provided by the present invention, it is allowed to use Beta zeolite matrix with different silicon-aluminum oxide molar ratios (molar ratio of SiO2 to Al2O3) to prepare the dealuminated Beta zeolite carrier modified by the chiseling. When Beta zeolite with a higher silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) is used as the matrix, a relatively mild combination of chiseling modification conditions is preferably used. The opposite is also true.

[0181] Example 1 was repeated, but in the first step of preparing the dealuminated Beta zeolite carrier, the Beta zeolite matrix with a silicon-aluminum oxide molar ratio (a molar ratio of SiO2 to Al2O3) of 40, 80, 100, 150 and 200 was synthesized by itself as the raw material for preparing the dealuminated Beta zeolite carrier according to the hydrothermal crystallization method provided in Chinese invention patent CN1108275C (application date 1999.9.10). After the synthesized Beta zeolite matrix was subjected to conventional filtration, washing, drying (110°C, 12h) and calcination to remove the template agent (540°C, 6h), the average grain size of the Beta zeolite matrix was observed by TEM to be of nanometer level and small grain (less than 1μm) level. As the silicon-aluminum oxide molar ratio (a molar ratio of SiO2 to Al2O3) increased, the grain size increased; no impurities were found in the matrix by XRD inspection, and the BET specific surface area calculated by the nitrogen physical adsorption data was higher than 500m 2 / g, and the molar ratio of silicon aluminum oxide (the molar ratio of SiO2 to Al2O3) measured by XRF method is 38, 72, 94, 136 and 189 respectively, which meets the technical requirements of the present invention for Beta zeolite matrix.

[0182] The above five Beta zeolite precursors were used for dealumination with concentrated nitric acid to prepare dealumination Beta zeolite carriers, and five dealumination Beta zeolite carriers Beta38c, Beta72c, Beta94c, Beta136c and Beta189c were obtained, and the molar ratio of silicon aluminum oxide (the molar ratio of SiO2 to Al2O3) was 870, 855, 932, 1088 and 960 respectively, which all met the technical requirements of dealumination Beta zeolite carriers. On this basis, according to the second step of Example 1, the above dealumination Beta zeolite carriers were subjected to a chiseling modification treatment with an aqueous solution of ethanolamine. The chiseling modification treatment conditions are: the concentration of the ethanolamine aqueous solution was changed to 0.01M, the liquid-solid ratio was changed to 20:1, the immersion temperature was changed to 80°C, and the immersion time was changed to 3h. After the chiseling modification is completed, the reaction material is filtered to recover the solid product, and then the solid product is repeatedly washed with deionized water until it is neutral, and then dried (overnight at 110°C) and calcined (550°C, 3h) to obtain the chiseled-modified dealuminated Beta zeolite carriers, named Beta38C, Beta72C, Beta94C, Beta136C and Beta189C. Seal and store for later use. According to the weight loss estimation, in the above-mentioned chiseled-modified dealuminated Beta zeolite carriers, the average number of skeleton silicon atoms (in terms of SiO2) chiseled out of the hydroxyl nest lattice defect sites of the dealuminated Beta zeolite carriers is 0.3, 0.7, 1.0, 1.8 and 2.5 respectively. That is, the above combination of cavitation modification conditions results in an insufficient degree of cavitation modification for the dealuminated Beta zeolite carrier prepared from a Beta zeolite matrix with a lower silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3), while the cavitation modification degree is too strong for the dealuminated Beta zeolite carrier prepared from a Beta zeolite matrix with a high silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3).

[0183] Further according to the third step of Example 1, copper is loaded in the pores of the zeolite by using an improved ammonia evaporation method to obtain a Cu-Beta zeolite catalyst with a copper content of 3 wt.%, wherein when the carrier is impregnated with an equal volume of a saturated solution of a copper-ammine complex at room temperature, the impregnation time is changed to 1 hour. When evaporating ammonia, the ammonia evaporation temperature is changed to 90°C and the ammonia evaporation time is changed to 1 hour. When dehydrating and drying the material after ammonia evaporation, the drying temperature and time are changed to 200°C and 1 hour, respectively. The subsequent calcination treatment temperature and time are changed to 550°C and 1 hour, respectively. The final hydrogen reduction treatment temperature, time and hydrogen flow rate are changed to 550°C, 1 hour and 5 hours, respectively. -1(After preparing a mixed gas with an appropriate amount of nitrogen, the feed is controlled by a mass flow meter). The catalyst codes are Cu3-Beta38C-9, Cu3-Beta72C-9, Cu3-Beta94C-9, Cu3-Beta136C-9 and Cu3-Beta189C-9 respectively.

[0184] The anti-sintering deactivation performance of the above catalysts and their samples calcined at 550℃ (3h) was evaluated by the gas-solid phase hydroamination of caprolactone to produce caprolactam. The results showed that under the same reaction conditions, the catalytic activity of Cu3-Beta38C-9, Cu3-Beta72C-9, Cu3-Beta94C-9, Cu3-Beta136C-9 and Cu3-Beta189C-9 catalysts decreased by approximately 4%, 7%, 7%, 8% and 11% respectively after high temperature calcination.

[0185] Example 10: This example is used to further illustrate that when preparing Cu-Beta zeolite catalysts according to the improved ammonia distillation method provided by the present invention, Beta zeolite matrix with different silicon-aluminum oxide molar ratios (molar ratios of SiO2 to Al2O3) is allowed to be used to prepare the dealuminated Beta zeolite carrier modified by the chiseling. When Beta zeolite with a higher silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) is used as the matrix, a relatively mild combination of chiseling modification conditions is preferably used. The opposite is also true.

[0186] Example 9 was repeated, but in the second step, when different dealuminated Beta zeolite carriers were subjected to the chiseling modification treatment with an aqueous solution of ethanolamine, the concentration of the aqueous solution of ethanolamine was changed to 0.08 M. After the chiseling modification was completed, the reaction materials were filtered to recover the solid product, and then the solid product was repeatedly washed with deionized water until neutral, and then dried (overnight at 110°C) and calcined (550°C, 3h) to obtain the chiseled-modified dealuminated Beta zeolite carriers, which were named Beta38C, Beta72C, Beta94C, Beta136C and Beta189C. They were sealed and stored for later use. According to the weight loss estimation, in the above-mentioned chiseled-modified dealuminated Beta zeolite matrix, the average values ​​of the number of skeleton silicon atoms (in terms of SiO2) chiseled out at the hydroxyl nest lattice defect sites of the dealuminated Beta zeolite carriers were 0.9, 1.6, 2.1, 3.0 and 4.3, respectively. That is, the above combination of cavitation modification conditions is more suitable for the dealuminated Beta zeolite carrier prepared from a Beta zeolite matrix with a lower silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3), while the cavitation modification degree is too strong for the dealuminated Beta zeolite carrier prepared from a Beta zeolite matrix with a high silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3).

[0187] The catalysts prepared by the improved ammonia distillation method on the above-mentioned dimple-modified dealuminized Beta zeolite carrier are coded Cu3-Beta38C-10, Cu3-Beta72C-10, Cu3-Beta94C-10, Cu3-Beta136C-10 and Cu3-Beta189C-10 respectively.

[0188] The anti-sintering deactivation performance of the above catalysts and their samples calcined at 550℃ (3h) was evaluated by the gas-solid phase hydroamination of caprolactone to produce caprolactam. The results showed that under the same reaction conditions, the catalytic activity of Cu3-Beta38C-10, Cu3-Beta72C-10, Cu3-Beta94C-10, Cu3-Beta136C-10 and Cu3-Beta189C-10 catalysts decreased by approximately 5%, 8%, 9%, 14% and 17% respectively after high-temperature calcination.

[0189] Example 11: This example is used to illustrate that when preparing Cu-Beta zeolite catalysts according to the improved ammonia distillation method provided by the present invention, it is allowed to use Beta zeolite precursors with different silicon-aluminum oxide molar ratios (molar ratios of SiO2 to Al2O3) to prepare the dealuminated Beta zeolite carrier modified by the chiseling. However, when the Beta zeolite precursor with a higher silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) is used to prepare the dealuminated Beta zeolite carrier modified by the chiseling, it is suitable for preparing Cu-Beta zeolite catalysts with lower copper loading.

[0190] Example 1 was repeated, but in the first step of preparing the dealuminated Beta zeolite carrier, a Beta zeolite matrix with a silicon aluminum oxide molar ratio (a molar ratio of SiO2 to Al2O3) of 100 was synthesized as a raw material for preparing the dealuminated Beta zeolite carrier according to the hydrothermal crystallization method provided in Chinese invention patent CN1108275C (application date 1999.9.10). The synthesized Beta zeolite matrix was subjected to conventional filtration, washing, drying (200°C, 3h) and calcination to remove the template agent (500°C, 8h). The average grain size of the synthesized Beta zeolite matrix was small (less than 1μm) by TEM observation. No impurities were found by XRD examination, and the BET specific surface area was calculated to be higher than 530m by nitrogen physical adsorption data. 2 / g, and the molar ratio of silicon aluminum oxide (the molar ratio of SiO2 to Al2O3) measured by XRF method is 94, which meets the technical requirements of the present invention for Beta zeolite matrix.

[0191] The Beta zeolite matrix was used for dealumination with concentrated nitric acid to prepare a dealumination Beta zeolite carrier (codenamed Beta94c) with a silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) of 932 (>900), and the silicon-aluminum oxide molar ratio (molar ratio of SiO2 to Al2O3) of the carrier met the technical requirements of the present invention. On this basis, according to the method of the second step of Example 1, the above-mentioned dealumination Beta zeolite carrier was subjected to a hole-modification treatment with an aqueous solution of ethanolamine to obtain a dealumination Beta zeolite carrier modified with a hole, named Beta94C. Further, according to the method of the third step of Example 1, a Cu-Beta zeolite catalyst with a copper content of 6 wt.% was prepared by using an improved ammonia evaporation method according to the method of two equal volume impregnations and two ammonia evaporations. The concentration of the copper ammonia complex solution used in the two equal-volume impregnations was 0.38 M. Since the concentration of the 0.38 M copper ammonia complex solution was very close to the concentration of the saturated copper ammonia complex solution prepared with a dilute ammonia base solution, 12.5 ml of the 0.4 M copper ammonia complex saturated solution was directly used to impregnate the Beta94C support in equal volumes. The prepared catalyst was codenamed Cu6-Beta94C-11.

[0192] The catalyst and its 550℃ calcined (3h) samples were evaluated for their anti-sintering deactivation performance by gas-solid phase hydroamination of caprolactone to produce caprolactam. The results showed that under the same reaction conditions, the catalytic activity (caprolactam yield) of the Cu6-Beta94C-11 catalyst decreased by 10% after high-temperature calcination.

Claims

1. A method for improving the stability of Cu-Beta zeolite catalyst for preparing caprolactone into caprolactam, characterized in that: Here are the steps: The first step is to prepare the dealuminated Beta zeolite carrier (1) Select Beta zeolite matrix The Beta zeolite matrix refers to a silica-alumina Beta zeolite that meets the following requirements: 1) there is no impurity crystal in the Beta zeolite matrix; 2) the crystallization of the Beta zeolite matrix is ​​good, that is, the BET specific surface area value of the Beta zeolite matrix measured by nitrogen physical adsorption method is ≥ 450m 2 / g; 3) the molar ratio of silicon aluminum oxide in the Beta zeolite matrix, that is, the molar ratio of SiO2 to Al2O3 is in the range of 10-200; (2) Preparation of dealuminated Beta zeolite carrier A dealuminated Beta zeolite carrier is prepared by an acid dealumination method based on a Beta zeolite matrix, and the molar ratio of silicon-aluminum oxide, i.e., the molar ratio of SiO2 to Al2O3, of the dealuminated Beta zeolite carrier is required to be ≥700; In the second step, the hydroxyl holes of the dealuminated Beta zeolite carrier are modified by chiseling holes with an aqueous solution of ethanolamine. The modification of the hydroxyl dimples is carried out by aqueous solution impregnation method, and the parameter requirements are as follows: The concentration of ethanolamine solution ranges from 0.01M to 0.4M; The ratio of the ethanolamine solution to the dealuminated Beta zeolite carrier, i.e., the liquid-solid ratio ranges from 1:1 to 100:1, and the unit of the liquid-solid ratio is ml / g; The immersion temperature range is 20℃-100℃; The immersion time ranges from 0.1h to 24h; The third step is to prepare a Cu-Beta zeolite catalyst by loading copper in the pores of the dealuminated Beta zeolite carrier modified by the improved ammonia evaporation method. The specific steps are as follows: (1) preparing a dilute ammonia basic solution and a saturated solution of a copper ammonia complex: preparing a dilute ammonia basic solution with a pH value of 11-12 according to a ratio of 4.4 g of industrial ammonia containing 25-28 wt.% NH3 to 100 ml of deionized water, and sealing and storing it for later use; then, using copper nitrate trihydrate as a soluble copper-containing compound and reacting with industrial ammonia to synthesize a copper ammonia complex according to a molar ratio of copper ions to ammonia molecules of 1:4; finally, dissolving the copper ammonia complex with the dilute ammonia basic solution at room temperature to prepare a saturated solution of the copper ammonia complex, and sealing and storing it for later use; the concentration of copper ammonia ions in the saturated solution of the copper ammonia complex is 0.4 M; (2) impregnating the zeolite carrier with an equal volume of a copper-ammine complex solution: first, measuring the saturated water absorption rate of the zeolite carrier, and calculating the amount of the copper-ammine complex solution used for impregnating the zeolite carrier with an equal volume; then, calculating the required concentration of the copper-ammine complex solution according to the copper loading of the Cu-Beta zeolite catalyst to be prepared; when the calculated concentration is equal to 0.4 M, directly impregnating the zeolite carrier with an equal volume of a saturated solution of the copper-ammine complex; when the calculated concentration is lower than 0.4 M, the saturated solution of the copper-ammine complex is appropriately diluted with a dilute ammonia base solution, and then impregnating the zeolite carrier with an equal volume; When the calculated value is higher than 0.4M, the concentration of the copper-ammine complex solution for a single equal-volume impregnation should be recalculated according to multiple equal-volume impregnations, and the copper-ammine complex solution of the required concentration should be prepared with the dilute ammonia basic solution and the saturated solution of the copper-ammine complex for each equal-volume impregnation; After each impregnation, the zeolite carrier is subjected to ammonia evaporation treatment; the equal volume impregnation is carried out at room temperature in a closed container; the equal volume impregnation time ranges from 0.5 to 24 hours; (3) Ammonia evaporation: The ammonia evaporation process is carried out under normal pressure or reduced pressure; the ammonia evaporation temperature and time range are 50-100°C and 0.5-48h; (4) Dehydration and drying after ammonia evaporation: the drying temperature and time ranges are 100-200°C and 0.5-48h respectively; (5) Calcination after ammonia evaporation: Calcination is carried out in an air atmosphere, and the calcination temperature and time ranges from 350-650°C and 0.5-24h respectively; The catalyst precursor is obtained through calcination treatment; (6) Hydrogen reduction treatment of catalyst precursor: the ranges of reduction temperature, time and hydrogen volume space velocity are 280-600°C, 0.5-20h and 1-2000h, respectively. -1 The catalyst precursor is reduced with hydrogen to become a Cu-Beta zeolite catalyst.

2. A method for improving the stability of a Cu-Beta zeolite catalyst for preparing caprolactone into caprolactam according to claim 1, characterized in that: In the first step (1), the molar ratio of silicon to aluminum oxide in the Beta zeolite matrix, that is, the molar ratio of SiO2 to Al2O3, is in the range of 20-100.

3. A method for improving the stability of a Cu-Beta zeolite catalyst for preparing caprolactone into caprolactam according to claim 2, characterized in that: In the first step (1), the molar ratio of silicon to aluminum oxide in the Beta zeolite matrix, that is, the molar ratio of SiO2 to Al2O3, is in the range of 25-60.

4. A method for preparing a Cu-Beta zeolite catalyst for improving the stability of caprolactone to caprolactam according to claim 1, characterized in that: In the first step (2), the molar ratio of silicon aluminum oxide, that is, the molar ratio of SiO2 to Al2O3 of the dealuminated Beta zeolite carrier prepared is required to be in the range of ≧800.

5. A method for preparing a Cu-Beta zeolite catalyst for improving the stability of caprolactone to caprolactam according to claim 4, characterized in that: In the first step (2), the molar ratio of silicon aluminum oxide, that is, the molar ratio of SiO2 to Al2O3 of the dealuminated Beta zeolite carrier prepared is required to be in the range of ≧900.

6. A method for preparing a Cu-Beta zeolite catalyst for improving the stability of caprolactone to caprolactam according to claim 1, characterized in that: In the first step (2), a Beta zeolite matrix is ​​acid-dealuminized with a concentrated nitric acid aqueous solution to prepare a dealuminated Beta zeolite carrier, as follows: 13M concentrated nitric acid is used as dealuminous acid solution, and the amount of acid solution is used according to a liquid-to-solid ratio of 20:1, and the unit of the liquid-to-solid ratio is ml / g; the dealuminous reaction is carried out at 95°C, and the dealuminous reaction time is 20h; after the dealuminous reaction is completed, the solid product is first recovered by solid-liquid separation, and then the solid product is washed with water to a neutral pH value, and then dried at a temperature of 80-200°C for 3-24h, and calcined at a temperature of 500°C-600°C for 3-8h to obtain the dealuminous Beta zeolite.

7. A method for improving the stability of a Cu-Beta zeolite catalyst for preparing caprolactone into caprolactam according to claim 1, characterized in that: In the second step, the hydroxyl holes of the dealuminated Beta zeolite carrier are modified by using an aqueous solution of ethanolamine. The parameters are as follows: The concentration of ethanolamine solution ranges from 0.02M to 0.3M; The ratio of the ethanolamine solution to the dealuminated Beta zeolite carrier, i.e., the liquid-solid ratio ranges from 2:1 to 50:1, and the unit of the liquid-solid ratio is ml / g; The immersion temperature range is 30℃-90℃; The immersion time ranges from 0.5h to 10h.

8. A method for improving the stability of a Cu-Beta zeolite catalyst for preparing caprolactone into caprolactam according to claim 7, characterized in that: In the second step, the hydroxyl holes of the dealuminated Beta zeolite carrier are modified by using an aqueous solution of ethanolamine. The parameters are as follows: The concentration of ethanolamine solution ranges from 0.03M to 0.16M; The ratio of the ethanolamine solution to the dealuminated Beta zeolite carrier, i.e., the liquid-solid ratio ranges from 3:1 to 20:1, and the unit of the liquid-solid ratio is ml / g; The immersion temperature range is 40℃-80℃; The immersion time ranges from 1 to 5 hours.

9. A method for improving the stability of a Cu-Beta zeolite catalyst for preparing caprolactone into caprolactam according to claim 1, characterized in that: In the third step (2), the equal volume immersion time ranges from 1 to 12 h; In the third step (3), the temperature and time of ammonia evaporation are in the range of 60-90°C and 1-24h; In the third step (4), the drying temperature and time ranges from 110 to 170°C and 1 to 24 h, respectively; In the third step (5), the calcination temperature and time range from 400 to 600°C and 1 to 12 h, respectively; In the third step (6), the reduction temperature, time and hydrogen volume space velocity ranges are 300-550°C, 1-15h and 10-1500h, respectively. -1 .

10. A method for improving the stability of Cu-Beta zeolite catalyst for preparing caprolactone into caprolactam according to claim 9, characterized in that: In the third step (2), the equal volume immersion time ranges from 2 to 6 h; In the third step (3), the temperature and time of ammonia evaporation are in the range of 65-85°C and 3-12h; In the third step (4), the drying temperature and time ranged from 120-150°C and 3-12h, respectively; In the third step (5), the calcination temperature and time range from 450-550°C and 2-6h, respectively; In the third step (6), the reduction temperature, time and hydrogen volume space velocity ranged from 350-500°C, 2-8h and 20-1000h, respectively. -1 .

11. The Cu-Beta zeolite prepared by the preparation method for improving the stability of the Cu-Beta zeolite catalyst for preparing caprolactone into caprolactam according to any one of claims 1 to 10 is used for catalyzing the gas-solid phase hydroamination of caprolactone into caprolactam.

12. The use according to claim 11, characterized in that: The reaction conditions are as follows: the reaction temperature is in the range of 120-350°C, the reaction pressure is in the range of 0.01-2 atm, and the feed space velocity of caprolactone is in the range of 0.1-5 h -1 The molar ratios of amino-ester, hydrogen-ester and water-ester are in the range of 1-50, 5-70 and 0-100 respectively.

Citation Information

Patent Citations

  • Copper-based catalyst prepared by ammonia distillation method and application of copper-based catalyst in oxidation carbonylation synthesis of alkyl carbonate

    CN103084201A

  • Method for converting n-butane into isobutane through using gold supported molecular sieve catalyst

    CN103145517A

  • Catalyst for producing caprolactam as well as preparation method and application thereof

    CN104307556A

  • Method for synthesizing hexamethylenediamine from caprolactam in one step

    CN113461540A

  • Preparation method and application of zinc ion modified Sn-Beta zeolite

    CN114210362A

Cited By

  • Preparation method for improving stability of cu-beta zeolite catalyst for preparing caprolactam from caprolactone, and use thereof

    WO2026001632A1

  • Method for preparing cu-beta zeolite catalyst for production of caprolactam from caprolactone, and use

    WO2026001633A1